Test method for oil well pipe resistance to hydrogen sulfide stress corrosion based on fracture specimens

Through the test method of hydrogen sulfide stress corrosion resistance of oil well tubes based on fracture samples, using slow tensile test and fracture morphology observation, the problems of harsh test conditions and long cycles in the existing technology are solved, and the rapid and accurate Evaluate the resistance to hydrogen sulfide stress corrosion of oil well pipe materials.

CN115356200BActive Publication Date: 2024-11-29ANGANG STEEL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202210910655.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-29
Publication Date
2024-11-29
Estimated Expiration
2042-07-29

AI Technical Summary

Technical Problem

When evaluating the performance of oil well tubes to stress corrosion of hydrogen sulfide, the test conditions are harsh and the cycle is long, and information about failure or failure can only be given, and the corrosion resistance level of the material cannot be accurately evaluated.

Method used

The stress corrosion resistance sensitivity test method of oil well tubes based on fracture samples was used, and the stress corrosion resistance sensitivity of the material was evaluated through slow tensile test and fracture morphology observation, and step crack parameters were used for quantitative analysis.

Benefits of technology

It achieves rapid and accurate evaluation of the hydrogen sulfide stress corrosion resistance of oil well pipe materials, shortens the test cycle, improves detection efficiency, and more accurately evaluates the corrosion resistance level of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115356200B_ABST
    Figure CN115356200B_ABST
Patent Text Reader

Abstract

The present invention provides a method for testing the hydrogen sulfide stress corrosion sensitivity of oil well pipes based on fractured specimens, comprising: processing the specimen into a set size and pre-treating its surface; installing the specimen on a stretching device in a reactor, adding an appropriate amount of test solution into the reactor, and sealing the reactor; adjusting the hydrogen sulfide concentration in the test solution, and rapidly stretching and pre-loading the specimen to 70% to 80% of the yield strength value; after the pre-load is stable, starting a slow tensile loading test at a set strain rate until the specimen is broken, and recording the test results; taking out the fractured tensile specimen, removing the corrosion products on the specimen surface and the fracture, and evaluating the stress corrosion resistance of the oil well pipe material by observing the fracture morphology and step crack parameters. The step crack parameters on the fracture are used to accurately analyze the slow tensile test results, so as to achieve the purpose of quantitatively analyzing the stress corrosion sensitivity of the oil well pipe material, shorten the test cycle, and improve the detection efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of corrosion testing, and in particular to a method for testing the sensitivity of oil well pipes to hydrogen sulfide stress corrosion based on fracture samples. Background Art

[0002] In recent years, with the exploration and development of ultra-deep, ultra-high temperature, ultra-high corrosion and harsh environment oil and gas wells, the working environment of oil and gas wells generally has the characteristics of "high temperature, high pressure, high CO2, high H2S, high Cl-, and high mineralization". These complex and harsh working conditions, coupled with special operating processes, lead to stress corrosion cracking failure of oil well pipes, which seriously affects the normal production and operation of oil and gas fields. In particular, in the process of exploration and exploitation of sulfur-containing oil and gas resources, the oil well pipes used are prone to hydrogen sulfide stress corrosion cracking, which is a low-stress brittle fracture with fast crack propagation speed and sudden fracture. It has the highest risk factor and is prone to cause major accidents and casualties.

[0003] In view of the above situation, relevant standards have been formulated at home and abroad to reduce the risks brought by hydrogen sulfide stress corrosion cracking (SSCC), and strict testing and evaluation of oil well pipe resistance to SSCC have been carried out. NACE Standard TM0177-2005 "Indoor test of metal resistance to sulfide stress corrosion cracking and stress corrosion cracking in H2S environment" and GB / T4157-2006 "Laboratory test of metal resistance to special forms of environmental cracking in hydrogen sulfide environment" both stipulate the standard tensile test (method A), and determine its resistance to hydrogen sulfide stress corrosion by the fracture time within the test cycle. Products that do not fracture for more than 720 hours are qualified, and products that fracture within 720 hours are unqualified. The test results can only provide information on failure and non-failure. Similarly, the four-point bending loading test in the ASTM G39-99 standard is also a common method for evaluating the stress corrosion resistance of oil well pipes. Using the A method standard solution, products that do not break within 720 hours are qualified, and products that break within 720 hours are unqualified. A 10x magnifying glass is used to observe whether there are cracks on the surface of the unbroken sample. The test results can only give information on failure or non-failure. The above methods have harsh test conditions, long test cycles, and the test results can only give relevant information such as qualified and unqualified. For samples that have not failed, it is impossible to evaluate their hydrogen sulfide stress corrosion resistance performance level. It is necessary to combine other experimental methods for comprehensive evaluation, which prolongs the test cycle and increases the test cost.

[0004] Therefore, it is necessary to find a new method that can quickly and accurately evaluate the hydrogen sulfide stress corrosion resistance of oil well pipe materials, shorten the test cycle, and reduce the test cost. The slow rate tensile test has been widely used by researchers because it is fast, accurate, highly reproducible, and obtains a lot of parameter information. It is currently one of the more mature and advanced standard methods for studying stress corrosion. When evaluating the hydrogen sulfide stress corrosion resistance of oil well pipes by slow tensile tests, fracture morphology and stress corrosion cracking sensitivity index are usually used for evaluation. If the fracture morphology is a brittle fracture feature, or the stress corrosion cracking sensitivity index is greater than a certain value (generally 25%), it is generally believed that the oil well pipe material has stress corrosion cracking sensitivity in the corresponding research system.

[0005] However, in the actual test process, it is often found that the fracture morphology is ductile fracture or mixed fracture mechanism, and the stress corrosion sensitivity index calculated by using the elongation after fracture, the shrinkage after fracture and the yield strength loss ratio is less than 25%. It is often believed that the material does not have stress corrosion sensitivity, but a step-shaped crack platform appears near the circumference of the fracture, indicating that the material actually has obvious stress corrosion sensitivity, which is inconsistent with the test results. In addition, even if the two materials have the same stress corrosion sensitivity index, the actual stress corrosion resistance is quite different, especially the crack steps perpendicular to the tensile direction in the fracture morphology are distributed along the circumferential direction, and their size and number are significantly different, which is not conducive to accurately evaluating the material's anti-SSCC performance.

[0006] Based on the above content, in order to accurately and quickly evaluate the hydrogen sulfide stress corrosion resistance of oil well pipe materials, the present invention is specially proposed. Summary of the invention

[0007] In order to overcome the shortcomings of the background technology, the present invention provides a method for testing the hydrogen sulfide stress corrosion sensitivity of oil well pipes based on fracture specimens, which can quickly and accurately evaluate the hydrogen sulfide stress corrosion resistance of oil well pipe materials, and use the step crack parameters on the fracture to accurately analyze the slow tensile test results, so as to achieve the purpose of quantitatively analyzing the stress corrosion sensitivity of oil well pipe materials, shorten the test cycle, and improve the detection efficiency.

[0008] In order to achieve the above object, the present invention adopts the following technical solutions:

[0009] A method for testing the susceptibility of oil well pipes to hydrogen sulfide stress corrosion based on fracture specimens comprises the following steps:

[0010] Step 1: Process the sample into a set size and pre-treat its surface;

[0011] Step 2: Install the sample on the stretching device in the reactor, add an appropriate amount of test solution into the reactor, and seal the reactor;

[0012] Step 3: Adjust the concentration of hydrogen sulfide in the test solution and quickly stretch and preload the sample to 70% to 80% of the yield strength value;

[0013] Step 4: After the preload is stable, start the slow tensile loading test at the set strain rate until the sample is broken and record the test results;

[0014] Step 5: Finally, take out the broken tensile specimen, remove the corrosion products on the specimen surface and fracture, and evaluate the stress corrosion resistance of the oil well pipe material by observing the fracture morphology and step crack parameters.

[0015] Furthermore, the strain rate of the slow tensile loading test is 1×10 -7 ~5×10 -5 mm / s.

[0016] Furthermore, the strain rate of the rapid stretching is greater than or equal to 1×10 -4 mm / s.

[0017] Furthermore, the step 5 of evaluating the stress corrosion resistance of the oil well pipe material specifically includes the following:

[0018] 1) The crack propagation direction is along the step crack plane, extending from the outer surface of the sample along the radius to the center and along the circumferential direction at the same time;

[0019] 2) The step crack plane with the largest area on the fracture is selected to measure the step crack parameters;

[0020] 3) Step crack parameters include plane length a and radial width b, where a and b are on the same step crack plane and the measurement directions are perpendicular to each other;

[0021] 4) The plane shape of the step crack is elliptical, and the sensitivity to hydrogen sulfide stress corrosion is related to the maximum plane area S of the step crack. Its sensitivity index R = Kπa*b, where K is a constant and ranges from 1 to 2.

[0022] Furthermore, the slow tensile loading test is loaded along the length direction of the sample, and the tensile direction is parallel to the length direction of the sample.

[0023] Furthermore, the stretching direction of the slow tensile loading test is perpendicular to the step crack plane, and the stretching direction is perpendicular to the crack propagation direction, with a difference of 90°.

[0024] Furthermore, the test solution is Nace standard A solution, and the hydrogen sulfide concentration is 0 to 3500 ppm.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] The present invention tests the stress corrosion resistance of oil well pipe materials in a service environment or a simulated actual environment, evaluates the stress corrosion resistance sensitivity of the oil well pipe materials by observing the fracture morphology and step crack parameters, and further evaluates the practicability of the oil well pipe materials in a specific working environment, thereby guiding material selection and equipment maintenance. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is the macroscopic fracture morphology of the fracture sample when the hydrogen sulfide concentration is zero;

[0028] Figure 2 This is the side morphology of the fracture sample when the hydrogen sulfide concentration is zero;

[0029] Figure 3 This is the macroscopic fracture morphology of the fracture sample when the hydrogen sulfide concentration is 1000ppm;

[0030] Figure 4 This is the side morphology of the fracture sample when the hydrogen sulfide concentration is 1000ppm;

[0031] Figure 5 This is the macroscopic fracture morphology of the fracture sample when the hydrogen sulfide concentration is 3500ppm;

[0032] Figure 6 This is the side morphology of the fracture sample when the hydrogen sulfide concentration is 3500ppm;

[0033] Figure 7 Diagram showing the measurement method of the plane length a and radial width b of the step crack. DETAILED DESCRIPTION

[0034] The specific implementation modes provided by the present invention are described in detail below with reference to the accompanying drawings.

[0035] A method for testing the susceptibility of oil well pipes to hydrogen sulfide stress corrosion based on fracture specimens comprises the following steps:

[0036] Step 1: Process the sample into a set size and pre-treat its surface;

[0037] Step 2: Install the sample on the stretching device in the reactor, add an appropriate amount of test solution into the reactor, and seal the reactor; the test solution is Nace standard A solution, and the hydrogen sulfide concentration is 0 to 3500 ppm.

[0038] Step 3: Adjust the concentration of hydrogen sulfide in the test solution, and quickly stretch the preloaded sample to 70% to 80% of the yield strength value; the strain rate of the rapid stretching is greater than or equal to 1×10 -4 mm / s.

[0039] Step 4: After the preload is stable, a slow tensile loading test is performed at a set strain rate until the sample is broken, and the test results are recorded; the strain rate of the slow tensile loading test is 1×10 -7 ~5×10 -5 mm / s.

[0040] Step 5: Finally, take out the broken tensile specimen, remove the corrosion products on the specimen surface and fracture, and evaluate the stress corrosion resistance of the oil well pipe material by observing the fracture morphology and step crack parameters. Specifically include the following:

[0041] 1) The crack propagation direction is along the step crack plane, extending from the outer surface of the sample along the radius to the center and along the circumferential direction at the same time;

[0042] 2) The step crack plane with the largest area on the fracture is selected to measure the step crack parameters;

[0043] 3) If Figure 7 As shown, the step crack parameters include the plane length a and the radial width b, a and b are on the same step crack plane, and the measurement directions are perpendicular to each other;

[0044] 4) The plane shape of the step crack is elliptical, and the sensitivity to hydrogen sulfide stress corrosion is related to the maximum plane area S of the step crack. Its sensitivity index R = Kπa*b, where K is a constant and ranges from 1 to 2.

[0045] The fracture morphology is observed using a microscope with a magnification of 10-100. When the step crack is small, a larger magnification is used, and when the step crack is large, a smaller magnification is used to ensure that the fracture morphology of the sample is fully presented and the step crack parameters are accurately measured.

[0046] The microscope includes an electron microscope or a laser confocal microscope. The fracture of the sample is uneven and there are step cracks in the circumferential direction of the sample, so it needs to have a strong focusing ability.

[0047] The slow tensile loading test is loaded along the length direction of the sample, and the tensile direction is parallel to the length direction of the sample. The tensile direction of the slow tensile loading test is perpendicular to the step crack plane, and the tensile direction is perpendicular to the crack extension direction, with a difference of 90°.

[0048] Example 1

[0049] The test material is sulfur-resistant oil well pipe 110S with a yield strength of 800 MPa. The method consists of Ⅰ sample processing, Ⅱ surface treatment, Ⅲ slow tensile loading test and Ⅳ fracture morphology observation and step crack parameter measurement.

[0050] The specimen processing in step I is to process the test material into a cylindrical tensile specimen with a length of 72 mm, a diameter of 6.40 mm, and a surface finish of 0.3 μm;

[0051] The surface treatment in step II is to use ultrasonic cleaning to clean the sample in step I in acetone and anhydrous ethanol respectively, so as to remove the residue and grease on the surface of the sample;

[0052] The slow tensile loading test in step III is carried out using a slow strain rate tensile testing machine. The test temperature is room temperature. Nace standard A solution is injected into the reactor, the reactor is closed, and high-purity nitrogen is introduced for deoxygenation for 2 hours. The hydrogen sulfide concentration in the solution is 0. The sample is pre-loaded to 600Mpa and the sample is kept in the elastic stress deformation stage. Then, the sample is subjected to 5*10 -6 The slow tensile loading test was started at a strain rate of mm / s. After the test, the test results were recorded, the broken tensile specimens were taken out, and the corrosion products on the surface and fracture of the specimens were removed to ensure that the surface of the specimens presented a metallic luster and the fracture morphology was clear;

[0053] The fracture morphology observation and step crack parameter measurement in step IV were performed using a scanning electron microscope. The broken tensile specimen was placed vertically on the stage with the tensile direction perpendicular to the stage plane. The working distance between the fracture and the lens was adjusted to 12.9 mm, the magnification was 58 times, and the fracture morphology was photographed after focusing clearly. Figure 1-2 The fracture is cup-cone shaped, which is a ductile fracture. No stress corrosion occurs. The step crack parameters a and b are both recorded as 0. When the stress corrosion sensitivity formula R=Kπa*b is substituted, K is taken as 2. The test results are shown in Table 1.

[0054] Example 2

[0055] The test material is sulfur-resistant oil well pipe 110S with a yield strength of 800 MPa. The method consists of Ⅰ sample processing, Ⅱ surface treatment, Ⅲ slow tensile loading test and Ⅳ fracture morphology observation and step crack parameter measurement.

[0056] The specimen processing in step I is to process the test material into a cylindrical tensile specimen with a length of 72 mm, a diameter of 6.40 mm, and a surface finish of 0.3 μm;

[0057] The surface treatment in step II is to use ultrasonic cleaning to clean the sample in step I in acetone and anhydrous ethanol respectively, so as to remove the residue and grease on the surface of the sample;

[0058] The slow tensile loading test in step III is carried out using a slow strain rate tensile testing machine. The test temperature is room temperature. Nace standard A solution is injected into the reactor, and high-purity nitrogen is used for deoxygenation for 2 hours. An appropriate amount of analytical pure sodium sulfide is added. After sufficient reaction, the hydrogen sulfide concentration in the solution is ensured to be 1000ppm. The reactor is closed and the sample is pre-loaded to 600Mpa to keep the sample in the elastic stress deformation stage. Then, the sample is subjected to 5*10 -6 The slow tensile loading test was started at a strain rate of mm / s. After the test, the test results were recorded, the broken tensile specimens were taken out, and the corrosion products on the surface and fracture of the specimens were removed to ensure that the surface of the specimens presented a metallic luster and the fracture morphology was clear;

[0059] The fracture morphology observation and step crack parameter measurement in step IV were performed using a scanning electron microscope. The broken tensile specimen was placed vertically on the stage with the tensile direction perpendicular to the stage plane. The working distance between the fracture and the lens was adjusted to 12.7 mm, the magnification was 41 times, and the fracture morphology was photographed after focusing clearly. Figure 3-4 , select the step crack plane with the largest area, and calculate the plane length a and radial width b through the software. a and b are located on the same step crack plane, and the measurement directions are perpendicular to each other. The stress corrosion sensitivity formula R=Kπa*b is introduced, and K is taken as 2. The test results are shown in Table 1.

[0060] Example 3

[0061] The test material is sulfur-resistant oil well pipe 110S with a yield strength of 800 MPa. The method consists of Ⅰ sample processing, Ⅱ surface treatment, Ⅲ slow tensile loading test and Ⅳ fracture morphology observation and step crack parameter measurement.

[0062] The specimen processing in step I is to process the test material into a cylindrical tensile specimen with a length of 72 mm, a diameter of 6.40 mm, and a surface finish of 0.3 μm;

[0063] The surface treatment in step II is to use ultrasonic cleaning to clean the sample in step I in acetone and anhydrous ethanol respectively, so as to remove the residue and grease on the surface of the sample;

[0064] The slow tensile loading test in step III is carried out using a slow strain rate tensile testing machine. The test temperature is room temperature. Nace standard A solution is injected into the reactor. The reactor is closed and high-purity nitrogen is introduced for deoxygenation for 2 hours. Then high-purity hydrogen sulfide gas is introduced until the solution is saturated. The concentration of hydrogen sulfide in the solution is 3500ppm under normal pressure. The sample is pre-loaded to 600Mpa to keep the sample in the elastic stress deformation stage. Then, the sample is subjected to 5*10 -6The slow tensile loading test was started at a strain rate of mm / s. After the test, the test results were recorded, the broken tensile specimens were taken out, and the corrosion products on the surface and fracture of the specimens were removed to ensure that the surface of the specimens presented a metallic luster and the fracture morphology was clear;

[0065] The fracture morphology observation and step crack parameter measurement in step IV were performed using a scanning electron microscope. The broken tensile specimen was placed vertically on the stage with the tensile direction perpendicular to the stage plane. The working distance between the fracture and the lens was adjusted to 11.7 mm, the magnification was 40 times, and the fracture morphology was photographed after focusing clearly. Figure 5-6 , select the step crack plane with the largest area, and calculate the plane length a and radial width b through the software. a and b are located on the same step crack plane, and the measurement directions are perpendicular to each other. The stress corrosion sensitivity formula R=Kπa*b is introduced, and K is taken as 2. The test results are shown in Table 1.

[0066] Table 1 Slow tensile test results of oil well pipes at different hydrogen sulfide concentrations

[0067]

[0068] From the above test results, it can be seen that in Nace standard A solution, when the hydrogen sulfide concentration is zero, the oil well pipe material does not suffer from stress corrosion, the fracture is cup-cone shaped, which is a ductile fracture, and the stress corrosion sensitivity index is 0. With the increase of hydrogen sulfide concentration, the stress corrosion sensitivity index of the oil well pipe material increases from 59.52 to 88.86, and the fracture morphology shows step cracks, with obvious stress corrosion characteristics, which is consistent with the conventional calculation results of stress corrosion sensitivity, such as elongation loss ratio and fracture time loss ratio. This method realizes the measurement of the stress corrosion sensitivity of oil well pipes, and through the observation of fracture morphology and the calculation of step crack parameters, the stress corrosion resistance of oil well pipe materials can be evaluated more accurately and comprehensively.

[0069] Example 4

[0070] The samples used in the test are two types of oil well pipes, A and B, and the two oil well pipes are two different oil well pipes (for example, oil well pipes with different materials or different rolling, heat treatment and other processes, the explanations here are the same in the following embodiments). The method consists of I sample processing, II surface treatment, III slow tensile loading test and IV fracture morphology observation and step crack parameter measurement.

[0071] The specimen processing in step I is to process the test material into a cylindrical tensile specimen with a length of 72 mm, a diameter of 6.40 mm, and a surface finish of 0.3 μm;

[0072] The surface treatment in step II is to use ultrasonic cleaning to clean the sample in step I in acetone and anhydrous ethanol respectively, so as to remove the residue and grease on the surface of the sample;

[0073] The slow tensile loading test in step III is carried out using a slow strain rate tensile testing machine. The test temperature is room temperature. Nace standard A solution is injected into the reactor. The reactor is sealed and high-purity nitrogen is introduced for deoxygenation for 2 hours. Then high-purity hydrogen sulfide gas is introduced until the solution is saturated. The concentration of hydrogen sulfide in the solution is 3500ppm under normal pressure. After the preload is stable, the 1*10 -7 The slow tensile loading test was started at a strain rate of mm / s. After the test, the test results were recorded, the broken tensile specimens were taken out, and the corrosion products on the surface and fracture of the specimens were removed to ensure that the surface of the specimens presented a metallic luster and the fracture morphology was clear;

[0074] The fracture morphology observation and step crack parameter measurement in step IV are carried out using a scanning electron microscope. The broken tensile specimen is placed vertically on the stage with the stretching direction perpendicular to the stage plane. The working distance between the fracture and the lens is adjusted to 10 mm, the magnification is 30 times, and the fracture morphology is photographed after focusing clearly. The step crack plane with the largest area is selected, and the plane length a and radial width b are calculated by software. a and b are located on the same step crack plane, and the measurement directions are perpendicular to each other. The stress corrosion sensitivity formula R=Kπa*b is used, and K is 2. The test results are shown in Table 2. Analysis shows that the stress corrosion sensitivity index is in the order of B>A from high to low, and the hydrogen sulfide stress corrosion resistance is in the order of A>B from high to low.

[0075] Table 2 Slow tensile test results of oil well pipe

[0076]

[0077] Example 5

[0078] The samples used in the test are two types of oil well pipes, A and B, and the two oil well pipes are two different oil well pipes (for example, oil well pipes with different materials or different rolling, heat treatment and other processes, the explanations here are the same in the following embodiments). The method consists of I sample processing, II surface treatment, III slow tensile loading test and IV fracture morphology observation and step crack parameter measurement.

[0079] The specimen processing in step I is to process the test material into a cylindrical tensile specimen with a length of 72 mm, a diameter of 6.40 mm, and a surface finish of 0.3 μm;

[0080] The surface treatment in step II is to use ultrasonic cleaning to clean the sample in step I in acetone and anhydrous ethanol respectively, so as to remove the residue and grease on the surface of the sample;

[0081] The slow tensile loading test in step III is carried out using a slow strain rate tensile testing machine. The test temperature is room temperature. Nace standard A solution is injected into the reactor, and high-purity nitrogen is used for deoxygenation for 2 hours. An appropriate amount of analytical pure sodium sulfide is added. After sufficient reaction, the hydrogen sulfide concentration in the solution is ensured to be 1000ppm. The reactor is closed. After the preload is stable, the test is started according to 5*10 -5 The slow tensile loading test was started at a strain rate of mm / s. After the test, the test results were recorded, the broken tensile specimens were taken out, and the corrosion products on the surface and fracture of the specimens were removed to ensure that the surface of the specimens presented a metallic luster and the fracture morphology was clear;

[0082] The fracture morphology observation and step crack parameter measurement in step IV are carried out using a scanning electron microscope. The broken tensile specimen is placed vertically on the stage, the stretching direction is perpendicular to the stage plane, the working distance between the fracture and the lens is adjusted to 20 mm, the magnification is 100 times, and the fracture morphology is photographed after focusing clearly. The step crack plane with the largest area is selected, and the plane length a and radial width b are calculated by software. a and b are located on the same step crack plane, and the measurement directions are perpendicular to each other. The stress corrosion sensitivity formula R=Kπa*b is introduced, and K is 2. The test results are shown in Table 3. Analysis shows that the stress corrosion sensitivity index is in the order of B>A from high to low, and the hydrogen sulfide stress corrosion resistance is in the order of A>B from high to low.

[0083] Table 3 Slow tensile test results of oil well pipe

[0084]

[0085] The above embodiments are implemented based on the technical solution of the present invention, and detailed implementation methods and specific operation processes are given, but the protection scope of the present invention is not limited to the above embodiments. The methods used in the above embodiments are conventional methods unless otherwise specified.

Claims

1. A method for testing the susceptibility of oil well pipe to hydrogen sulfide stress corrosion based on fracture specimens, characterized in that: The steps include: Step 1: Process the sample into a set size and pre-treat its surface; Step 2: Install the sample on the stretching device in the reactor, add an appropriate amount of test solution into the reactor, and seal the reactor; Step 3: Adjust the concentration of hydrogen sulfide in the test solution and quickly stretch and preload the specimen to 70%~80% of the yield strength value; Step 4: After the preload is stable, start the slow tensile loading test at the set strain rate until the sample is broken and record the test results; Step 5: Finally, take out the broken tensile specimen, remove the corrosion products on the specimen surface and fracture, and evaluate the stress corrosion resistance of the oil well pipe material by observing the fracture morphology and step crack parameters; The step 5 of evaluating the stress corrosion resistance of the oil well pipe material specifically includes the following: 1) The crack propagates in the direction along the step crack plane, extending from the outer surface of the specimen in the radial direction and in the circumferential direction simultaneously; 2) The step crack plane with the largest area on the fracture is selected to measure the step crack parameters; 3) The step crack parameters include plane length a and radial width b, where a and b are on the same step crack plane and the measurement directions are perpendicular to each other; 4) The plane shape of the step crack is elliptical, and the sensitivity to hydrogen sulfide stress corrosion is related to the largest plane area S of the step crack. Its sensitivity index R=Kπa*b, K is a constant, and K is 2; The slow tensile loading test is performed in a direction parallel to the length of the sample. The tensile direction of the slow tensile loading test is perpendicular to the step crack plane, and the tensile direction is perpendicular to the crack propagation direction, with a difference of 90°.

2. The method for testing the susceptibility of oil well pipe to hydrogen sulfide stress corrosion based on fracture specimens according to claim 1, characterized in that: The strain rate of the slow tensile loading test is 1×10 -7 ~ 5×10 -5 mm / s.

3. The method for testing the susceptibility of oil well pipe to hydrogen sulfide stress corrosion based on fracture specimens according to claim 1, characterized in that: The strain rate of the rapid stretching is greater than or equal to 1×10 -4 mm / s.

Citation Information

Patent Citations

  • Method for testing hydrogen sulfide stress corrosion resistance of oil well pipe

    CN109813612A

  • Method for evaluating slow tensile stress corrosion sensitivity of metal material

    CN112557229A

  • Method and device for estimating fatigue life of industrial pure aluminum wire

    CN112730211A

  • Reheating crack sensitivity evaluation method for improving calculation precision of percentage reduction of area

    CN114577626A

  • Quantitative evaluation method for mechanical property attenuation of pipe

    CN114646533A