Current collector and preparation method thereof, negative electrode and electrochemical energy storage device

By using a current collector with an alternating stacked structure in the lithium battery negative electrode, adjusting the lithophilicity of the metal foil layer and the polymer layer, and setting through holes, the energy density and cycle stability problems caused by the porous metal foil layer are solved and achieved. Higher electrochemical consistency and safety performance.

CN115440986BActive Publication Date: 2024-10-11BYD CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202110608569.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-06-01
Publication Date
2024-10-11
Estimated Expiration
2041-06-01

AI Technical Summary

Technical Problem

If the porous metal foil layer of the negative electrode of a lithium battery is too thick, it will reduce the energy density. If it is too thin, there will be insufficient space for lithium deposition and the risk of current collector fracture due to volume expansion stress during cycling, affecting the performance of the lithium battery.

Method used

A current collector with an alternating laminated structure is used, including a metal foil layer and a polymer layer. By adjusting the lithophilicity of the metal foil layer and the polymer layer in the laminated structure, through holes are set through the current collector to ensure that lithium is deposited in the metal foil layer. Within, the generation of lithium dendrites is avoided, stress is dispersed through multiple metal foil layers and polymer layers, and current distribution and cycle performance are optimized.

Benefits of technology

It improves the electrochemical consistency of the current collector, inhibits the generation of lithium dendrites, extends the cycle life of the battery, improves the energy density and safety performance, and avoids the risk of fracture caused by uneven current density and volume expansion of the lithium battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115440986B_ABST
    Figure CN115440986B_ABST
Patent Text Reader

Abstract

The present application provides a current collector, which includes a stacking structure, wherein the stacking structure has M layers of metal foil layers and M+1 layers of polymer layers, and the metal foil layers and the polymer layers are alternately stacked, M is a positive integer greater than 1, and when M≥2, the lithium affinity of the polymer layer gradually decreases from the M+1th layer in the stacking structure to the two ends in the stacking direction, and / or when M≥3, the lithium affinity of the metal foil layer gradually decreases from the M+1th layer in the stacking structure to the two ends in the stacking direction, and the current collector has a plurality of through holes penetrating the two relative surfaces of the current collector along the stacking direction. The current collector provided by the present application has excellent electrochemical properties, which is conducive to its application. The present application also provides a method for preparing the current collector, a negative electrode, and an electrochemical energy storage device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of energy storage technology, and in particular to a current collector and a preparation method thereof, a negative electrode and an electrochemical energy storage device. Background Art

[0002] Lithium batteries have high energy density, good cycle stability, safety and other characteristics, and are widely used in many fields such as mobile phones, computers, automobiles and power grid energy storage. In theory, the negative electrode of lithium batteries can use only current collectors without other negative electrode active materials, and porous metal foil can provide a certain reserved space for the deposition of lithium metal, and at the same time reduce the current density during lithium deposition, which is conducive to the uniform deposition of lithium. It has become one of the research schemes for current collectors. However, if the porous metal foil layer is too thick, the energy density of the battery system will be reduced. If it is too thin, there will be insufficient reserved space for lithium deposition and the risk of current collector fracture due to volume expansion stress during the cycle. All of the above reasons affect the performance of porous metal foil current collectors and lithium batteries, limiting the application of lithium batteries. Summary of the invention

[0003] The present application discloses a current collector with excellent electrochemical performance, which is beneficial to its application.

[0004] In a first aspect, the present application provides a current collector, the current collector comprising a stacking structure, the stacking structure having M layers of metal foil layers and M+1 layers of polymer layers, and the metal foil layers and the polymer layers are alternately stacked, M is a positive integer greater than 1,

[0005] When M≥2, the lithium affinity of the polymer layer pair gradually decreases from the M+1th layer in the stacking structure to both ends in the stacking direction.

[0006] and / or

[0007] When M≥3, the lithium affinity of the metal foil layer gradually decreases from the M+1th layer in the stacking structure to both ends in the stacking direction.

[0008] The current collector has a plurality of through holes penetrating two opposite surfaces of the current collector in a stacking direction.

[0009] The current collector provided in the present application is provided with a through hole that penetrates the current collector, thereby improving the electrochemical consistency inside the current collector and inhibiting the generation of lithium dendrites; the outermost sides of the stacked structure in the current collector are both polymer layers, and the metal foil layer is arranged inside the current collector, which can induce lithium to be deposited on the metal foil layer inside the current collector, thereby avoiding lithium deposition on the surface of the current collector; the multi-layer metal foil layer can effectively avoid the metal foil layer from breaking, and at the same time, the change in the affinity of the multi-layer metal foil layer to lithium optimizes the distribution of current in the stacking direction; the change in the lithium affinity of the multi-layer polymer layer can avoid excessive lithium-containing byproducts from being coated on the surface of the current collector, thereby ensuring the normal operation of the current collector.

[0010] Wherein, the plurality of through holes are distributed in an array form, and the aperture of the through holes is less than or equal to 10 μm.

[0011] Wherein, the current collector further includes a conductive layer, and the conductive layer is arranged on the inner side wall of the through hole.

[0012] The material of the metal foil layer includes at least one of copper, gold, silver, magnesium, zinc, titanium and nickel, or stainless steel; the material of the polymer layer includes at least one of polyethylene terephthalate, polyether polymer, polycarbonate polymer, polyolefin polymer and polyimide polymer.

[0013] Wherein, the thickness of the metal foil layer is less than or equal to 2 μm, and the thickness of the polymer layer is 6 μm-12 μm.

[0014] The thicknesses of the plurality of metal foil layers are equal, and the thicknesses of the plurality of polymer layers are equal.

[0015] Wherein, the current collector further includes a lithium-containing metal layer, the lithium-containing metal layer is arranged in the metal foil layer, and the thickness of the lithium-containing metal layer is 10nm-2μm.

[0016] Wherein, the current collector also includes a flame retardant layer, the stacking structure has a first surface and a second surface arranged opposite to each other in the stacking direction, the flame retardant layer is arranged on the first surface, and / or the flame retardant layer is arranged on the second surface; the thickness of the flame retardant layer is 10nm-1μm.

[0017] The polymer layer contains a lithium-replenishing material, which includes at least one of Li-Mg, Li-Al, Li-Si, Li-Ag, Li-Au, Li-Sn, Li-In and Li-Ge alloys, and the mass proportion of the lithium-replenishing material in the polymer layer is 0.1wt%-5wt%.

[0018] In a second aspect, the present application also provides a method for preparing a current collector, comprising:

[0019] M layers of metal foil films and M+1 layers of polymer films are alternately stacked in sequence to form a first composite structure, where M is a positive integer greater than 1, and when M≥2, the lithium affinity of the polymer film gradually decreases from the M+1th layer in the first composite structure to both ends in the stacking direction, and / or when M≥3, the lithium affinity of the metal foil film gradually decreases from the M+1th layer in the first composite structure to both ends in the stacking direction;

[0020] Disposing a first protective film and a second protective film respectively on the outermost two sides of the first composite structure in a stacking direction to form a second composite structure;

[0021] forming a plurality of through holes on the second composite structure, wherein the through holes penetrate two opposite surfaces of the second composite structure in the stacking direction;

[0022] The first protective film and the second protective film are removed to obtain a current collector.

[0023] In a third aspect, the present application further provides a negative electrode, which comprises a current collector prepared by the preparation method described in the first aspect or the second aspect.

[0024] In a fourth aspect, the present application further provides an electrochemical energy storage device, which comprises a positive electrode and the negative electrode described in the third aspect.

[0025] Among them, the porosity β of the current collector, the surface capacity C of the positive electrode, the thickness d of the current collector in the stacking direction and the capacity-thickness constant k satisfy the formula:

[0026]

[0027] The β≥50%, the C≥5mAh / cm 2 , k = 5 × 10 -4 cm 3 / mAh. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the technical solutions in the implementation modes of the present application, the drawings required for use in the implementation modes will be briefly introduced below. Obviously, the drawings described below are only some implementation modes of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0029] Figure 1 A schematic top view of a current collector provided in one embodiment of the present application.

[0030] Figure 2 for Figure 1 Schematic cross-sectional view along line II.

[0031] Figure 3 A schematic cross-sectional view of a current collector provided in another embodiment of the present application.

[0032] Figure 4 A schematic cross-sectional view of a current collector provided in another embodiment of the present application.

[0033] Figure 5 A schematic cross-sectional view of a current collector provided in another embodiment of the present application.

[0034] Figure 6 A schematic cross-sectional view of a current collector provided in another embodiment of the present application.

[0035] Figure 7 A method for preparing a current collector provided in one embodiment of the present application.

[0036] Figure 8 A schematic cross-sectional view of an electrochemical energy storage device provided in one embodiment of the present application.

[0037] Description of Figure Numbers:

[0038] Current collector-1, stacking structure-11, polymer layer-111, metal foil layer-112, first surface-113, second surface-114, through hole-12, conductive layer-13, lithium metal containing layer-14, flame retardant layer-15, electrochemical energy storage device-2, positive electrode-21, negative electrode-22, separator-23. DETAILED DESCRIPTION

[0039] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0040] This application provides a current collector 1, please refer to Figure 1 and Figure 2 , Figure 1 A schematic top view of a current collector provided in one embodiment of the present application; Figure 2 for Figure 1The schematic cross-sectional view along line II in FIG. The current collector 1 comprises a stacking structure 11, the stacking structure 11 comprises M layers of metal foil layers 112 and M+1 layers of polymer layers 111, and the metal foil layers 112 and the polymer layers 111 are alternately stacked, and M is a positive integer greater than 1; when M≥2, the lithium affinity of the polymer layer 111 gradually decreases from the M+1th layer in the stacking structure 11 to both ends in the stacking direction; and / or when M≥3, the lithium affinity of the metal foil layer 112 gradually decreases from the M+1th layer in the stacking structure 11 to both ends in the stacking direction, and the current collector 1 has a plurality of through holes 12 penetrating two opposite surfaces of the current collector 1 in the stacking direction.

[0041] The current collector 1 provided in the present application is provided with a through hole 12 that penetrates the current collector 1, which is conducive to the effective infiltration of the current collector 1 by the electrolyte and improves the electrochemical consistency inside the current collector 1; the provision of the through hole 12 increases the specific surface area and internal space of the current collector 1, and these internal spaces accommodate the lithium precipitated during the charging and discharging process, and inhibit the generation of lithium dendrites. Compared with the current collector 1 with a single metal layer, the outermost sides of the stacking structure 11 in the current collector 1 provided in the present application are both polymer layers 111, and the metal foil layer 112 is provided inside the current collector 1, which can induce lithium to be deposited on the metal foil layer 112 inside the current collector 1, avoiding the deposition of lithium on the surface of the current collector 1, and effectively ensuring its performance and safety performance; the single metal layer is subjected to stress during the preparation and use of the current collector 1, and cracks are easily generated, thereby causing some areas to lose electronic conductivity, resulting in an increase in internal resistance, and even adverse phenomena such as short circuits, which is not conducive to the use of the current collector 1, and the current collector 1 provided in the present application A multi-layer metal foil layer 112 is provided, which can effectively disperse the stress and avoid the metal foil layer 112 from breaking, thereby ensuring the performance of the current collector 1; at the same time, from the M+1th layer in the stacking structure 11 to the two ends in the stacking direction, the affinity of the metal foil layer 112 to lithium gradually decreases, which optimizes the distribution of current in the stacking direction, transmits electrons more evenly to the outside, and has better transmission efficiency, which is beneficial to reduce the DC internal resistance of the battery system during application and improve the battery rate performance. In addition, the affinity of the metal foil layer 112 to lithium gradually decreases, so that the metal lithium is preferentially deposited inside the current collector 1 to obtain the smallest volume expansion. During the operation of the current collector 1, lithium-containing by-products generated after the current collector 1 reacts with lithium may be coated on its surface. In the present application, from the M+1th layer in the stacking structure 11 to the two ends in the stacking direction, the lithium affinity of the polymer layer 111 gradually decreases, that is, the stability of the polymer layer 111 to lithium gradually decreases, that is, the polymer layer 111 close to the surface of the stacking structure 11 has a greater reaction activity with lithium, which can accelerate the reaction with lithium-containing by-products, thereby avoiding excessive lithium-containing by-products from coating on the surface of the current collector 1, avoiding the formation of lithium dendrites, avoiding short circuits, improving safety performance, and ensuring the normal operation of the current collector 1. The polymer layer 111 in the middle has strong stability to lithium, can avoid reaction with lithium, reduce lithium loss, and improve cycle performance.

[0042] It should be noted that, in the present application, the outermost two surfaces of the stacking structure 11 in the stacking direction are defined as a first surface 113 and a second surface 114 respectively; Figure 2The arrow in is the stacking direction shown in one embodiment of the present application. Since the metal foil layer 112 and the polymer layer 111 are alternately stacked, and the number of layers of the polymer layer 111 is one more than the number of layers of the metal foil layer 112, the outermost layers of the stacking structure 11 in the stacking direction must be the polymer layer 111, that is, the first surface 113 and the second surface 114 are both the side surfaces of the polymer layer 111 on the outermost sides of the stacking structure 11 in the stacking direction away from the metal foil layer 112. In the present application, from the M+1th layer in the stacking structure 11 to the two ends in the stacking direction can be understood as the M+1th layer in the stacking structure 11 to the first surface 113, and the M+1th layer in the stacking structure 11 to the second surface 114.

[0043] In the present application, the stacking structure 11 is formed by alternately stacking polymer layers 111 and metal foil layers 112 from the first surface 113 to the second surface 114. If the layers in the stacking structure 11 are marked in sequence starting from "1", they can be divided into the 1st layer, the 2nd layer... the M-1th layer, the Mth layer, the M+1th layer, ..., the 2Mth layer, and the 2M+1th layer stacked from the first surface 113 to the second surface 114. It can be understood that since the number of layer structures in the stacking structure 11 is 2M+1 layers, the M+1th layer is the middle layer in the stacking structure 11. When M is an odd number or an even number, the M+1th layer can be the metal foil layer 112 or the polymer layer 111. For example, when M is 3, please refer to Figure 2 , the total number of layers in the stacked structure 11 is 7, the M+1th layer, i.e. the fourth layer, is the metal foil layer 112; when M is 2, please refer to Figure 3 , is a schematic cross-sectional view of a current collector provided in another embodiment of the present application. The total number of layer structures in the stacking structure 11 is 5 layers, and the M+1th layer, i.e. the third layer, is a polymer layer 111.

[0044] In the present application, when M≥2, the lithium affinity of the polymer layer 111 gradually decreases from the M+1th layer in the stacking structure 11 to both ends in the stacking direction; and / or when M≥3, the lithium affinity of the metal foil layer 112 gradually decreases from the M+1th layer in the stacking structure 11 to both ends in the stacking direction. In one embodiment, M≥2, the lithium affinity of the polymer layer 111 gradually decreases from the M+1th layer in the stacking structure 11 to both ends in the stacking direction. In another embodiment, M≥3, the lithium affinity of the metal foil layer 112 gradually decreases from the M+1th layer in the stacking structure 11 to both ends in the stacking direction. In yet another embodiment, M≥3, the lithium affinity of the polymer layer 111 gradually decreases from the M+1th layer in the stacking structure 11 to both ends in the stacking direction, and the lithium affinity of the metal foil layer 112 gradually decreases from the M+1th layer in the stacking structure 11 to both ends in the stacking direction.

[0045] It can be understood that, since the current collector 1 has through holes 12 , the polymer layer 111 and the metal foil layer 112 are both porous layer structures.

[0046] In the present application, the setting of the polymer layer 111 avoids the deposition of lithium on the surface of the current collector 1, effectively ensuring its performance and safety performance; when the lithium affinity of the polymer layer 111 gradually decreases from the M+1 layer to the two ends in the stacking direction in the stacking structure 11, the polymer layers 111 on the outermost sides of the adjacent stacking structure 11 in the stacking direction have a strong reaction activity with lithium, which can accelerate the reaction with lithium-containing by-products, thereby avoiding excessive lithium-containing by-products from coating the surface of the current collector 1, avoiding the occurrence of lithium dendrites and short circuits, and ensuring the normal operation of the current collector 1. The polymer layer 111 close to the middle of the stacking structure 11 has strong stability to lithium, low reaction activity with lithium, can avoid reaction with lithium, reduce lithium loss, and improve cycle performance.

[0047] In this embodiment, the material of the polymer layer 111 includes at least one of polyethylene terephthalate, polyether polymers, polycarbonate polymers, polyolefin polymers and polyimide polymers. Specifically, the material of the polymer layer 111 may be, but is not limited to, one or more of polyethylene terephthalate, polyethylene, polypropylene, polyimide, polytetrafluoroethylene, polyvinylidene fluoride, polycarbonate and polyether. In one embodiment, the multilayer polymer layer 111 in the stacked structure 11 includes at least one layer of polyether polymer layer and at least one layer of polycarbonate polymer layer, and the stability of the polyether polymer layer to lithium is higher than the stability of the polycarbonate polymer layer to lithium. When the M+1th layer is the polymer layer 111, the material of the polymer layer 111 of the M+1th layer may be a polyether polymer with high stability to lithium, and the polymer layers 111 from the M+1th layer in the stacking structure 11 to the two ends in the stacking direction may be polycarbonate polymers with reduced stability to lithium; similarly, when the M+1th layer is the metal foil layer 112, the material of the polymer layer 111 of the adjacent M+1th layer may be a polyether polymer with high stability to lithium, and the polymer layers 111 from the M+1th layer in the stacking structure 11 to the two ends in the stacking direction may be polycarbonate polymers with reduced stability to lithium.

[0048] In this embodiment, the polycarbonate polymer includes an aliphatic polycarbonate polymer (PBC). In one embodiment of the present application, the structural formula of the aliphatic polycarbonate polymer is

[0049]

[0050] Among them, 3≤n≤10000, R 1 , R 2 , R 3 and R 4At least one of them is -F, -CF 3 , -CHF 2 and -(CH 2 ) k At least one of F, k is a positive integer, 2≤k≤10. In one embodiment, R 1 In another embodiment, R 1 For -F, R 3 -CHF 2 , n is 500. In yet another embodiment, R 3 -CH 2 F 2 , R 4 For-CF 3 , n is 2000.

[0051] In this embodiment, the polyether polymer includes polyether polyaluminium chloride (PAC). In one embodiment of the present application, the structural formula of polyether polyaluminium chloride is

[0052]

[0053] Among them, 3≤m≤10000, R 5 , R 6 , R 7 and R 8 At least one of them is -F, -CF 3 , -CHF 2 and -(CH 2 ) p At least one of F, p is a positive integer, 2≤p≤10. In one embodiment, R 5 In another embodiment, R 5 For -F, R 6 -CH 2 CH 2 F 2 , n is 1000. In yet another embodiment, R 5 -CH 2 F 2 , R 7 For-CF 3 , n is 3000.

[0054] In this embodiment, the thickness of the polymer layer 111 is 6μm-12μm. That is, the thickness of each polymer layer 111 in the stacking direction is 6μm-12μm, and the thickness of the multiple polymer layers 111 may be the same or different. Further, the thickness of the polymer layer 111 is 8μm-10μm. Specifically, the thickness of the polymer layer 111 may be, but is not limited to, 6μm, 7μm, 8μm, 11μm, 12μm, etc. In this embodiment. In one embodiment, the thickness of the plurality of polymer layers 111 is equal. In other words, the thickness of each layer in the M+1 layer of polymer layers 111 is equal, so that the chemical reaction of different parts of the current collector 1 is more evenly distributed, further improving the electrochemical performance of the current collector 1.

[0055] In the present application, each layer in the multi-layer polymer layer 111 has different stability to lithium. As the working time of the current collector 1 increases, the thickness of the lithium-containing by-products on each polymer layer 111 is different. For example, after the same working time, the thickness of the lithium-containing by-products on the polymer layer 111 with poor stability to lithium is less than the thickness of the lithium-containing by-products on the polymer layer 111 with good stability to lithium.

[0056] In this embodiment, the polymer layer 111 contains lithium supplementing materials. Thus, the consumed lithium is replenished during the charge and discharge process, and the energy density and cycle life are improved. That is to say, at least one of the M+1 polymer layers 111 contains lithium supplementing materials. Specifically, it can be, but not limited to, one polymer layer 111 contains lithium supplementing materials, or two polymer layers 111 contain lithium supplementing materials, or M+1 polymer layers 111 contain lithium supplementing materials, etc. In the present application, the two outermost layers of the stacked structure 11 are both polymer layers 111, that is, the first layer and the 2M+1 layer are polymer layers 111; when the first layer and / or the 2M+1 layer contain lithium supplementing materials, the first surface 113 and / or the second surface 114 are insulated, thereby ensuring that metallic lithium is not deposited on the first surface 113 and / or the second surface 114. Further, the lithium supplementing material includes at least one of Li-Mg, Li-Al, Li-Si, Li-Ag, Li-Au, Li-Sn, Li-In and Li-Ge alloys. Thus, lithium can be effectively supplemented. Furthermore, the mass proportion of the lithium supplement material in the polymer layer 111 is 0.1wt%-5wt%, which is beneficial to the supplement of lithium and does not affect the insulation performance of the polymer layer 111. Specifically, the mass proportion of the lithium supplement material in the polymer layer 111 may be, but is not limited to, 0.1wt%, 0.5wt%, 1wt%, 2wt%, 3wt% or 4wt%, etc. It can be understood that when at least two polymer layers 111 contain lithium supplement materials, the material and content of the lithium supplement materials in different polymer layers 111 may be the same or different. In the present application, when the polymer layer 111 adopts the above-mentioned content of lithium supplement material, the electronic conductivity of the polymer layer 111 is relatively low, thereby ensuring that metallic lithium will not be preferentially deposited on the surface of the polymer layer 111. In one embodiment, the first surface 113 of the stacked structure 11 is insulated, and the second surface 114 of the stacked structure 11 is insulated. Specifically, the first surface 113 of the stacked structure 11 is insulated, that is, the first surface 113 of the stacked structure 11 has no electronic conductivity; similarly, the second surface 114 of the stacked structure 11 is insulated, that is, the second surface 114 of the stacked structure 11 has no electronic conductivity. It can be understood that this arrangement prevents lithium from being deposited on the first surface 113 and the second surface 114 of the stacked structure 11, avoids the generation of dead lithium, and also prolongs the service life of the current collector 1.

[0057] In the present application, the metal foil layer 112 disposed inside the current collector 1 ensures that lithium is preferentially deposited inside the current collector 1, avoids the generation of lithium dendrites, and is beneficial to the improvement of its electrochemical performance; the single-layer metal layer is subjected to stress during the preparation and use of the current collector 1, and is prone to cracks, thereby causing a partial area to lose electronic conductivity, resulting in an increase in internal resistance, and even undesirable phenomena such as short circuits, which is not conducive to the use of the current collector 1. The current collector 1 provided in the present application is provided with a multi-layer metal foil layer 112, which can effectively disperse the stress and avoid the metal foil layer 112 from breaking, thereby ensuring the performance of the current collector 1. The stacking structure 11 in the current collector 1 is arranged so that the metal foil layer 112 is arranged inside the current collector 1, which can induce lithium to be deposited on the metal foil layer 112 inside the current collector 1, inhibit the generation of lithium dendrites, avoid the generation of dead lithium, reduce interface impedance, avoid the loss of active lithium, and improve electrochemical performance and safety of use. The change in the affinity of the multi-layer metal foil layer 112 for lithium ensures that lithium is preferentially deposited inside the current collector 1, while optimizing the distribution of current in the stacking direction, transmitting electrons more evenly outward with better transmission efficiency, which is beneficial to reducing the DC internal resistance of the battery system during application, improving the battery rate performance, and also facilitating the deposition of metallic lithium into the interior of the current collector 1 to obtain minimal volume expansion.

[0058] It should be noted that the lithium affinity of the material of the metal foil layer 112 can be distinguished by the increase of lithium deposition time, and the thickness of the deposited lithium on the metal foil layers 112 of different materials is different, so that the overpotential of the metal foil layers 112 of different materials is different. For example, under the same lithium deposition time, more lithium is deposited on the metal foil layer 112 with good lithium affinity, so the overpotential of the metal foil layer 112 with good lithium affinity is greater than the overpotential of the metal foil layer 112 with poor lithium affinity.

[0059] In this embodiment, the material of the metal foil layer 112 includes at least one of copper, gold, silver, magnesium, zinc, titanium and nickel or stainless steel. Specifically, the metal foil layer 112 can be, but is not limited to, copper foil, copper alloy foil, stainless steel foil, silver foil, titanium foil or nickel foil. In one embodiment, the metal foil layer 112 is copper foil or copper alloy foil. For example, when the M+1th layer is a metal foil layer 112, the material of the metal foil layer 112 of the M+1th layer may be a composite metal of copper and a first metal having a higher affinity for lithium, wherein the first metal includes one or more of gold, silver, magnesium, zinc, indium, etc., and the affinity of the metal foil layer 112 to lithium decreases from the M+1th layer in the stacking structure 11 to the two ends in the stacking direction, and the material of the outermost metal foil layer 112 of the stacking structure 11 may be but is not limited to copper element; similarly, when the M+1th layer is a polymer layer 111, the material of the metal foil layer 112 of the adjacent M+1th layer may be a composite metal of copper and a first metal having a higher affinity for lithium, and the affinity of the metal foil layer 112 to lithium decreases from the M+1th layer in the stacking structure 11 to the two ends in the stacking direction, and the material of the outermost metal foil layer 112 of the stacking structure 11 may be but is not limited to copper element.

[0060] In this embodiment, the thickness of the metal foil layer 112 is less than or equal to 2μm. That is, the thickness of each metal foil layer 112 in the stacking direction is less than or equal to 2μm, and the thickness of the multiple metal foil layers 112 may be the same or different. Further, the thickness of the metal foil layer 112 is 0.2μm-1.5μm. Specifically, the thickness of the metal foil layer 112 may be, but is not limited to, 0.5μm, 0.7μm, 0.8μm, 1.1μm, 1.4μm, etc. In one embodiment, the thickness of the multiple metal foil layers 112 is equal. In other words, the thickness of each layer in the M layers of metal foil layers 112 is equal, so that the chemical reaction of different parts of the current collector 1 is more even, further improving the electrochemical performance of the current collector 1.

[0061] In this embodiment, the thickness of the metal foil layer 112 is less than the thickness of the polymer layer 111, so that the metal foil layer 112 accounts for a smaller proportion in the overall current collector 1, which can reduce the mass and volume proportion of the inactive ingredients and improve the energy density of the current collector 1; at the same time, the setting of the through hole 12 will not excessively affect the strength of the current collector 1, which is beneficial to increase the pore size of the through hole 12 and the porosity of the current collector 1.

[0062] In the present application, the current collector 1 has a plurality of through holes 12 penetrating two opposite surfaces of the current collector 1 in the stacking direction. The current collector 1 is provided with through holes 12 penetrating the current collector 1, which is conducive to the effective infiltration of the current collector 1 by the electrolyte and improves the electrochemical consistency inside the current collector 1; at the same time, the provision of the through holes 12 increases the specific surface area and internal space of the current collector 1, and these internal spaces accommodate the lithium precipitated during the charge and discharge process and inhibit the generation of lithium dendrites.

[0063] In this embodiment, the through holes 12 are distributed in an array. The through holes 12 are evenly distributed in an array, which is conducive to the uniform deposition of lithium precipitated during the charge and discharge process, avoiding excessive local lithium deposition and protrusion, and further improving the safety performance.

[0064] In this embodiment, the aperture of the through hole 12 is less than or equal to 10 μm. Further, the aperture of the through hole 12 is less than 8 μm. Specifically, the aperture of the through hole 12 can be, but is not limited to, 3 μm, 4 μm, 5 μm, 6 μm, 8 μm, etc. By providing the through hole 12 with a small aperture, it is further ensured that the electrolyte passes through the through hole 12 slowly, and the current collector 1 is well immersed in the electrolyte, thereby further improving the consistency of the electrochemical performance.

[0065] In this embodiment, the aperture shape of the through hole 12 in the current collector 1 includes at least one of a cylindrical, rectangular tube, cubic tube, trapezoidal cylindrical, and triangular pyramidal shape. The present application does not limit the aperture shape of the through hole 12. Specifically, the cross-section of the through hole 12 may be, but is not limited to, a polygonal, circular, elliptical, irregular shape, etc., and the longitudinal section of the through hole 12 may be, but is not limited to, a rectangular, trapezoidal, quasi-trapezoidal, conical, quasi-conical, irregular shape, etc. In one embodiment, the inner side wall of the through hole 12 is inclined, and the cross-section of the through hole 12 gradually increases from the M+1 layer to both ends in the stacking direction. Thereby increasing the specific surface area of ​​the through hole 12, which is beneficial to the deposition of lithium. Please refer to Figure 1 and Figure 2 , wherein the aperture shape of the through hole 12 is cylindrical. Figure 3 , wherein the aperture longitudinal section of the through hole 12 is a trapezoidal shape. In one embodiment, when the cross section of the through hole 12 is circular and the longitudinal section is a trapezoidal shape, the through hole 12 is a trapezoidal cylindrical shape. Further, the aperture longitudinal section of the through hole 12 is a trapezoidal shape, wherein the short sides of two trapezoids intersect, and the cross section of the through hole 12 gradually increases from the M+1th layer to both ends in the stacking direction. In this embodiment, as Figure 3As shown, the aperture of the through hole 12 adjacent to the first surface 113 or the second surface 114 is larger than the aperture of the through hole 12 away from both the first surface 113 and the second surface 114. It can be understood that when the current collector 1 has a conductive layer 13, this arrangement makes it easier for the conductive material to be deposited on the inner wall of the through hole 12 and to be deposited inside the stacked structure 11, thereby avoiding clogging the through hole 12.

[0066] In one embodiment, please refer to Figure 4 , Figure 4 A schematic cross-sectional view of a current collector provided in another embodiment of the present application, the current collector 1 further includes a conductive layer 13, and the conductive layer 13 is disposed on the inner side wall of the through hole 12. It can be understood that the conductive layer 13 does not block the through hole 12, and the interior of the current collector 1 still has a hollow space. By disposing the conductive layer 13 in the through hole 12, metallic lithium can be deposited in the internal space of the current collector 1, avoiding deposition on the surface of the current collector 1, effectively reducing the formation of dead lithium, and improving the electrochemical performance.

[0067] In one embodiment, by depositing or impregnating a conductive material on the inner side wall of the through hole 12 to form a conductive layer 13, the phenomenon of byproduct generation can be effectively reduced, thereby extending the service life of the current collector 1. In one embodiment, the material of the conductive layer 13 includes at least one of a metal material, a carbon material, and a conductive polymer material. Specifically, the material of the conductive layer 13 includes at least one of gold, silver, copper, nickel, iron, aluminum, germanium, tin, zinc, indium, vanadium, magnesium, cobalt, carbon, polyaniline, and polypyrrole. In this embodiment, from the M+1 layer in the stacking structure 11 to both ends in the stacking direction, the lithium affinity of the metal foil layer 112 gradually decreases, so that when the conductive material is deposited or impregnated on the inner side wall of the through hole 12, the conductive material will be preferentially deposited on the inner side wall of the through hole 12 adjacent to the M+1 layer, avoiding excessive deposition of the conductive material on the inner side wall of the through hole 12 adjacent to the first surface 113 or the second surface 114, effectively reducing the overall thickness of the current collector 1 and the risk of clogging the through hole 12.

[0068] Please also read Figure 5 , Figure 5A schematic cross-sectional view of a current collector provided in another embodiment of the present application. The current collector 1 also includes a lithium-containing metal layer 14, which is disposed in the metal foil layer 112. By providing a lithium-containing metal layer 14, the lithium consumed by the reaction between the electrolyte and the deposited lithium can be supplemented, thereby improving the energy density and cycle life. In one embodiment, the material of the lithium-containing metal layer 14 may include at least one of a lithium element and a lithium alloy. Specifically, the lithium alloy includes at least one of Li-Ag, Li-Mg, Li-Zn, Li-AL, Li-Au, Li-Si, Li-Sn and Li-Ge alloys. In one embodiment, the thickness of the lithium-containing metal layer 14 is 10nm-2μm. Further, the thickness of the lithium-containing metal layer 14 is 100nm-1.5μm. Further, the thickness of the lithium-containing metal layer 14 is 300nm-1000nm. Specifically, the thickness of the lithium-containing metal layer 14 may be, but is not limited to, 100 nm, 400 nm, 500 nm, 800 nm, 1 μm, 1.5 μm, 1.8 μm, 2 μm, etc. In one embodiment, the lithium-containing metal layer 14 is disposed inside the metal foil layer 112. That is, the lithium-containing metal layer 14 is coated by the metal foil layer 112. In another embodiment, the metal foil layer 112 includes a first porous metal layer and a second porous metal layer, and the first porous metal layer, the lithium-containing metal layer 14 and the second porous metal layer are stacked in sequence. It should be noted that the through hole 12 also passes through the lithium-containing metal layer 14, and the first porous metal layer and the second porous metal layer are counted as one layer of metal foil layer 112 in number.

[0069] Please also read Figure 6 , Figure 6A schematic cross-sectional view of a current collector provided for another embodiment of the present application, wherein the current collector 1 further includes a flame retardant layer 15, the flame retardant layer 15 is disposed on the first surface 113 of the stacked structure 11, and / or the flame retardant layer 15 is disposed on the second surface 114 of the stacked structure 11. When the current collector 1 is used in the electrochemical energy storage device 2, the metal lithium is highly active, and it is easy to cause the combustion of the electrochemical energy storage device 2 when a short circuit occurs, causing a safety accident. By providing the flame retardant layer 15, in the early stage of the short circuit, the flame retardant layer 15 can be melted by heat, and the holes can be blocked, and the metal lithium deposited in the through hole 12 can be wrapped to avoid further contact between the metal lithium and the electrolyte to cause thermal runaway, and the melted flame retardant layer 15 can block the opening of the through hole 12 of the adjacent first surface 113, and / or the opening of the through hole 12 of the second surface 114, isolating the ion channel, eliminating safety hazards, and improving safety in use. Further, the melting point of the material of the flame retardant layer 15 is 120°C-155°C. The use of low melting point flame retardant materials is more conducive to flame retardancy. It should be noted that when the flame retardant layer 15 is arranged on the first surface 113 of the stacking structure 11, and / or the second surface 114 of the stacking structure 11, the through hole 12 also penetrates the flame retardant layer 15; that is, the flame retardant layer 15 is also provided with a plurality of holes, and the holes are correspondingly connected to the through holes 12. In this embodiment, the material of the flame retardant layer 15 includes one or more of polyethylene wax, polypropylene wax and polyethylene oxide wax. In this embodiment, in order not to affect the overall thickness of the current collector 1, the thickness of the flame retardant layer 15 is relatively small, and its thickness range can be but is not limited to 10nm-1μm, 50nm-0.8μm, 100nm-0.7μm or 200nm-0.5μm, etc.

[0070] The present application does not specifically limit the specific preparation method of the current collector 1. Next, an example of a preparation method of the current collector 1 provided in the present application will be described.

[0071] This application also provides a method for preparing the current collector 1, please refer to Figure 7 , Figure 7 The method for preparing a current collector provided in one embodiment of the present application includes steps S701, S702, S703, and S704. Steps S701, S702, S703, and S704 are described in detail as follows.

[0072] S701: M layers of metal foil film and M+1 layers of polymer film are alternately stacked in sequence to form a first composite structure, where M is a positive integer greater than 1, and when M≥2, the lithium affinity of the polymer film gradually decreases from the M+1th layer in the first composite structure to the two ends in the stacking direction, and / or when M≥3, the lithium affinity of the metal foil film gradually decreases from the M+1th layer in the first composite structure to the two ends in the stacking direction.

[0073] In one embodiment, the M layers of metal foil and the M+1 layers of polymer films are alternately stacked in sequence, including: depositing metal on the first layer of polymer film to form a metal foil; and then forming a second layer of polymer film on the metal foil by at least one of liquid coating, atomic deposition and melt extrusion calendering processes, and cyclically replicating to obtain a first composite structure. Specifically, the deposition can be, but is not limited to, magnetron sputtering, ion plating, vacuum evaporation, etc. Further, the first layer of polymer film can be installed in a vacuum magnetron sputtering coating machine, and a vacuum pump can be used to evacuate the chamber to a vacuum degree of 8×10 -2 Pa, and then a certain amount of argon is introduced to adjust the vacuum degree to 2×10 -1 Pa, the first layer of polymer film is cleaned by a surface ion source for 5min-15min. After the cleaning is completed, the ion source power is turned off; the metal plating power is started to magnetron sputter the metal foil film for 5min-100min to obtain a metal foil film with a thickness less than or equal to 2μm. In another embodiment, M layers of metal foil film and M+1 layers of polymer film are alternately stacked in sequence, including: providing a substrate, depositing metal on the substrate, peeling to form a metal foil film; then forming a polymer film on the two opposite surfaces of the metal foil film through at least one of liquid coating, atomic deposition and melt extrusion calendering processes, and then depositing metal on the outer surfaces of the two polymer films to form a metal foil film, and cyclically replicating to obtain a first composite structure.

[0074] S702: Disposing a first protective film and a second protective film respectively on two outermost surfaces of the first composite structure in a stacking direction to form a second composite structure.

[0075] In this embodiment, the first protective film and the second protective film may be, but are not limited to, at least one of transparent adhesive, engineering paper, and plastic wrap.

[0076] S703: forming a plurality of through holes on the second composite structure, wherein the through holes penetrate two opposite surfaces of the second composite structure in the stacking direction.

[0077] In this embodiment, the through hole 12 penetrates the second composite structure, so that the polymer film and the metal foil film form a porous structure, and the polymer layer 111 and the metal foil layer 112 are obtained respectively.

[0078] In this embodiment, multiple through holes 12 may be formed on the second composite structure by, but are not limited to, ultrafast laser.

[0079] S704: Remove the first protective film and the second protective film to obtain a current collector.

[0080] In this embodiment, the preparation method of the current collector 1 further includes depositing a conductive material on the inner side wall of the through hole 12 to form a conductive layer 13 before removing the first protective film and the second protective film. Specifically, the conductive material can be disposed on the inner side wall of the through hole 12 by thermal evaporation sputtering, magnetron sputtering or dipping to form the conductive layer 13. It should be noted that by controlling the length of time for depositing the conductive material, the conductive material can be controlled to be partially deposited on the inner side wall of the through hole 12, thereby avoiding the conductive material from blocking the through hole 12 due to excessive deposition time.

[0081] The present application also provides a negative electrode 22, and the negative electrode 22 includes the current collector 1 in any of the above embodiments. Specifically, the current collector 1 is described above and will not be described again here. In the present application, the current collector 1 can be used directly as the negative electrode 22, and the negative electrode 22 does not need to be provided with a negative electrode active material layer. At this time, the negative electrode 22 is the current collector 1, that is, a lithium-free negative electrode; when the current collector 1 provided in the present application is used as the negative electrode 22, the electrochemical performance and safety performance of the negative electrode 22 can be greatly improved.

[0082] The present application also provides an electrochemical energy storage device 2, which includes the negative electrode 22 as described above. Figure 8 , is a cross-sectional schematic diagram of an electrochemical energy storage device provided in one embodiment of the present application, wherein the electrochemical energy storage device 2 includes a positive electrode 21 and a negative electrode 22. In one embodiment, the current collector 1 serves as the negative electrode 22 of the electrochemical energy storage device 2.

[0083] Specifically, in the present embodiment, the electrochemical energy storage device 2 is a lithium-free negative electrode-lithium battery, that is, a negative electrode-free battery. In other possible embodiments, the electrochemical energy storage device 2 may also be other types of batteries, which is not limited in the present application.

[0084] In this embodiment, the porosity β of the current collector 1, the surface capacity C of the positive electrode 21, the thickness d of the current collector 1 in the stacking direction, and the capacity-thickness constant k satisfy the formula:

[0085]

[0086] Where k = 5 × 10 -4 cm 3 / mAh.

[0087] It should be noted that, in general, the electrochemical energy storage device 2 includes a positive electrode 21 and a negative electrode 22, and the current collector 1 serves as the negative electrode 22 of the electrochemical energy storage device 2. The porosity β of the current collector 1 refers to the percentage of the total volume of the through-holes 12 to the total volume of the current collector 1, and the surface capacity of the positive electrode 21 refers to the total number of electrons that can be released per unit surface area of ​​the positive electrode 21 of the electrochemical energy storage device 2. By setting the porosity of the current collector 1 and the thickness of the current collector 1, the surface capacity of the positive electrode 21 can be increased, thereby increasing the overall energy density. In one embodiment, β ≥ 50%, C ≥ 5mAh / cm 2 The higher porosity can ensure that the space required for lithium deposition can be met when the thickness of the current collector 1 is relatively low, avoiding the volume expansion caused by disordered lithium deposition and improving the safety performance of the current collector 1. Furthermore, β ≥ 60%, C ≥ 6 mAh / cm 2 .

[0088] In this embodiment, the positive electrode 21 includes a positive electrode current collector and a positive electrode active material layer. In one embodiment, the material of the positive electrode active material layer includes LiFe a Mn b M c PO 4 , Li 3 V 2 (PO 4 ) 3 , Li 3 V 3 (PO 4 ) 3 、LiNi 0.5-d Mn 1.5-e N d + e O 4 、LiVPO 4 F. Li 1 + f L 1-g-h H g R h O 2 , Li 2 CuO 2 , Li 5 FeO 4One or more of; wherein, 0≤a≤1, 0≤b≤1, 0≤c≤1, a+b+c=1, M is at least one of Al, Mg, Ga, Ti, Cr, Cu, Zn, and Mo; -0.1≤d≤0.5, 0≤e≤1.5, N is at least one of Li, Co, Fe, Al, Mg, Ca, Ti, Mo, Cr, Cu, and Zn; -0.1≤f≤0.2, 0≤g≤1, 0≤h≤1, 0≤g+h≤1.0, L, H, and R are independently selected from at least one of Li, Co, Mn, Ni, Fe, Al, Mg, Ga, Ti, Cr, Cu, Zn, Mo, F, I, S, and B. In a specific embodiment, the material of the positive electrode active material layer includes LiAl 0.05 Co 0.15 Ni 0.80 O 2 、LiNi 0.80 Co 0.10 Mn 0.10 O 2 、LiNi 0.90 Co 0.05 Mn 0.05 O 2 、LiNi 0.60 Co 0.20 Mn 0.20 O 2 、LiCoO 2 、LiMn 2 O 4 、LiFePO 4 、LiMnPO 4 、LiNiPO 4 、LiCoPO 4 、LiNi 0.5 Mn 1.5 O 4 and Li 3 V 3 (PO 4 ) 3 In another specific embodiment, the material of the positive electrode active material layer includes lithium sulfide, lithium-intercalated V 2 O 5 , Lithium-intercalated MnO 2 , Li-intercalated TiS 2 and lithium-intercalated FeS 2 At least one of .

[0089] In this embodiment, the electrochemical energy storage device 2 further includes a separator 23 disposed between the positive electrode 21 and the negative electrode 22. The separator 23 is used to separate the positive electrode 21 and the negative electrode 22 of the electrochemical energy storage device 2, and the present application does not limit the material of the separator 23.

[0090] The electrochemical energy storage device 2 provided in the embodiment of the present application includes the above-mentioned current collector 1, and the current collector 1 enables the electrochemical energy storage device 2 to have a high energy density, a high charge and discharge capacity, is not prone to the generation of lithium dendrites, has high safety performance, and a long cycle life.

[0091] Next, the implementation methods of the present application will be further described with reference to a number of examples.

[0092] Example 1

[0093] A method for preparing a current collector, comprising:

[0094] (1) A PET polymer film (9 μm thick) substrate roll was installed in a vacuum magnetron sputtering coating machine and the vacuum degree of the chamber was evacuated by a vacuum pump to 8 × 10 -2 Pa, and then a certain amount of argon is introduced to adjust the vacuum degree to 2×10 - 1 Pa, the polymer film is cleaned by ion source on the surface for 5 minutes. After the cleaning is completed, the ion source power is turned off; then the copper plating power is started to perform the magnetron sputtering copper plating process. The sputtering copper foil time is 8 minutes, and the thickness of the copper foil is 1 μm;

[0095] (2) using a melt extrusion calender (melting temperature set at 300° C.) to calender the surface of the PET plated with metallic copper to prepare a PET film with a thickness of about 9 μm;

[0096] (3) Repeating step (1) in sequence, increasing the sputtering time to 20 min, and the thickness of the metal copper foil is 2 μm; then repeating steps (2), (1) and (2) in sequence to obtain a first composite structure, wherein the first composite structure comprises a stacked arrangement of a 9 μm thick PET polymer film A, a 1 μm thick metal copper foil, a 9 μm thick PET polymer film B, a 2 μm thick metal copper foil, a 9 μm thick PET polymer film C, a 1 μm thick metal copper foil, and a 9 μm thick PET polymer film D, wherein the stability of the PET polymer film B to lithium is greater than the stability of the PET polymer film A to lithium, and the stability of the PET polymer film C to lithium is greater than the stability of the PET polymer film D to lithium, wherein the material of the PET polymer film A and the PET polymer film D are the same, and the material of the PET polymer film B and the PET polymer film C are the same;

[0097] (4) a layer of transparent adhesive protective film is respectively attached to the outer surfaces of the PET polymer film A and the PET polymer film D in the first composite structure, and then a plurality of through holes arranged in an array are formed on the first composite structure by ultrafast laser, wherein the through holes penetrate two opposite surfaces of the composite structure in the stacking direction, and the aperture of the through holes is 10 μm, thereby obtaining a porous composite layer;

[0098] (5) The porous composite layer was transferred to the thermal evaporator and the vacuum pump was evacuated to a vacuum degree of 4×10 -1 Pa, raise the temperature to 700°C, deposit metallic copper on the inner wall surface of the through hole in the porous composite layer for 10 min, cool to 100°C, turn off the vacuum, take out the porous composite layer and peel off the transparent adhesive protective layer to obtain the current collector Z1 with a porosity of 75%.

[0099] Example 2

[0100] A method for preparing a current collector, comprising:

[0101] (1) A PET polymer film (thickness 6 μm) substrate roll was installed in a vacuum magnetron sputtering coating machine, and a vacuum pump was used to evacuate the chamber to a vacuum degree of 8 × 10 -2 Pa, and then a certain amount of argon is introduced to adjust the vacuum degree to 2×10 - 1 Pa, the polymer film is cleaned by ion source on the surface for 5 minutes. After the cleaning is completed, the ion source power is turned off; then the copper plating power is started to perform magnetron sputtering copper plating process. The sputtering copper foil time is 5 minutes, and the thickness of the copper foil is 0.5 μm;

[0102] (2) using a melt extrusion calender (melting temperature set at 300° C.) to calender the surface of the PET plated with copper to prepare a PET film with a thickness of about 6 μm;

[0103] (3) Repeating step (1) in sequence, increasing the sputtering time to 8 min, the thickness of the metal copper foil is 1 μm, and then repeating the above steps in sequence to obtain a first composite structure, wherein the first composite structure comprises a stacked 6 μm thick PET polymer film A, a 0.5 μm thick metal copper foil, a 6 μm thick PET polymer film B, a 1 μm thick metal copper foil, a 6 μm thick PET polymer film C, a 1 μm thick metal copper foil, a 6 μm thick PET polymer film D, a 1 μm thick metal copper foil, a 6 μm thick PET polymer film F, a 0.5 μm thick metal copper foil, a 6 μm thick PET polymer film E, and the stability to lithium is: PET polymer film A<PET polymer film B<PET polymer film C, PET polymer film E<PET polymer film F<PET polymer film D;

[0104] (4) a layer of transparent adhesive protective film is respectively attached to the outer surfaces of the PET polymer film A and the PET polymer film E in the first composite structure, and then a plurality of through holes arranged in an array are formed on the first composite structure by ultrafast laser, wherein the through holes penetrate two opposite surfaces of the composite structure in the stacking direction, and the aperture of the through holes is 10 μm, thereby obtaining a porous composite layer;

[0105] (5) The porous composite layer was transferred to the thermal evaporator and the vacuum pump was evacuated to a vacuum degree of 4×10 -1 Pa, raise the temperature to 700°C, deposit metallic copper on the inner wall surface of the through hole in the porous composite layer for 10 minutes, cool to 100°C, turn off the vacuum, take out the porous composite layer and peel off the transparent adhesive protective layer to obtain the current collector Z2 with a porosity of 75%.

[0106] Example 3

[0107] A method for preparing a current collector, comprising:

[0108] (1) A PET polymer film (thickness 6 μm) substrate roll was installed in a vacuum magnetron sputtering coating machine, and a vacuum pump was used to evacuate the chamber to a vacuum degree of 8 × 10 -2 Pa, and then a certain amount of argon is introduced to adjust the vacuum degree to 2×10 - 1 Pa, the polymer film is cleaned by ion source on the surface for 5 minutes. After the cleaning is completed, the ion source power is turned off; then the copper plating power is started to perform the magnetron sputtering copper plating process. At the same time of copper plating, the silver plating power is turned on. The sputtering copper foil time is 5 minutes, and the thickness of the metal copper foil is 0.5μm;

[0109] (2) using a melt extrusion calender (melting temperature set at 300° C.) to calender the surface of the PET plated with copper to prepare a PET film with a thickness of about 6 μm;

[0110] (3) Repeat step (1) in sequence, change the silver target to a magnesium target, turn on the power supply for magnesium plating while plating copper, increase the sputtering time to 8 min, and the thickness of the metal copper-silver composite foil is 1 μm;

[0111] (4) Steps (2) and (3) are then repeated in sequence, but only copper plating is performed at this time, and the sputtering is performed for 8 minutes, and the thickness of the metal copper-magnesium composite foil is 1 μm;

[0112] (5) Steps (2), (3), (2), (1) and (2) are sequentially repeated to obtain a first composite structure, wherein the first composite structure sequentially comprises a stacked 6 μm thick PET polymer film A, a 0.5 μm thick metal copper foil, a 6 μm thick PET polymer film B, a 1 μm thick metal copper-magnesium composite foil, a 6 μm thick PET polymer film C, a 1 μm thick metal copper-silver composite foil, a 6 μm thick PET polymer film D, a 1 μm thick metal copper-magnesium composite foil, a 6 μm thick PET polymer film F, a 0.5 μm thick metal copper foil, and a 6 μm thick PET polymer film E, wherein the stability to lithium is: PET polymer film A<PET polymer film B<PET polymer film C, PET polymer film E<PET polymer film F<PET polymer film D, and the affinity to lithium is: metal copper-silver composite foil>metal copper-magnesium composite foil>metal copper foil;

[0113] (6) a layer of transparent adhesive protective film is attached to both sides of the first composite structure, and then a plurality of through holes arranged in an array are formed on the first composite structure by ultrafast laser, wherein the through holes penetrate two opposite surfaces of the composite structure in the stacking direction, and the aperture of the through holes is 10 μm, thereby obtaining a porous composite layer;

[0114] (7) The porous composite layer was transferred to a thermal evaporator and the vacuum pump was used to evacuate the chamber until the vacuum degree reached 4×10 -1 Pa, raise the temperature to 700°C, deposit metallic copper on the inner wall surface of the through hole in the porous composite layer for 10 min, cool to 100°C, turn off the vacuum, take out the porous composite layer and peel off the transparent adhesive protective layer to obtain the current collector Z3 with a porosity of 75%.

[0115] Example 4

[0116] A method for preparing a current collector, comprising:

[0117] (1) A PET polymer film (thickness 12 μm) substrate roll was installed in a vacuum magnetron sputtering coating machine, and a vacuum pump was used to evacuate the chamber to a vacuum degree of 8×10 -2 Pa, and then a certain amount of argon is introduced to adjust the vacuum degree to 2×10 - 1 Pa, the polymer film is cleaned by ion source on the surface for 5 minutes. After the cleaning is completed, the ion source power is turned off; then the copper plating power is started to perform the magnetron sputtering copper plating process. The sputtering copper foil time is 8 minutes, and the thickness of the copper foil is 1 μm;

[0118] (2) using a melt extrusion calender (melting temperature set at 300° C.) to calender the surface of the PET plated with metallic copper to prepare a PET film with a thickness of about 11 μm;

[0119] (3) Repeating step (1) in sequence, increasing the sputtering time to 20 min, and the thickness of the metal copper foil is 2 μm; then repeating steps (2), (1) and (2) in sequence to obtain a first composite structure, wherein the first composite structure comprises a stacked arrangement of a 12 μm thick PET polymer film A, a 1 μm thick metal copper foil, a 11 μm thick PET polymer film B, a 2 μm thick metal copper foil, a 11 μm thick PET polymer film C, a 1 μm thick metal copper foil, and a 12 μm thick PET polymer film D, wherein the stability of the PET polymer film B to lithium is greater than that of the PET polymer film A to lithium, and the stability of the PET polymer film C to lithium is greater than that of the PET polymer film D to lithium;

[0120] (4) a layer of transparent adhesive protective film is respectively attached to the outer surfaces of the PET polymer film A and the PET polymer film D in the first composite structure, and then a plurality of through holes arranged in an array are formed on the first composite structure by ultrafast laser, wherein the through holes penetrate two opposite surfaces of the composite structure in the stacking direction, and the aperture of the through holes is 10 μm, thereby obtaining a porous composite layer;

[0121] (5) The porous composite layer was transferred to the thermal evaporator and the vacuum pump was evacuated to a vacuum degree of 4×10 -1 Pa, raise the temperature to 700°C, deposit metallic copper on the inner wall surface of the through hole in the porous composite layer for 10 min. After cooling to 100°C, turn off the vacuum, take out the porous composite layer and peel off the transparent adhesive protective layer to obtain the current collector Z4 with a porosity of 60%.

[0122] Example 5

[0123] A method for preparing a current collector, comprising:

[0124] It is substantially the same as Example 1, except that the diameter of the through hole is 15 μm, and a current collector Z5 is obtained with a porosity of 75%.

[0125] Example 6

[0126] A method for preparing a current collector, comprising:

[0127] It is substantially the same as Example 1, except that the transparent adhesive protective layer is directly removed after step (4) and step (5) is not performed, to obtain a current collector Z6, the pore size of the through hole is 10 μm, and the porosity of the current collector Z5 is 75%.

[0128] Example 7

[0129] A method for preparing a current collector, comprising:

[0130] It is substantially the same as Example 1, except that a plurality of through holes are arranged in a disordered manner to obtain a current collector Z7.

[0131] Example 8

[0132] A method for preparing a current collector, comprising:

[0133] The method is substantially the same as Example 1, except that the porosity and pore size are 50% and 10 μm, respectively, to obtain current collector Z8.

[0134] Example 9

[0135] A method for preparing a current collector comprises: (1) installing a PET polymer film (thickness 6 μm) substrate roll film in a vacuum magnetron sputtering coating machine, and using a vacuum pump to evacuate the chamber to a vacuum degree of 8×10 -2 Pa, and then a certain amount of argon is introduced to adjust the vacuum degree to 2×10 -1 Pa, the polymer film is cleaned by ion source on the surface for 5 minutes. After the cleaning is completed, the ion source power is turned off; then the copper plating power is started to perform the magnetron sputtering copper plating process. At the same time of copper plating, the silver plating power is turned on. The sputtering copper foil time is 5 minutes, and the thickness of the metal copper foil is 0.5μm;

[0136] (2) using a melt extrusion calender (melting temperature set at 300° C.) to calender the surface of the PET plated with copper to prepare a PET film with a thickness of about 6 μm;

[0137] (3) Repeat step (1) in sequence, change the silver target to a magnesium target, turn on the power supply for magnesium plating while plating copper, increase the sputtering time to 8 min, and the thickness of the metal copper-silver composite foil is 1 μm;

[0138] (4) Steps (2) and (3) are then repeated in sequence, but only copper plating is performed at this time, and the sputtering is performed for 8 minutes, and the thickness of the metal copper-magnesium composite foil is 1 μm;

[0139] (5) Steps (2), (3), (2), (1) and (2) are repeated in sequence to obtain a first composite structure, wherein the first composite structure comprises a stacked 6 μm thick PET polymer film A, a 0.5 μm thick metal copper foil, a 6 μm thick PET polymer film A, a 1 μm thick metal copper-magnesium composite foil, a 6 μm thick PET polymer film A, a 1 μm thick metal copper-silver composite foil, a 6 μm thick PET polymer film A, a 1 μm thick metal copper-magnesium composite foil, a 6 μm thick PET polymer film A, a 0.5 μm thick metal copper foil, a 6 μm thick PET polymer film A, and the affinity for lithium is: metal copper-silver composite foil>metal copper-magnesium composite foil>metal copper foil;

[0140] (6) a layer of transparent adhesive protective film is attached to both sides of the first composite structure, and then a plurality of through holes arranged in an array are formed on the first composite structure by ultrafast laser, wherein the through holes penetrate two opposite surfaces of the composite structure in the stacking direction, and the aperture of the through holes is 10 μm, thereby obtaining a porous composite layer;

[0141] (7) The porous composite layer was transferred to a thermal evaporator and the vacuum pump was used to evacuate the chamber until the vacuum degree reached 4×10 -1 Pa, raise the temperature to 700°C, deposit metallic copper on the inner wall surface of the through hole in the porous composite layer for 10 min, cool to 100°C, turn off the vacuum, take out the porous composite layer and peel off the transparent adhesive protective layer to obtain the current collector Z9 with a porosity of 75%.

[0142] Example 10

[0143] A method for preparing a current collector, comprising:

[0144] The method is substantially the same as Example 1, except that a porous polypropylene wax flame retardant layer is provided on the outer surface of the PET polymer film A and the PET polymer film D to obtain a current collector Z10.

[0145] Embodiment 11

[0146] A method for preparing a current collector, comprising:

[0147] The method is substantially the same as Example 1, except that the porosity and pore size are 80% and 10 μm, respectively, to obtain a current collector Z11.

[0148] Comparative Example 1

[0149] A method for preparing a current collector, comprising:

[0150] (1) A PET polymer film (thickness 18 μm) substrate roll was installed in a vacuum magnetron sputtering coating machine, and a vacuum pump was used to evacuate the chamber to a vacuum degree of 8 × 10 -2 Pa, and then a certain amount of argon is introduced to adjust the vacuum degree to 2×10 - 1 Pa, the polymer film is cleaned by ion source on the surface for 5 minutes. After the cleaning is completed, the ion source power is turned off; then the copper plating power is started to perform magnetron sputtering copper plating process. The sputtering copper foil time is 30 minutes, and the thickness of the copper foil is 4μm;

[0151] (2) using a melt extrusion calender (melting temperature set at 300° C.) to calender the surface of the PET plated with copper to prepare a PET film with a thickness of about 18 μm;

[0152] (3) a layer of transparent adhesive protective film is attached to both sides of the composite film obtained in step (2), and then a plurality of through holes arranged in an array are formed on the composite layer using an ultrafast laser, wherein the through holes penetrate two opposite surfaces of the composite structure in the stacking direction, and the porosity and pore size are 75% and 10 μm respectively, thus forming a porous composite layer;

[0153] (4) The porous composite layer was transferred to the thermal evaporator and the vacuum degree of the chamber was 4×10 -1 Pa, raise the temperature to 700°C, deposit metal copper on the inner wall surface of the through hole for 10 min, cool to 100°C, turn off the vacuum, take out the porous composite layer and peel off the transparent adhesive protective layer to obtain the current collector DZ1.

[0154] Comparative Example 2

[0155] A method for preparing a current collector, comprising:

[0156] It is roughly the same as Example 1, except that the order of thermal evaporation and stripping of the protective film in steps (4) and (5) is changed. The surface protective film is first stripped off and then the same thermal evaporation is performed to obtain a current collector DZ2.

[0157] Comparative Example 3

[0158] A method for preparing a current collector, comprising:

[0159] It is roughly the same as Example 1, except that the processing time of each laser hole making in step (4) is changed and the time is shortened by half, so that a non-through hole array porous structure with a pore size of 10 μm can be obtained. Due to the non-through holes, the porosity is 60%, and the resulting current collector is DZ3.

[0160] Comparative Example 4

[0161] A method for preparing a current collector, comprising:

[0162] It is roughly the same as Comparative Example 1, except that the multiple through holes are arranged in a disordered manner, and the resulting current collector is DZ4.

[0163] In order to illustrate the electrochemical performance of the current collector provided in the embodiment of the present application, the following test steps are now performed:

[0164] (1) Preparation and electrochemical cycle testing of full batteries:

[0165] ①Use a vacuum mixer to mix the positive electrode active material (LiFePO 4) 49g, conductive agent (acetylene black) 0.5g and binder (polyvinylidene fluoride, PVDF) 0.5g were mixed in NMP to form a stable uniform slurry, wherein the stirring speed was 1000rpm and the time was 12h; then the obtained slurry was coated on the current collector aluminum sheet, and the surface density was controlled to be 220g / m 2 , and then dried at 80℃, and then cut into 61×72mm positive electrode sheets; then dried at 80℃, and rolled by a roller press to obtain positive electrode sheets, one of which was cut into 13mm diameter sheets to assemble button batteries for capacity calibration, and the calibrated capacity was 6mAh / cm 2 .

[0166] ② The current collector Z or DZ obtained in the above examples and comparative examples is directly used as the negative electrode, and is stacked layer by layer with the separator and the positive electrode sheet to assemble into a battery, and 0.4g of electrolyte is added dropwise, and the electrolyte is 1wt% LiNO 3 Dissolved in 4M LiFSI in ethylene glycol dimethyl ether (DME), and then packaged to obtain batteries S1-S11 and DS1-DS3 respectively.

[0167] Take 5 batteries S1-S11 and DS1-DS3 respectively, and test the battery charge and discharge cycle at 0.2C at 25℃ on the secondary battery performance test device. The steps are as follows: leave for 10 minutes; charge at 0.2C constant current to 3.8V, charge at constant voltage to 3.8V / 0.05C; leave for 10 minutes; discharge at 0.5C to 2.7V, which is 1 cycle. Repeat this step. When the battery capacity is lower than 80% of the initial discharge capacity during the cycle, the cycle is terminated. The number of cycles is the cycle life of the battery. The average value is taken for each group. The data of this parameter and the average initial discharge capacity of the battery, as well as the thickness change rate before and after the battery cycle are shown in Table 1.

[0168] Table 1 Data of average initial discharge capacity of the battery and thickness change rate before and after battery cycling

[0169]

[0170] (2) Strength and electronic conductivity test: Take the negative electrode sheets Z1~Z11 and DZ1~DZ3 with a size of 10 cm*10 cm and use an electronic universal testing machine to perform resistance tests at different tensile strengths (conventional multimeter). The experimental results are shown in Table 2.

[0171] Table 2 Resistance test table of negative electrode sheets at different tensile strengths

[0172]

[0173]

[0174] (3) Lithium metal deposition experiment: Two batteries S1-S11 and 2 batteries DS1-DS3 were used for the first lithium deposition. 2 The battery was charged to 3.8 V at a current density of , and the lithium deposition position was observed. The experimental results are shown in Table 3.

[0175] Table 3 Lithium deposition location table

[0176]

[0177]

[0178] (4) Rate performance and impedance test:

[0179] ① Take 2 batteries S1-S11 and 2 batteries DS1-DS3, and perform rate cycle test and impedance test. The rate test steps are as follows: leave for 5 minutes; charge at 0.5C constant current to 3.8V, and charge at 3.8V / 0.05C constant voltage until cut off; leave for 10 minutes; discharge at 0.5C to 2.7V, which is 1 cycle. Repeat this step 10 times. After the 10th discharge to 2.7V and stand for 2 hours, perform impedance test (amplitude 5mV, frequency 1000~0.01Hz).

[0180] ②Take 2 more batteries and repeat the above experiment ①, changing the charge and discharge rate from 0.5C to 1C.

[0181] ③Take 2 more batteries and repeat the above experiment ①, changing the charge and discharge rate from 0.5C to 1.5C.

[0182] ④Take 2 more batteries and repeat the above experiment ①, changing the charge and discharge rate from 0.5C to 2C.

[0183] ⑤Take another 2 batteries and repeat the above experiment ①, changing the charge and discharge rate from 0.5C to 3C.

[0184] ⑥Take 2 more batteries and repeat the above experiment ①, changing the charge and discharge rate from 0.5C to 5C.

[0185] The relevant experimental results are shown in Table 4.

[0186] Table 4 Rate performance and impedance test table

[0187]

[0188]

[0189] It can be understood that from the above table data, it can be concluded that both the embodiment and the comparative example have a higher capacity at the beginning of the battery, but the cycle life of the 80% capacity retention rate in the embodiment is longer, and the thickness change of the battery prepared by the embodiment is the smallest; the conductivity test under different tensile strengths shows that the embodiment can maintain good conductivity at higher tensile strengths, indicating that the current collector provided by the embodiment can withstand higher expansion stress in practical applications and ensure good electronic conductivity; the multi-layer metal foil structure design in the current collector provided by the present application ensures a good and uniform electronic conductivity network in the hole in the longitudinal direction of the stack, and compared with the comparative example, the embodiment shows better rate performance and low impedance. In summary, the battery provided by the embodiment of the present application includes the current collector provided by the present application, so that the battery has a high energy density, a high charge and discharge capacity, is not easy to produce lithium dendrites, has a high safety performance, and a long cycle life.

[0190] This article uses specific examples to illustrate the principles and implementation methods of the present application. The description of the above implementation methods is only used to help understand the core idea of ​​the present application. At the same time, for general technical personnel in this field, according to the idea of ​​the present application, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.

Claims

1. A current collector, characterized in that: The current collector comprises a stacking structure, wherein the stacking structure comprises M metal foil layers and M+1 polymer layers, and the metal foil layers and the polymer layers are alternately stacked, where M is a positive integer greater than 1. When M≥2, the lithium affinity of the polymer layer gradually decreases from the M+1th layer in the stacking structure to both ends in the stacking direction. and / or When M≥3, the lithium affinity of the metal foil layer gradually decreases from the M+1th layer in the stacking structure to both ends in the stacking direction. The current collector has a plurality of through holes penetrating two opposite surfaces of the current collector in a stacking direction.

2. The current collector according to claim 1, characterized in that The plurality of through holes are distributed in an array, and the aperture of the through holes is less than or equal to 10 μm.

3. The current collector according to claim 1, characterized in that The current collector further includes a conductive layer, and the conductive layer is disposed on the inner sidewall of the through hole.

4. The current collector according to claim 1, characterized in that: The material of the metal foil layer includes at least one of copper, gold, silver, magnesium, zinc, titanium and nickel, or stainless steel; the material of the polymer layer includes at least one of polyethylene terephthalate, polyether polymer, polycarbonate polymer, polyolefin polymer and polyimide polymer.

5. The current collector according to claim 1, characterized in that: The thickness of the metal foil layer is less than or equal to 2 μm, and the thickness of the polymer layer is 6 μm-12 μm.

6. The current collector according to claim 1, characterized in that The thicknesses of the plurality of metal foil layers are equal, and the thicknesses of the plurality of polymer layers are equal.

7. The current collector according to claim 1, characterized in that: The current collector further includes a lithium-containing metal layer, which is disposed in the metal foil layer, and has a thickness of 10 nm to 2 μm.

8. The current collector according to claim 1, characterized in that The current collector further includes a flame retardant layer. The stacking structure has a first surface and a second surface opposite to each other in the stacking direction. The flame retardant layer is arranged on the first surface, and / or the flame retardant layer is arranged on the second surface. The thickness of the flame retardant layer is 10 nm-1 μm.

9. The current collector according to claim 1, characterized in that: The polymer layer contains a lithium supplement material, which includes at least one of Li-Mg, Li-Al, Li-Si, Li-Ag, Li-Au, Li-Sn, Li-In and Li-Ge alloys. The mass proportion of the lithium supplement material in the polymer layer is 0.1wt%-5wt%.

10. A method for preparing a current collector, characterized in that: include: M layers of metal foil films and M+1 layers of polymer films are alternately stacked in sequence to form a first composite structure, where M is a positive integer greater than 1, and when M≥2, the lithium affinity of the polymer film gradually decreases from the M+1th layer in the first composite structure to both ends in the stacking direction, and / or when M≥3, the lithium affinity of the metal foil film gradually decreases from the M+1th layer in the first composite structure to both ends in the stacking direction; Disposing a first protective film and a second protective film respectively on the outermost two sides of the first composite structure in a stacking direction to form a second composite structure; forming a plurality of through holes on the second composite structure, wherein the through holes penetrate two opposite surfaces of the second composite structure in the stacking direction; The first protective film and the second protective film are removed to obtain a current collector.

11. A negative electrode, characterized in that: The negative electrode comprises a current collector prepared by the preparation method described in any one of claims 1 to 9 or claim 10.

12. An electrochemical energy storage device, characterized in that: The electrochemical energy storage device comprises a positive electrode and the negative electrode according to claim 11.

13. The electrochemical energy storage device according to claim 12, characterized in that: The porosity β of the current collector, the surface capacity C of the positive electrode, the thickness d of the current collector in the stacking direction and the capacity-thickness constant k satisfy the formula: The β≥50%, the C≥5mAh / cm 2 , k = 5 × 10 -4 cm 3 / mAh.

Citation Information

Patent Citations

  • Alloyed negative electrode, preparation method thereof and lithium ion battery

    CN112103473A

  • Flexible composite lithium metal electrode, preparation thereof and lithium metal battery

    CN112490425A

  • Anode for rechargeable lithium secondary battery, method of preparing thereof, and rechargeable lithium secondary battery comprising the same

    KR100866863B1