Silicon wafer texturing and cleaning method, solar cell and preparation method thereof

By using a combination of specific cleaning additives and ammonia in the silicon wafer texturing cleaning process, the problems of high chemical consumption and foam accumulation are solved, production costs are reduced, and the yield of the cells is improved.

CN115483299BActive Publication Date: 2024-10-11TONGWEI SOLAR ENERGY (CHENGDU) CO LID
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211281281.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-19
Publication Date
2024-10-11
Estimated Expiration
2042-10-19

AI Technical Summary

Technical Problem

The high chemical consumption during the texturing and cleaning process of HJT batteries results in high production costs and low cell yields. Moreover, foam and bubbles tend to accumulate on the surface of the cleaning bath, affecting the cleaning effect of the cells.

Method used

Use a specific type and content of cleaning additives in the post-cleaning fluid, combined with an appropriate amount of ammonia and hydrogen peroxide, to control the concentration and circulation flow of the post-cleaning fluid, reduce the dosage of alkali and hydrogen peroxide, reduce foam generation, and improve the cleaning effect.

Benefits of technology

It effectively reduces the production cost of silicon wafer texturing and cleaning, reduces the liquid contamination of cells and the defective rate, and improves the yield rate of solar cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115483299B_ABST
    Figure CN115483299B_ABST
Patent Text Reader

Abstract

The present invention provides a silicon wafer texturing and cleaning method, a solar cell and a preparation method thereof. The silicon wafer texturing and cleaning method comprises the following steps: texturing the silicon wafer; placing the silicon wafer after the texturing treatment in a post-cleaning liquid for post-cleaning treatment; wherein the post-cleaning liquid comprises, by weight, 5 to 8 parts of ammonia water with a mass concentration of 30% to 40%, 10 to 15 parts of hydrogen peroxide with a mass concentration of 30% to 35%, 1 to 2 parts of a cleaning additive and 160 to 200 parts of water; the cleaning additive comprises, by weight percentage, 1.5% to 1.98% of a chelating agent, 0.5% to 0.56% of a non-aqueous solvent, 2.4% to 2.54% of a surfactant, 1.60% to 1.69% of a wetting agent and 93% to 94% of water. The silicon wafer texturing and cleaning method can reduce the consumption of medicines in the silicon wafer texturing and cleaning process, reduce production costs and improve the yield rate of solar cells.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of solar cells, and in particular to a silicon wafer texturing and cleaning method, a solar cell and a preparation method thereof. Background Art

[0002] HJT (Heterojunction with Intrinsic Thin Layer) cells have many natural advantages due to their unique double-sided symmetrical structure and excellent passivation effect of amorphous silicon layer, such as high conversion efficiency, high bifaciality, almost no light-induced degradation, good temperature characteristics, the use of thin silicon wafers, and the stacking of perovskites. In addition, the manufacturing process of HJT cells is relatively short, and the cell process only takes about 2.5 hours.

[0003] The unique process of HJT battery lies in the deposition of amorphous silicon thin film and TCO (transparent conductive film). Due to its special structure, HJT battery has the natural advantages of high efficiency and high power generation. Compared with the current mainstream PERC (Passivated Emitter and Rear Cell) technology, the biggest problem of HJT battery is its high cost.

[0004] HJT batteries require high investment in raw and auxiliary materials and equipment, which has become the main factor restricting its rapid development. The continuous improvement of product yield and production efficiency is an important prerequisite for its large-scale mass production; however, the existing texturing and cleaning machine process has an abnormally high unit chemical consumption, which seriously affects product cost control and capacity ramp-up. In addition, during the texturing and cleaning process of silicon wafers, a large amount of foam and bubbles are easily accumulated on the surface of the cleaning tank liquid, resulting in a large number of liquid contamination on silicon wafers after texturing and cleaning, which affects the battery yield. Summary of the invention

[0005] Based on this, it is necessary to provide a silicon wafer texturing and cleaning method, a solar cell and a preparation method thereof, which can reduce the chemical consumption in the silicon wafer texturing and cleaning process, reduce production costs and improve the cell yield.

[0006] According to a first aspect of the present invention, a method for cleaning a silicon wafer is provided, comprising the following steps:

[0007] Texturing the silicon wafer; and

[0008] Placing the silicon wafer after the texturing treatment in a post-cleaning solution for post-cleaning treatment;

[0009] The post-cleaning solution comprises, by weight: 5 to 8 parts of ammonia water with a mass concentration of 30% to 40%, 10 to 15 parts of hydrogen peroxide with a mass concentration of 30% to 35%, 1 to 2 parts of a cleaning additive and 160 to 200 parts of water;

[0010] The cleaning additive comprises, by weight percentage, 1.5% to 1.98% of a chelating agent, 0.5% to 0.56% of a non-aqueous solvent, 2.4% to 2.54% of a surfactant, 1.60% to 1.69% of a wetting agent, and 93% to 94% of water.

[0011] In some embodiments, the cleaning additive further includes a preservative, and the preservative accounts for 0.5% to 0.63% of the cleaning additive by weight.

[0012] In some embodiments, the post-cleaning treatment is performed at a temperature of 40° C. to 50° C. and for a time of 200 s to 300 s.

[0013] In some embodiments, during the post-cleaning process, after cleaning every 320 to 400 silicon wafers, 300 mL to 500 mL of ammonia water with a mass concentration of 30% to 40%, 100 mL to 150 mL of hydrogen peroxide with a mass concentration of 30% to 35%, 20 mL to 40 mL of a cleaning additive, and 0.5 L to 1 L of water are added, and then 1000 mL to 1200 mL of the post-cleaning liquid is discharged; the volume of the tank for the post-cleaning treatment is 230 L to 240 L.

[0014] In some of the embodiments, the post-cleaning liquid is circulated during the post-cleaning treatment process, and the circulation flow rate of the post-cleaning liquid is 25 L / min to 30 L / min.

[0015] In some embodiments, before the texturing process, the preparation method further comprises the following steps:

[0016] The silicon wafer is pre-cleaned with a pre-cleaning liquid; the pre-cleaning liquid includes, by weight, 1 to 2 parts of sodium hydroxide or potassium hydroxide with a mass concentration of 40% to 46%, 10 to 15 parts of hydrogen peroxide with a mass concentration of 30% to 35%, 2 to 3 parts of the cleaning additive, and 160 to 200 parts of water.

[0017] In some embodiments, the pre-cleaning treatment is performed at a temperature of 50° C. to 60° C. for 200 s to 250 s.

[0018] In some of the embodiments, during the pre-cleaning process, after cleaning every 320 to 400 silicon wafers, 100 mL to 200 mL of sodium hydroxide or potassium hydroxide, 120 mL to 170 mL of hydrogen peroxide, 30 mL to 50 mL of cleaning additives, and 0.8 L to 1.2 L of water are added, and then 1000 mL to 1300 mL of the pre-cleaning liquid is discharged; the volume of the tank for the post-cleaning treatment is 230 L to 240 L, and the circulation flow rate is 25 L / min to 30 L / min.

[0019] In some embodiments, before the pre-cleaning process, the preparation method further comprises the following steps:

[0020] Performing rough polishing on the silicon wafer using an alkaline solution; and

[0021] The silicon wafer after the damage removal treatment is subjected to ozone cleaning treatment using a solution containing HF, HCl and O3.

[0022] In some embodiments, after the post-cleaning treatment, the preparation method further comprises the following steps:

[0023] Using a solution containing HF, HCl and O3 to perform rounding treatment on the silicon wafer after post-cleaning treatment;

[0024] Passivating the silicon wafer after the rounding treatment by using a solution containing HF; and

[0025] The silicon wafer after the passivation treatment is sequentially washed, dehydrated and dried.

[0026] According to a second aspect of the present invention, there is provided a method for preparing a solar cell, comprising the following steps:

[0027] The silicon wafer is textured and cleaned by the silicon wafer texturing and cleaning method according to the first aspect of the present invention; and the silicon wafer after the textured and cleaned is made into a solar cell.

[0028] In some embodiments, the process of making a solar cell from the silicon wafer after texturing and cleaning comprises the following steps:

[0029] The silicon wafer after texturing and cleaning is sequentially subjected to the steps of depositing an amorphous silicon film, depositing a transparent conductive film and preparing electrodes to obtain the solar cell.

[0030] According to a third aspect of the present invention, a solar cell is provided. The solar cell is manufactured using the method for manufacturing a solar cell according to the second aspect of the present invention.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] By adding specific types and amounts of cleaning additives to the post-cleaning liquid used in the post-cleaning treatment step, the amount of alkali, hydrogen peroxide and other chemicals used in the post-cleaning process can be effectively reduced, thereby reducing the production cost of silicon wafer texturing and cleaning, while having a good cleaning effect on silicon wafers and reducing liquid contamination of solar cells; and, by using a specific amount of ammonia water as the alkali in the post-cleaning liquid, while ensuring a good cleaning effect of the post-cleaning treatment, the generation of foam on the surface of the post-cleaning liquid is effectively reduced, thereby improving the yield of solar cells.

[0033] In addition, by adding specific types and amounts of cleaning additives to the pre-cleaning liquid used in the pre-cleaning treatment, the amount of alkali, hydrogen peroxide and other chemicals used in the pre-cleaning process can be effectively reduced, while ensuring a good cleaning effect on the silicon wafer, further reducing the production cost of silicon wafer texturing and cleaning. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 The present invention is a flowchart of a method for cleaning silicon wafer texturing according to an embodiment of the present invention. DETAILED DESCRIPTION

[0035] In order to make the above-mentioned purpose, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.

[0036] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.

[0037] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0038] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0039] In the process of preparing heterojunction solar cells, the silicon wafer needs to be textured, and a pre-cleaning treatment and a post-cleaning treatment are required before and after the texture treatment. At present, the main bath components of the pre-cleaning tank and the post-cleaning tank are sodium hydroxide, hydrogen peroxide, and deionized water; their main function is to use a low-concentration alkaline solution with a relatively strong oxidizing hydrogen peroxide to oxidize the organic matter on the surface of the silicon wafer without corroding the silicon wafer, and use sodium hydroxide to dissolve the oxidation product. This oxidation-dissolution, re-oxidation-re-dissolution method is used to remove organic film, particulate matter and metal impurities on the surface of the silicon wafer.

[0040] However, due to the volatility of hydrogen peroxide, especially when the liquid temperature is high, the amount of hydrogen peroxide volatilized is particularly large. In order to ensure a good cleaning effect, the only way is to increase the amount of hydrogen peroxide added and the number of additions to compensate for the loss of hydrogen peroxide volatilization. Moreover, even when the amount of hydrogen peroxide added is increased, the liquid often becomes ineffective and loses its cleaning ability due to the rapid volatilization of hydrogen peroxide, and the battery cells are often dirty and defective. Increasing the amount of hydrogen peroxide added will also greatly increase production costs.

[0041] In addition, during the pre-cleaning and post-cleaning processes of silicon wafers, a large amount of foam and bubbles are easily accumulated on the surface of the cleaning tank liquid, which causes the silicon wafers to be easily contaminated with liquid after texturing and cleaning, affecting the yield of solar cells.

[0042] To solve the above problems, see Figure 1 An embodiment of the present invention provides a silicon wafer texturing and cleaning method, the silicon wafer texturing and cleaning method comprises the following steps S1 to S10:

[0043] Step S1: performing rough polishing on the silicon wafer.

[0044] In some of the embodiments, the silicon wafer is roughly polished with an alkaline solution to remove a damaged layer on the surface of the silicon wafer caused by a mechanical processing process.

[0045] It is understood that the type of alkaline solution used can be an alkaline solution commonly used in the art for removing damaged layers (such as sodium hydroxide solution). The present invention does not limit the concentration of the alkaline solution used, and it can be selected according to actual production conditions.

[0046] Step S2: using a solution containing HF, HCl and O3 to perform ozone cleaning on the silicon wafer after the damage removal treatment.

[0047] By using a solution containing HF, HCl and O3 to perform ozone cleaning on the silicon wafer after the damage removal treatment, organic matter and metal impurities on the surface of the silicon wafer can be effectively cleaned. The present invention does not specifically limit the content of each component such as HF, HCl, O3 in the above-mentioned solution containing HF, HCl and O3, and can be adjusted according to actual production conditions.

[0048] Step S3: pre-cleaning the silicon wafer using a pre-cleaning solution.

[0049] In some embodiments, the pre-cleaning solution used includes, by weight, 1 to 2 parts of sodium hydroxide or potassium hydroxide with a mass concentration of 40% to 46%, 10 to 15 parts of hydrogen peroxide with a mass concentration of 30% to 35%, 2 to 3 parts of the cleaning additive, and 160 to 200 parts of water. The cleaning additive includes, by weight percentage, 1.5% to 1.98% of a chelating agent, 0.5% to 0.56% of a non-aqueous solvent, 2.4% to 2.54% of a surfactant, 1.60% to 1.69% of a wetting agent, and 93% to 94% of water.

[0050] The present invention adds a certain amount of the above-mentioned cleaning additive into the pre-cleaning liquid. The cleaning additive can fully activate the hydrogen peroxide, improve the cleaning ability of the pre-cleaning liquid, greatly improve the utilization efficiency of the pre-cleaning liquid, and greatly reduce the liquid contamination and efficiency loss of the battery cell; it can reduce the consumption of alkali and hydrogen peroxide in the pre-cleaning process, thereby reducing production costs.

[0051] Among the above-mentioned cleaning additives, the chelating agent mainly plays the role of chelating metal ions, so that there is no metal ion residue on the surface of the silicon wafer; the non-aqueous solvent mainly plays the role of dissolving residual organic matter on the silicon wafer, promoting the separation and cleaning of organic matter; the surfactant mainly plays the role of increasing the affinity between the silicon wafer and the pre-cleaning solution and activating hydrogen peroxide; the wetting agent mainly plays the role of wetting the surface of the silicon wafer, destroying the diaphragm on the surface of the silicon wafer, and reducing the interfacial energy. This cleaning additive can effectively improve the activity of hydrogen peroxide, effectively remove metal ions and residual liquid on the surface of the silicon wafer, and dissolve organic matter, etc., making the silicon wafer cleaner and greatly improving the yield of the battery cell.

[0052] In some specific examples, the chelating agent is sodium tripolysulfate, the non-aqueous solvent is acetonitrile, the surfactant is polyethylene glycol, and the wetting agent is methyl glycol. It is understood that the chelating agent, non-aqueous solvent, surfactant and wetting agent in the cleaning additive of the present invention are not limited to the specific types mentioned above.

[0053] In some embodiments, the cleaning additive may also include a preservative, which mainly serves to make the cleaning additive easier to preserve and prevent the cleaning additive from becoming ineffective. In a specific example, the preservative is sodium benzoate.

[0054] In some embodiments, the pre-cleaning treatment is performed at a temperature of 50° C. to 60° C. and for a time of 200 s to 250 s. Under the above-mentioned pre-cleaning temperature and time conditions, the cleaning effect of the pre-cleaning can be further improved.

[0055] In some of the embodiments, during the pre-cleaning process, after cleaning every 320 to 400 silicon wafers, 100 mL to 200 mL of sodium hydroxide or potassium hydroxide, 120 mL to 170 mL of hydrogen peroxide, 30 mL to 50 mL of cleaning additives, and 0.8 L to 1.2 L of water are added, and then 1000 mL to 1300 mL of the pre-cleaning liquid is discharged; the volume of the tank for the post-cleaning treatment is 230 L to 240 L, and the circulation flow rate is 25 L / min to 30 L / min.

[0056] The above-mentioned fixed replenishment and fixed discharge method can further improve the pre-cleaning effect.

[0057] Step S4: performing texturing treatment on the silicon wafer.

[0058] In some of the embodiments, an alkaline solution containing a texturing additive is used to texturing the pre-cleaned silicon wafer to form a pyramid-shaped textured light-trapping structure on the surface of the silicon wafer, thereby improving the light utilization rate of the solar cell.

[0059] It should be noted that the present invention does not specifically limit the type and amount of texturing additives and alkali in the texturing solution used in the texturing treatment. The texturing additives and alkali commonly used in the field can be used, and their amounts can also be determined according to actual production conditions.

[0060] Step S5: placing the silicon wafer after the texturing treatment in a post-cleaning solution for post-cleaning treatment.

[0061] In some of the embodiments, the post-cleaning liquid used includes, by weight, 5 to 8 parts of ammonia water with a mass concentration of 30% to 40%, 10 to 15 parts of hydrogen peroxide with a mass concentration of 30% to 35%, 1 to 2 parts of a cleaning additive and 160 to 200 parts of water; wherein the cleaning additive includes, by weight percentage, 1.5% to 1.98% of a chelating agent, 0.5% to 0.56% of a non-aqueous solvent, 2.4% to 2.54% of a surfactant, 1.60% to 1.69% of a wetting agent and 93% to 94% of water.

[0062] By performing post-cleaning treatment on the silicon wafer after texturing in the above-mentioned post-cleaning liquid, the residual liquid and metal impurities on the surface of the silicon wafer after texturing can be effectively removed. The present invention adds a certain amount of cleaning additives to the post-cleaning liquid, and the cleaning additives can fully activate hydrogen peroxide, improve the cleaning ability of the post-cleaning liquid, so that the utilization efficiency of the post-cleaning liquid is greatly improved, and the liquid contamination and efficiency loss of the battery cell are greatly reduced; at the same time, the consumption of alkali and hydrogen peroxide in the post-cleaning process can be reduced, thereby reducing production costs.

[0063] It is understood that the components in the cleaning additive may be the same as the cleaning additive used in the pre-cleaning solution.

[0064] In addition, the alkali used in the post-cleaning solution used in the traditional post-cleaning treatment is a strong alkali such as sodium hydroxide. Hydrogen peroxide will decompose in a strong alkaline solution to produce a large number of OH (hydroxyl radicals) and other free radicals with strong oxidizing ability, causing a large number of foams and bubbles to form in the post-cleaning solution. These foams and bubbles will accumulate on the surface of the cleaning tank liquid, resulting in a large amount of liquid dirt on the silicon wafer after post-cleaning, which in turn has a significant impact on the yield of the battery cell.

[0065] The present invention uses ammonia water as the base in the post-cleaning liquid and limits the content of ammonia water; the addition of weak alkalinity and appropriate amount of ammonia water makes the post-cleaning liquid not only have a good cleaning effect, but also prevent excessive decomposition of hydrogen peroxide, reduce the generation of foam, thereby avoiding the situation where a large amount of liquid dirt appears on the silicon wafer, and improve the yield of the battery cell. At the same time, ammonia water is a good precipitant, which can react with a variety of metal ions to generate insoluble weak alkaline or amphoteric hydroxides; ammonium ions can react with Ag + , Cu 2+ Cr 3+ 、Zn 2+ The metal ions undergo complexation reactions, which is beneficial to the removal of metal impurities on the surface of the silicon wafer.

[0066] However, it should be noted that in order to ensure a good cleaning effect and avoid generating too much foam, the amount of ammonia added to the post-cleaning solution needs to be controlled. In the present invention, 5 to 8 parts of ammonia with a mass concentration of 30% to 40% is used in the post-cleaning solution, which can ensure a good cleaning effect and avoid generating too much foam, thereby ensuring the yield of the battery cell.

[0067] When the amount of ammonia water is too small, the concentration of hydroxyl radicals produced by decomposition in the post-cleaning liquid is low, the cleaning ability of the post-cleaning liquid is reduced, and the expected cleaning effect cannot be achieved; when the amount of ammonia water is too large, it will cause excessive decomposition of hydrogen peroxide, produce more serious foaming, lead to a decrease in the yield of the battery cell, and also increase the consumption of hydrogen peroxide, thereby increasing production costs.

[0068] In some embodiments, the post-cleaning treatment is performed at a temperature of 40° C. to 50° C. and for a time of 200 s to 300 s. Under such treatment temperature and time conditions, a better cleaning effect can be obtained.

[0069] In some embodiments, during the post-cleaning process, after cleaning every 320 to 400 silicon wafers, 300 mL to 500 mL of ammonia water with a mass concentration of 30% to 40%, 100 mL to 150 mL of hydrogen peroxide with a mass concentration of 30% to 35%, 20 mL to 40 mL of cleaning additives, and 0.5 L to 1 L of water are added, and then 1000 mL to 1200 mL of the post-cleaning liquid is discharged; and the volume of the tank used for the post-cleaning process is 230 L to 240 L. By adopting the above-mentioned method of fixed replenishment and discharge of post-cleaning liquid, the surface cleanliness of the silicon wafer can be made higher, and the liquid contamination and efficiency loss of the battery cell can be further reduced.

[0070] In some embodiments, the post-cleaning liquid is circulated during the post-cleaning process, and the circulation flow rate of the post-cleaning liquid is controlled at 25L / min to 30L / min. The post-cleaning effect can be further improved by circulating the post-cleaning liquid at the above flow rate during the post-cleaning process.

[0071] It should be noted that, since texturing treatment is required after the pre-cleaning treatment, some foam and liquid dirt on the surface of the silicon wafer can be removed, so a strong alkaline solution such as sodium hydroxide can be used in the pre-cleaning solution; and texturing treatment will not be performed after the post-cleaning treatment. The present invention uses ammonia water, which can reduce foam in the post-cleaning process and reduce liquid dirt on the surface of the silicon wafer.

[0072] Step S6: using a solution containing HF, HCl and O3 to perform rounding treatment on the silicon wafer after the post-cleaning treatment.

[0073] After the post-cleaning treatment, the present invention uses a solution containing HF, HCl and O3 to perform rounding treatment on the silicon wafer after the post-cleaning treatment, and can polish the pyramid velvet structure on the surface of the silicon wafer after velveting to make the pyramid structure smooth.

[0074] It can be understood that the contents of HF, HCl and O3 in the solution used for rounding treatment can be specifically adjusted and determined according to actual production conditions.

[0075] Step S7: using a solution containing HF to passivate the silicon wafer after the rounding treatment.

[0076] After the rounding treatment, the present invention uses a solution containing HF to treat the silicon wafer to remove the oxide layer on the surface of the silicon wafer and passivate the surface of the silicon wafer.

[0077] Step S8: washing the silicon wafer after the passivation treatment.

[0078] After the passivation treatment, the present invention uses pure water to wash the surface of the silicon wafer to remove the chemical solution on the surface of the silicon wafer, thereby further improving the cleanliness of the surface of the silicon wafer.

[0079] Step S9: Slowly pull and dehydrate the washed silicon wafer.

[0080] The water on the surface of the silicon wafer is removed as much as possible by slow pulling and dehydration.

[0081] Step S10: drying the silicon wafer after the slow pulling and dehydration.

[0082] In some of the embodiments, nitrogen gas is purged to dry the silicon wafer to remove water droplets on the surface of the silicon wafer.

[0083] An embodiment of the present invention further provides a method for preparing a solar cell, comprising the following steps:

[0084] First, the silicon wafer is textured and cleaned by the silicon wafer texturing and cleaning method of the present invention, and then an amorphous silicon film is deposited on the front and back sides of the silicon wafer after the textured and cleaned process, and then a transparent conductive film is deposited on the amorphous silicon film on the front and back sides of the silicon wafer, and then metal electrodes are made on the transparent conductive films on the front and back sides of the silicon wafer, respectively, to prepare a solar cell.

[0085] In general, the present invention can effectively reduce the amount of alkali, hydrogen peroxide and other agents used in the pre-cleaning and post-cleaning processes by adding specific cleaning additives to the cleaning liquids of the pre-cleaning and post-cleaning processes, thereby reducing the production cost of solar cells, while having a good cleaning effect and reducing the liquid contamination of the battery cells. The present invention uses a specific amount of ammonia water as the alkali in the post-cleaning liquid, while ensuring a good cleaning effect, effectively reducing the generation of foam and improving the yield of the battery cells.

[0086] The present invention will be further described below in conjunction with specific embodiments and comparative examples, but they should not be construed as limiting the scope of protection of the present invention.

[0087] Embodiment 1:

[0088] A method for preparing a solar cell comprises the following steps:

[0089] 1) Rough polishing

[0090] The silicon wafer is roughly polished with sodium hydroxide solution to remove the damaged layer on the surface of the silicon wafer caused by the mechanical processing process.

[0091] 2) Ozone cleaning treatment

[0092] The silicon wafer after the damage removal treatment is subjected to ozone cleaning treatment using a solution containing HF, HCl and O3 to clean off organic matter and metal impurities on the surface of the silicon wafer.

[0093] 3) Pre-cleaning treatment

[0094] The silicon wafer is pre-cleaned using a pre-cleaning liquid. The pre-cleaning liquid used includes, by weight, 1 part of sodium hydroxide with a mass concentration of 40%, 10 parts of hydrogen peroxide with a mass concentration of 30%, 2 parts of cleaning additives, and 180 parts of water. Among them, the cleaning additive includes, by weight percentage, 1.5% of chelating agent sodium tripolysulfate, 0.5% of non-aqueous solvent acetonitrile, 2.4% of surfactant polyethylene glycol, 1.60% of wetting agent methyl glycol, 0.5% of preservative sodium benzoate, and 93.5% of water.

[0095] During the pre-cleaning process, 100 mL of the above-mentioned sodium hydroxide, 120 mL of the above-mentioned hydrogen peroxide, 30 mL of the cleaning additive, and 0.8 L of water were added to the pre-cleaning liquid after cleaning 320 silicon wafers, and then 1000 mL of the pre-cleaning liquid was discharged; and the tank volume used for the post-cleaning process was 240 L. The pre-cleaning treatment time for each silicon wafer was 200 s, and the pre-cleaning treatment temperature was 55°C. The circulation flow rate of the pre-cleaning liquid was 25 L / min.

[0096] 4) Velvet treatment

[0097] The pre-cleaned silicon wafer is subjected to texturing treatment by using an alkaline solution containing a texturing additive to form a pyramid-shaped textured light-trapping structure on the surface of the silicon wafer.

[0098] 5) Post-cleaning treatment

[0099] The silicon wafer after the texturing treatment is placed in a post-cleaning liquid for post-cleaning treatment. The post-cleaning liquid used includes, by weight, 5 parts of ammonia water with a mass concentration of 35%, 10 parts of hydrogen peroxide with a mass concentration of 30%, 1 part of a cleaning additive and 180 parts of water; wherein, the cleaning additive includes, by weight percentage, 1.5% of chelating agent sodium tripolysulfate, 0.5% of non-aqueous solvent acetonitrile, 2.4% of surfactant polyethylene glycol, 1.60% of wetting agent methyl glycol, 0.5% of preservative sodium benzoate and 93.5% of water.

[0100] The temperature of the post-cleaning treatment is 45°C, and the cleaning time for each silicon wafer is 200s. During the post-cleaning treatment, after cleaning 320 silicon wafers, 300mL of 35% ammonia water, 100mL of 30% hydrogen peroxide, 20mL of cleaning additives, and 0.5L of water are added to the post-cleaning liquid, and 1000mL of the post-cleaning liquid is discharged; the tank volume used for the post-cleaning treatment is 240L. The circulation flow rate of the post-cleaning liquid is 25L / min.

[0101] 6) Smooth processing

[0102] The silicon wafer after post-cleaning treatment is smoothed by using a solution containing HF, HCl and O3, so as to polish the pyramid velvet structure on the surface of the silicon wafer after velvet making, so that the pyramid structure becomes smooth.

[0103] 7) Passivation treatment

[0104] The silicon wafer is treated with a solution containing HF to remove the oxide layer on the surface of the silicon wafer and to passivate the surface of the silicon wafer.

[0105] 8) Washing

[0106] The surface of the silicon wafer is washed with pure water to remove the chemical solution on the surface of the silicon wafer and further improve the cleanliness of the silicon wafer surface.

[0107] 9) Slow pulling and dehydration

[0108] The washed silicon wafer is subjected to a slow pulling and dehydration treatment in a slow pulling and dehydration tank.

[0109] 10) Drying

[0110] The silicon wafer is dried by nitrogen purge to obtain the silicon wafer after texturing and cleaning.

[0111] 11) Deposition of amorphous silicon thin film

[0112] Amorphous silicon thin films are deposited on the front and back sides of the silicon wafer prepared above.

[0113] 12) Deposition of transparent conductive film

[0114] Transparent conductive films are deposited on the amorphous silicon films on the front and back sides of the silicon wafer respectively.

[0115] 13) Making metal electrodes

[0116] Metal electrodes are prepared on the transparent conductive films on the front and back of the silicon wafer respectively to obtain finished solar cells.

[0117] The appearance of the prepared solar cell is good, and the yield is 98.65%. The various properties of the prepared solar cell are tested by simulating sunlight irradiation and using the photoelectric principle of the IV tester to test the defects and power generation capacity of the cell under standard conditions. The test results are shown in Table 1.

[0118] Embodiment 2:

[0119] A method for preparing a solar cell comprises the following steps:

[0120] 1) Rough polishing

[0121] The silicon wafer is roughly polished with sodium hydroxide solution to remove the damaged layer on the surface of the silicon wafer caused by the mechanical processing process.

[0122] 2) Ozone cleaning treatment

[0123] The silicon wafer after the damage removal treatment is subjected to ozone cleaning treatment using a solution containing HF, HCl and O3 to clean off organic matter and metal impurities on the surface of the silicon wafer.

[0124] 3) Pre-cleaning treatment

[0125] The silicon wafer is pre-cleaned using a pre-cleaning liquid. The pre-cleaning liquid used includes, by weight, 2 parts of sodium hydroxide with a mass concentration of 40%, 12 parts of hydrogen peroxide with a mass concentration of 30%, 2.5 parts of cleaning additives, and 180 parts of water. Among them, the cleaning additives include, by weight percentage, 1.55% of chelating agent sodium tripolysulfate, 0.55% of non-aqueous solvent acetonitrile, 2.4% of surfactant polyethylene glycol, 1.65% of wetting agent methyl glycol, 0.5% of preservative sodium benzoate, and 93.35% of water.

[0126] During the pre-cleaning process, 150 mL of sodium hydroxide, 160 mL of hydrogen peroxide, 35 mL of cleaning additives, and 1 L of water were added to the pre-cleaning liquid after cleaning 320 silicon wafers, and 1100 mL of the pre-cleaning liquid was discharged; and the tank volume used for post-cleaning was 240 L. The pre-cleaning time for each silicon wafer was 220 s, and the pre-cleaning temperature was 58 ° C. The circulation flow rate of the pre-cleaning liquid was 25 L / min.

[0127] 4) Velvet treatment

[0128] The pre-cleaned silicon wafer is subjected to texturing treatment by using an alkaline solution containing a texturing additive to form a pyramid-shaped textured light-trapping structure on the surface of the silicon wafer.

[0129] 5) Post-cleaning treatment

[0130] The silicon wafer after the texturing treatment is placed in a post-cleaning liquid for post-cleaning treatment. The post-cleaning liquid used includes, by weight, 7.5 parts of ammonia water with a mass concentration of 35%, 12 parts of hydrogen peroxide with a mass concentration of 30%, 1 part of a cleaning additive and 180 parts of water; wherein, the post-cleaning liquid includes 1.55% of chelating agent sodium tripolysulfate, 0.55% of non-aqueous solvent acetonitrile, 2.4% of surfactant polyethylene glycol, 1.65% of wetting agent methyl glycol, 0.5% of preservative sodium benzoate and 93.35% of water.

[0131] The temperature of the post-cleaning treatment is 48°C, and the cleaning time for each silicon wafer is 225s. During the post-cleaning treatment, after cleaning 320 silicon wafers, 350mL of ammonia water with a mass concentration of 35%, 120mL of hydrogen peroxide with a mass concentration of 30%, 30mL of cleaning additives, 0.8L of water are added to the post-cleaning liquid, and 1150mL of the post-cleaning liquid is discharged; the tank volume used for the post-cleaning treatment is 240L. The circulation flow rate of the post-cleaning liquid is 25L / min.

[0132] 6) Smooth processing

[0133] The silicon wafer after post-cleaning treatment is smoothed by using a solution containing HF, HCl and O3, so as to polish the pyramid velvet structure on the surface of the silicon wafer after velvet making, so that the pyramid structure becomes smooth.

[0134] 7) Passivation treatment

[0135] The silicon wafer is treated with a solution containing HF to remove the oxide layer on the surface of the silicon wafer and to passivate the surface of the silicon wafer.

[0136] 8) Washing

[0137] The surface of the silicon wafer is washed with pure water to remove the chemical solution on the surface of the silicon wafer and further improve the cleanliness of the silicon wafer surface.

[0138] 9) Slow pulling and dehydration

[0139] The washed silicon wafer is subjected to a slow pulling and dehydration treatment in a slow pulling and dehydration tank.

[0140] 10) Drying

[0141] The silicon wafer is dried by nitrogen purge to obtain the silicon wafer after texturing and cleaning.

[0142] 11) Deposition of amorphous silicon thin film

[0143] Amorphous silicon thin films are deposited on the front and back sides of the silicon wafer prepared above.

[0144] 12) Deposition of transparent conductive film

[0145] Transparent conductive films are deposited on the amorphous silicon films on the front and back sides of the silicon wafer respectively.

[0146] 13) Making metal electrodes

[0147] Metal electrodes are prepared on the transparent conductive films on the front and back of the silicon wafer respectively to obtain finished solar cells.

[0148] The appearance of the prepared solar cell is good, and the yield is 98.85%. The various properties of the prepared solar cell are tested in the same way as in Example 1. The test results are shown in Table 1.

[0149] Comparative Example 1:

[0150] A method for preparing a solar cell comprises the following steps:

[0151] 1) Rough polishing

[0152] The silicon wafer is roughly polished with sodium hydroxide solution to remove the damaged layer on the surface of the silicon wafer caused by the mechanical processing process.

[0153] 2) Ozone cleaning treatment

[0154] The silicon wafer after the damage removal treatment is subjected to ozone cleaning treatment using a solution containing HF, HCl and O3 to clean off organic matter and metal impurities on the surface of the silicon wafer.

[0155] 3) Pre-cleaning treatment

[0156] The silicon wafer is pre-cleaned using a pre-cleaning liquid. The pre-cleaning liquid used includes, by weight, 5 parts of sodium hydroxide with a mass concentration of 30%, 16 parts of hydrogen peroxide with a mass concentration of 30%, 1 part of a cleaning additive, and 130 parts of water. Among them, the cleaning additive includes, by weight percentage, 1.7% of chelating agent sodium tripolysulfate, 0.6% of non-aqueous solvent acetonitrile, 1.8% of surfactant polyethylene glycol, 2.9% of wetting agent methyl glycol, 0.65% of preservative sodium benzoate, and 92.35% of water.

[0157] During the pre-cleaning process, 50 mL of the above-mentioned sodium hydroxide, 200 mL of the above-mentioned hydrogen peroxide, 50 mL of the cleaning additive, and 1 L of water were added to the pre-cleaning liquid after cleaning every 320 silicon wafers, and 1500 mL of the pre-cleaning liquid was discharged; and the tank volume used for the post-cleaning process was 240 L. The pre-cleaning treatment time for each silicon wafer was 268 s, and the pre-cleaning treatment temperature was 75°C. The circulation flow rate of the pre-cleaning liquid was 25 L / min.

[0158] 4) Velvet treatment

[0159] The pre-cleaned silicon wafer is subjected to texturing treatment by using an alkaline solution containing a texturing additive to form a pyramid-shaped textured light-trapping structure on the surface of the silicon wafer.

[0160] 5) Post-cleaning treatment

[0161] The silicon wafer after the texturing treatment is placed in a post-cleaning liquid for post-cleaning treatment. The post-cleaning liquid used includes, by weight, 10 parts of ammonia water with a mass concentration of 35%, 16 parts of hydrogen peroxide with a mass concentration of 30%, 1 part of a cleaning additive and 140 parts of water; wherein, the cleaning additive includes, by weight percentage, 1.7% of chelating agent sodium tripolysulfate, 0.6% of non-aqueous solvent acetonitrile, 1.8% of surfactant polyethylene glycol, 2.9% of wetting agent methyl glycol, 0.65% of preservative sodium benzoate and 92.35% of water.

[0162] The temperature of the post-cleaning treatment is 55°C, and the cleaning time for each silicon wafer is 260s. During the post-cleaning treatment, 350mL of 35% ammonia water, 200mL of 30% hydrogen peroxide, and 0.8L of water are added to the post-cleaning liquid after cleaning 320 silicon wafers, and 1550mL of the post-cleaning liquid is discharged; the tank volume used for the post-cleaning treatment is 240L. The circulation flow rate of the post-cleaning liquid is 10L / min.

[0163] 6) Smooth processing

[0164] The silicon wafer after post-cleaning treatment is smoothed by using a solution containing HF, HCl and O3, so as to polish the pyramid velvet structure on the surface of the silicon wafer after velvet making, so that the pyramid structure becomes smooth.

[0165] 7) Passivation treatment

[0166] The silicon wafer is treated with a solution containing HF to remove the oxide layer on the surface of the silicon wafer and to passivate the surface of the silicon wafer.

[0167] 8) Washing

[0168] The surface of the silicon wafer is washed with pure water to remove the chemical solution on the surface of the silicon wafer and further improve the cleanliness of the silicon wafer surface.

[0169] 9) Slow pulling and dehydration

[0170] The washed silicon wafer is subjected to a slow pulling and dehydration treatment in a slow pulling and dehydration tank.

[0171] 10) Drying

[0172] The silicon wafer is dried by nitrogen purge to obtain the silicon wafer after texturing and cleaning.

[0173] 11) Deposition of amorphous silicon thin film

[0174] Amorphous silicon thin films are deposited on the front and back sides of the silicon wafer prepared above.

[0175] 12) Deposition of transparent conductive film

[0176] Transparent conductive films are deposited on the amorphous silicon films on the front and back sides of the silicon wafer respectively.

[0177] 13) Making metal electrodes

[0178] Metal electrodes are prepared on the transparent conductive films on the front and back of the silicon wafer respectively to obtain finished solar cells.

[0179] The appearance of the prepared solar cell is good, and the yield is 92.63%. The various properties of the prepared solar cell are tested in the same way as in Example 1. The test results are shown in Table 1.

[0180] Table 1 Performance of solar cells prepared in various embodiments and comparative examples

[0181] Serial number Battery efficiency (%) Open circuit voltage(V) Short circuit current(A) Yield (%) Example 1 24.17 0.747 8.53 98.65 Example 2 24.19 0.746 8.52 98.85 Comparative Example 1 24.09 0.741 8.49 92.63

[0182] It can be seen from Table 1 that:

[0183] 1) By using the silicon wafer texturing and cleaning method of the present invention to texturize and clean silicon wafers (Example 1 and Example 2), the proportion of liquid-containing defects in silicon wafers on the production line is significantly reduced, and the overall yield of heterojunction solar cells is increased by more than 5%, with a significant improvement in yield.

[0184] 2) The electrical properties of solar cells made of silicon wafers treated by the silicon wafer texturing and cleaning method of the present invention are tested, and it can be seen that the cell efficiency of Example 1 and Example 2 is improved by more than 0.08% compared with that of Comparative Example 1. The reason is that the silicon wafer surface is less liquid-carrying after the treatment of the present invention, the impurities entrained are significantly reduced, the cleanliness is greatly improved, the coating deposition effect is better, and the recombination center is reduced. At the same time, the Voc of the cells of Example 1 and Example 2 of the present invention is improved by about 5mV compared with Comparative Example 1, and other electrical properties are also slightly improved.

[0185] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0186] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the attached claims, and the description and drawings can be used to interpret the content of the claims.

Claims

1. A method for cleaning silicon wafer texturing, characterized in that: The steps include: Carry out texturing treatment on silicon wafers; as well as Placing the silicon wafer after the texturing treatment in a post-cleaning solution for post-cleaning treatment; The post-cleaning solution comprises, by weight: 5 to 8 parts of ammonia water with a mass concentration of 30% to 40%, 10 to 15 parts of hydrogen peroxide with a mass concentration of 30% to 35%, 1 to 2 parts of a cleaning additive and 160 to 200 parts of water; The cleaning additive comprises, by weight percentage: 1.5% to 1.98% of a chelating agent, 0.5% to 0.56% of a non-aqueous solvent, 2.4% to 2.54% of a surfactant, 1.60% to 1.69% of a wetting agent, and 93% to 94% of water; During the post-cleaning treatment process, after cleaning every 320 to 400 silicon wafers, 300 mL to 500 mL of ammonia water with a mass concentration of 30% to 40%, 100 mL to 150 mL of hydrogen peroxide with a mass concentration of 30% to 35%, 20 mL to 40 mL of a cleaning additive, and 0.5 L to 1 L of water are added, and then 1000 mL to 1200 mL of the post-cleaning liquid is discharged; the volume of the tank for the post-cleaning treatment is 230 L to 240 L.

2. The method for cleaning silicon wafer texture according to claim 1, characterized in that: The post-cleaning treatment is performed at a temperature of 40° C. to 50° C. and for a time of 200 s to 300 s.

3. The silicon wafer texturing and cleaning method according to claim 1, characterized in that: During the post-cleaning treatment, the post-cleaning liquid is circulated, and the circulation flow rate of the post-cleaning liquid is 25L / min to 30L / min.

4. The silicon wafer texturing and cleaning method according to any one of claims 1 to 3, characterized in that: Before the texturing process, the method further comprises the following steps: The silicon wafer is pre-cleaned with a pre-cleaning liquid; the pre-cleaning liquid includes, by mass, 1 to 2 parts of sodium hydroxide or potassium hydroxide with a mass concentration of 40% to 46%, 10 to 15 parts of hydrogen peroxide with a mass concentration of 30% to 35%, 2 to 3 parts of the cleaning additive, and 160 to 200 parts of water.

5. The silicon wafer texturing and cleaning method according to claim 4, characterized in that: The pre-cleaning treatment is performed at a temperature of 50° C. to 60° C. for 200 s to 250 s.

6. The silicon wafer texturing and cleaning method according to claim 4, characterized in that: During the pre-cleaning process, after cleaning every 320 to 400 silicon wafers, 100 mL to 200 mL of sodium hydroxide or potassium hydroxide, 120 mL to 170 mL of hydrogen peroxide, 30 mL to 50 mL of cleaning additives, and 0.8 L to 1.2 L of water are added, and then 1000 mL to 1300 mL of the pre-cleaning liquid is discharged; the volume of the tank for the post-cleaning treatment is 230 L to 240 L, and the circulation flow rate is 25 L / min to 30 L / min.

7. The silicon wafer texturing and cleaning method according to claim 4, characterized in that: Before the pre-cleaning process, the following steps are also included: Performing rough polishing on the silicon wafer using an alkaline solution; and The silicon wafer after the damage removal treatment is subjected to ozone cleaning treatment using a solution containing HF, HCl and O3.

8. The method for cleaning silicon wafer texturing according to any one of claims 1 to 3, 5, 6, and 7, characterized in that: After the post-cleaning process, the following steps are also included: Using a solution containing HF, HCl and O3 to perform rounding treatment on the silicon wafer after post-cleaning treatment; Passivating the silicon wafer after the rounding treatment by using a solution containing HF; as well as The silicon wafer after the passivation treatment is sequentially washed, dehydrated and dried.

9. A method for preparing a solar cell, characterized in that: The steps include: The silicon wafer is cleaned by using the silicon wafer texturing and cleaning method according to any one of claims 1 to 8; and The silicon wafer after texturing and cleaning is made into a solar cell.

10. The method for preparing a solar cell according to claim 9, characterized in that: The steps of making the silicon wafer after texturing and cleaning into a solar cell include: The silicon wafer after texturing and cleaning is sequentially subjected to the steps of depositing an amorphous silicon film, depositing a transparent conductive film and preparing electrodes to obtain the solar cell.

11. A solar cell, characterized in that: The solar cell is prepared by the method for preparing a solar cell according to any one of claims 9 or 10.