A carbon-coated hollow multi-shell spherical lithium iron phosphate and its preparation method and application

By using a carbon-coated hollow multi-shell spherical structure design on the lithium iron phosphate material, the problem of low electronic conductivity and ion migration rate is solved, the low-temperature conductivity and electrochemical performance are significantly improved, and the scope of its application is expanded.

CN115498161BActive Publication Date: 2024-10-22SHANDONG ZHAOWEN NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211221381.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-08
Publication Date
2024-10-22
Estimated Expiration
2042-10-08

AI Technical Summary

Technical Problem

Lithium iron phosphate materials have problems such as low electronic conductivity and low ion migration rate. Especially under high-rate discharge conditions, the electrochemical polarization effect is large, which limits its application in the market.

Method used

The structural design of carbon-coated hollow multi-shell spherical lithium iron phosphate is used. Hollow multi-shell carbon microspheres are prepared by spray drying. On this basis, a hydrothermal reaction is performed to form a lithium iron phosphate-carbon microsphere shell. Finally, The carbon coating layer is formed by high-temperature baking in an inert atmosphere, which improves the structure and pore structure of the material, increases its contact area with the electrolyte, and reduces the resistance to lithium ion migration.

Benefits of technology

The low-temperature conductivity and electrochemical properties of lithium iron phosphate are improved, making it more stable under high-rate discharge conditions and expanding its application scope.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115498161B_ABST
    Figure CN115498161B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of lithium ion battery materials, and relates to a carbon-coated hollow multi-shell spherical lithium iron phosphate and a preparation method and application. It includes a multi-shell structure from the inside to the outside, a cavity structure between adjacent shell structures, a shell structure including a lithium iron phosphate-carbon microsphere shell and a carbon coating layer, a lithium iron phosphate-carbon microsphere shell attached to the inner surface of the carbon coating layer, and a lithium iron phosphate-carbon microsphere shell including a carbon microsphere shell and attached lithium iron phosphate. The preparation method is: using sucrose as a carbon source to prepare porous hollow multi-shell carbon microspheres by a spray drying method; reacting with a lithium source and a phosphate salt, sintering to obtain a hollow multi-shell lithium phosphate-carbon microsphere shell; and then mixing with an iron salt for hydrothermal reaction to obtain a hollow multi-shell spherical lithium iron phosphate-carbon microsphere shell. The problem of low conductivity and low ion migration rate of lithium iron phosphate is solved, and the problem of large electrochemical polarization effect under high-rate discharge conditions is solved, so that the application of lithium iron phosphate is more extensive.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium ion battery materials, and in particular relates to a carbon-coated hollow multi-shell spherical lithium iron phosphate and a preparation method and application thereof. Background Art

[0002] Lithium-ion power batteries mainly include lithium iron phosphate, lithium manganese oxide, and ternary materials of lithium nickel cobalt manganese oxide and lithium nickel cobalt aluminum oxide. Because lithium iron phosphate has an orthorhombic olivine structure, it hinders the diffusion movement of lithium ions to a certain extent, which leads to the problems of low electronic conductivity and low ion migration rate of lithium iron phosphate, and the electrochemical polarization effect is large under high rate discharge conditions. The existence of these problems seriously hinders the application of lithium iron phosphate in the market. Summary of the invention

[0003] In view of the problems existing in the above-mentioned prior art, the purpose of the present invention is to provide a carbon-coated hollow multi-shell spherical lithium iron phosphate and a preparation method and application thereof.

[0004] In order to solve the above technical problems, the technical solution of the present invention is:

[0005] In the first aspect, a carbon-coated hollow multi-shell spherical lithium iron phosphate includes a multi-shell structure from the inside to the outside, a cavity structure between adjacent shell structures, the shell structure includes a lithium iron phosphate-carbon microsphere shell layer and a carbon coating layer, the inner side of the innermost shell structure is a cavity structure, the lithium iron phosphate-carbon microsphere shell layer is attached to the inner surface of the carbon coating layer, and the lithium iron phosphate-carbon microsphere shell layer includes a carbon microsphere shell layer and attached lithium iron phosphate.

[0006] The spherical lithium iron phosphate in the present invention has special structural and morphological characteristics. The carbon microspheres with a hollow multi-shell structure provide a template for the special structure of the lithium iron phosphate. The carbon-coated lithium iron phosphate makes the obtained lithium iron phosphate have a hollow, multi-shell structure. The improved structure and increased specific surface area, increased interlayer distance, reduced resistance to lithium ion migration, increased contact area with the electrolyte, promoted lithium ion conduction, and thus improved its electrical conductivity; it is beneficial to improve the low-temperature performance of the lithium iron phosphate and improve the low-temperature electrical conductivity of the lithium iron phosphate.

[0007] In some embodiments of the present invention, in the lithium iron phosphate-carbon microsphere shell layer, the lithium iron phosphate carbon is attached to the outer surface, the inner surface and the pore structure of the microsphere shell layer.

[0008] In some embodiments of the present invention, the shell layer and the carbon coating layer of the lithium iron phosphate-carbon microspheres have a porous structure.

[0009] In some embodiments of the present invention, the porous structure of the shell layer of lithium iron phosphate-carbon microspheres is a mesoporous and macroporous structure.

[0010] In some embodiments of the present invention, the carbon-coated hollow multi-shell spherical lithium iron phosphate has a porous double-shell structure.

[0011] In a second aspect, a method for preparing a carbon-coated hollow multi-shell spherical lithium iron phosphate is provided, the method comprising:

[0012] 1) using sucrose as a carbon source to prepare precursor microspheres by a spray drying method, and then calcining the precursor microspheres to obtain a hollow multi-shell carbon microsphere structure after carbonization;

[0013] 2) adding the hollow multi-shell carbon microspheres, lithium source and phosphate salt into a solvent for reaction to obtain hollow multi-shell lithium phosphate-carbon microsphere shells;

[0014] 3) The hollow multi-shell lithium phosphate-carbon microsphere shell and the iron salt are mixed, and a hollow multi-shell spherical lithium iron phosphate-carbon microsphere shell is generated by a hydrothermal reaction, and then reacted in a citric acid solution and then calcined at a high temperature under an inert atmosphere to finally obtain a carbon-coated hollow multi-shell spherical lithium iron phosphate.

[0015] In some embodiments of the present invention, the method for preparing hollow multi-shell carbon microspheres from sucrose in step 1) is: preparing hollow multi-shell carbon microspheres from a sucrose solution by spray drying and calcining; and the temperature of the further spray drying is 150-200° C. The present invention uses a spray drying method to spray-dry a sucrose solution in the form of droplets to obtain precursor carbon microspheres. After being heated, the sucrose shrinks to form a hollow multi-shell structure, which is beneficial to the control of the structure and morphology of lithium iron phosphate.

[0016] In some embodiments of the present invention, the hollow multi-shell carbon microspheres in step 1) are carbonized in a tubular sintering furnace under an inert atmosphere to obtain porous hollow multi-shell carbon microspheres. Carbonization under an inert atmosphere is conducive to the formation of a porous carbon microsphere structure.

[0017] There is no particular limitation on the solvent in step 2) provided that it can dissolve the lithium source and the phosphate salt. In some embodiments of the present invention, the solvent is ethanol, ethylene glycol, etc. A single solvent may be used independently, or a mixed solvent containing two or more thereof may be used.

[0018] In some embodiments of the present invention, the lithium source in step 2) is a lithium salt such as LiOH, Li2CO3, LiCH3COO, etc. A single lithium salt or a combination of multiple lithium salts can be used.

[0019] In some embodiments of the present invention, the phosphate salt in step 2) is a phosphorus-containing solution such as NH4H2PO4, (NH4)2HPO4, etc. A single phosphate salt or a combination of multiple phosphate salts can be used.

[0020] In some embodiments of the present invention, the molar ratio of the lithium source to the phosphate salt in step 2) is 0.9-1.2:1; further 1-1.02:1.

[0021] In some embodiments of the present invention, the reaction time in the solvent in step 2) is 1-3 hours, and then the reaction is allowed to stand for precipitation. Furthermore, the standing time is 5-10 hours. The reaction is carried out in the solvent to generate lithium phosphate.

[0022] In some embodiments of the present invention, the precipitate in step 2) is sintered under air conditions. Further, the sintering temperature is 300-400°C, and the sintering time is 3-6h. As the sintering process proceeds, the substance shrinks from the surface layer inward. When the reaction reaches a certain degree, the metal salt solution forms a dense oxide, the surface layer is hard and difficult to shrink, and a layer of outer shell is formed. The unreacted substance inside continues to shrink to form a certain gap. The reaction is continued until the reaction is completed, and a hollow multi-shell lithium phosphate-carbon microsphere shell layer can be obtained. The lithium phosphate-carbon microsphere shell layer is a composite shell layer of lithium phosphate and carbon microspheres, and lithium phosphate is attached to the surface and pores of the carbon microsphere shell layer. After the reaction is completed, it is allowed to stand and cool at room temperature, vacuum filtered and separated, washed twice with deionized water and anhydrous ethanol respectively, and placed in a vacuum drying oven for 8-15h to obtain a hollow multi-shell structure of lithium phosphate-carbon microsphere shell layer.

[0023] In some embodiments of the present invention, the iron salt in step 3) is a ferrous salt, specifically Fe(NO3)2. The iron in lithium iron phosphate is divalent, so a divalent iron salt is selected.

[0024] In some embodiments of the present invention, the temperature of step 3) hydrothermal synthesis is 160-180° C. and the time is 3-12 h.

[0025] In some embodiments of the present invention, the precipitate obtained by hydrothermal synthesis in step 3) is dried under an inert atmosphere. Further, the drying temperature is 350-450°C and the drying time is 3-6 hours. Drying is performed under an inert atmosphere (Ar, N2) to prevent Fe 2+ Oxidation, finally obtaining the surface hollow multi-shell lithium iron phosphate-carbon microsphere shell.

[0026] In some embodiments of the present invention, the hollow multi-shell spherical lithium iron phosphate obtained after drying in step 3) is immersed in a citric acid solution and then calcined at a temperature of 600-900°C and a heating rate of 5°C·min -1 The heat preservation time is 3 hours, and a carbon-coated hollow multi-shell spherical lithium iron phosphate product is obtained. The carbon coating layer obtained on the outer surface is beneficial to improve the low-temperature performance of lithium iron phosphate, so that lithium iron phosphate maintains its electrochemical performance under low temperature conditions.

[0027] Thirdly, the application of the above-mentioned carbon-coated hollow multi-shell spherical lithium iron phosphate in lithium batteries.

[0028] One or more technical solutions of the present invention have the following beneficial effects:

[0029] The present invention proposes a carbon-coated hollow multi-shell spherical lithium iron phosphate with a special structure, which solves the problems of low electrical conductivity and low ion migration rate of lithium iron phosphate, and the problem of large electrochemical polarization effect under high-rate discharge conditions, making the application of lithium iron phosphate more extensive.

[0030] The method for preparing the carbon-coated hollow multi-shell spherical lithium iron phosphate of the present invention first prepares carbon microspheres with a hollow multi-shell structure, then forms a lithium iron phosphate-carbon microsphere shell layer with a hollow multi-shell structure on the basis of the carbon microspheres with a hollow multi-shell structure, and then forms a carbon coating layer. It is beneficial to obtain lithium iron phosphate with a special structure. The performance of the lithium iron phosphate material is improved. The improvement of the structure and the improvement of the pore structure are beneficial to the increase of the specific surface area of ​​the lithium iron phosphate material, the reduction of the resistance to lithium ion migration, and the increase of the contact area with the electrolyte, thereby improving the low-temperature conductivity of the lithium iron phosphate. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] The drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present application. The illustrative embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0032] Figure 1 This is a transmission electron microscope image of the carbon-coated hollow multi-shell spherical lithium iron phosphate of Example 1. DETAILED DESCRIPTION

[0033] It should be noted that the following detailed descriptions are all illustrative and intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0034] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this specification, they indicate the presence of features, steps, operations, devices, components and / or combinations thereof. The present invention is further described below in conjunction with the embodiments

[0035] Embodiment 1:

[0036] Prepare 35ml sucrose solution, prepare carbon microspheres by spray drying, the spray drying condition is 160℃, and then carbonize to obtain hollow multi-shell carbon microspheres. Disperse LiOH:(NH4)2HPO4 in a ratio of 1:1 and the prepared carbon microspheres in ethylene glycol solvent, stir magnetically for 3h under argon atmosphere, stand for 8h, centrifuge the generated precipitate, and sinter at 400℃ for 5h under the protection of argon atmosphere to obtain the hollow multi-shell lithium phosphate-carbon microsphere shell. Mix the obtained lithium phosphate and Fe(NO3)2 solution in a ratio of 1.02:1, and obtain the hollow multi-shell structure of lithium iron phosphate by hydrothermal synthesis. The conditions of hydrothermal synthesis are: temperature control at 180℃, reaction for 8h, vacuum filtration separation, and vacuum drying the obtained material at 400℃ for 5h to obtain the hollow multi-shell lithium iron phosphate-carbon microsphere shell. The obtained lithium iron phosphate sample is immersed in a citric acid solution for 36 hours, and then vacuum dried to obtain a carbon-coated hollow multi-shell lithium iron phosphate sample.

[0037] Embodiment 2:

[0038] Prepare 30ml sucrose solution, prepare carbon microspheres by spray drying, the spray drying condition is 160℃, and then carbonize to obtain hollow multi-shell carbon microspheres. Disperse LiOH: (NH4) 2HPO4 in a ratio of 1.02: 1 and the prepared hollow multi-shell carbon microspheres in ethylene glycol solvent, stir magnetically for 2h under nitrogen atmosphere, stand for 8h, centrifuge the generated precipitate, and sinter at 350℃ for 5h under the protection of nitrogen atmosphere to obtain the hollow multi-shell structure of lithium phosphate-carbon microsphere shell. Mix the obtained lithium phosphate and Fe(NO3) 2 solution in a ratio of 1: 1, and obtain the hollow multi-shell structure of lithium iron phosphate by hydrothermal synthesis. The conditions of hydrothermal synthesis are: temperature control at 180℃, reaction for 8h, vacuum filtration separation, and vacuum drying the obtained material at 400℃ for 6h to obtain the surface hollow multi-shell lithium iron phosphate-carbon microsphere shell. The obtained lithium iron phosphate sample is immersed in a citric acid solution for 48 hours, and then vacuum dried to obtain a carbon-coated hollow multi-shell lithium iron phosphate sample.

[0039] The hollow multi-shell lithium iron phosphate samples prepared in Example 1 and Example 2 were used as positive electrode materials for lithium-ion batteries and ordinary commercial lithium iron phosphate positive electrode materials (comparative example). The positive electrode materials, conductive agent Super-P, and binder PVDF were mixed and ground in a ratio of 94:3:3 to obtain a uniform positive electrode slurry. The prepared positive electrode slurry was coated on the current collector aluminum foil to obtain a positive electrode sheet. Lithium-ion button half-cells were prepared in the order of negative electrode shell, lithium sheet, diaphragm, electrolyte (non-aqueous electrolyte), positive electrode sheet, spring sheet, steel sheet, and positive electrode shell for testing. The charge and discharge capacitance of the battery at room temperature of 20°C and the electrochemical performance at a low temperature of -20°C were tested respectively. Table 1 shows the corresponding electrochemical test data.

[0040] Table 1 Lithium-ion battery performance

[0041]

[0042] The 1C first cycle low-temperature efficiency at -20℃ specifically refers to the coulombic efficiency of 1C cycle at -20℃.

[0043] It can be seen from Table 1 that the hollow multi-shell lithium iron phosphate material of the present invention has a higher charge and discharge capacitance, excellent low temperature performance, and a higher electrical conductivity and ion migration rate.

[0044] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A carbon-coated hollow multi-shell spherical lithium iron phosphate, characterized in that: It includes a multi-shell structure from the inside to the outside, with a cavity structure between adjacent shell structures, the shell structure includes a lithium iron phosphate-carbon microsphere shell layer and a carbon coating layer, the inner side of the innermost shell structure is a cavity structure, the lithium iron phosphate-carbon microsphere shell layer is attached to the inner surface of the carbon coating layer, and the lithium iron phosphate-carbon microsphere shell layer includes a carbon microsphere shell layer and attached lithium iron phosphate.

2. The method for preparing the carbon-coated hollow multi-shell spherical lithium iron phosphate according to claim 1, characterized in that: The method is: 1) Precursor microspheres are prepared by spray drying using sucrose as a carbon source, and then the precursor microspheres are calcined and carbonized to obtain a hollow multi-shell carbon microsphere structure; 2) The hollow multi-shell carbon microspheres, lithium source and phosphate salt are added to a solvent to react to obtain a hollow multi-shell lithium phosphate-carbon microsphere shell; 3) The hollow multi-shell lithium phosphate-carbon microsphere shell and the iron salt are mixed, and a hollow multi-shell spherical lithium iron phosphate-carbon microsphere shell is generated by a hydrothermal reaction. The shell is then reacted in a citric acid solution and then calcined at a high temperature under an inert atmosphere to finally obtain a carbon-coated hollow multi-shell spherical lithium iron phosphate.

3. The method for preparing the carbon-coated hollow multi-shell spherical lithium iron phosphate according to claim 2, characterized in that: In step 1), the method for preparing hollow multi-shell carbon microspheres with sucrose is as follows: a sucrose solution is spray-dried to prepare precursor microspheres.

4. The method for preparing the carbon-coated hollow multi-shell spherical lithium iron phosphate according to claim 2, characterized in that: Step 1) The precursor microspheres are carbonized in a tubular sintering furnace under an inert atmosphere to obtain porous hollow multi-shell structured carbon microspheres.

5. The method for preparing the carbon-coated hollow multi-shell spherical lithium iron phosphate according to claim 2, characterized in that: In step 2), the lithium source is LiOH, Li2CO3 or LiCH3COO; The phosphate salt is NH4H2PO4 and / or (NH4)2HPO4.

6. The method for preparing the carbon-coated hollow multi-shell spherical lithium iron phosphate according to claim 2, characterized in that: In step 2), the reaction time in the solvent is 1-3 hours, and then the mixture is allowed to stand and precipitate; The precipitate in step 2) is sintered under an inert atmosphere at a temperature of 300-400° C. for 3-6 hours.

7. The method for preparing the carbon-coated hollow multi-shell spherical lithium iron phosphate according to claim 2, characterized in that: Step 3) the iron salt is a ferrous salt; Step 3) The temperature of hydrothermal synthesis is 160-180°C and the time is 3-12h.

8. The method for preparing the carbon-coated hollow multi-shell spherical lithium iron phosphate according to claim 2, characterized in that: Step 3) The precipitate obtained by hydrothermal synthesis is dried under an inert atmosphere.

9. Use of the carbon-coated hollow multi-shell spherical lithium iron phosphate according to claim 1 in lithium batteries.