A medium-high entropy layered lithium-rich cathode oxide and preparation method thereof

Through the multi-element doping and citric acid combustion method of medium-high entropy layered lithium-rich cathode oxides, the problems of irreversible oxygen release and structural phase change of layered lithium-rich cathode materials under high voltage in the existing technology are solved, and the Higher capacity and more stable battery performance at lower voltages.

CN115566186BActive Publication Date: 2024-10-22PEKING UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202211421676.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-14
Publication Date
2024-10-22
Estimated Expiration
2042-11-14

AI Technical Summary

Technical Problem

Existing layered lithium-rich cathode materials suffer from irreversible oxygen release and structural phase change at high voltages, resulting in voltage decay and poor compatibility, making it difficult to achieve high capacity at lower voltages.

Method used

Using medium-high entropy layered lithium-rich cathode oxide Li1+xNi1-x-y-zMnyMzO2, it is prepared by multi-element doping and citric acid combustion method to increase the configuration entropy, reduce the activation voltage of oxygen anions, and perform in air or oxygen atmosphere Sintering improves the structural stability of the material.

Benefits of technology

Obtaining higher discharge specific capacity in the voltage range of 2.0-4.5V, reducing the voltage decay rate and oxygen anion activation voltage, improving compatibility with electrolytes, and extending the cycle stability of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115566186B_ABST
    Figure CN115566186B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a medium-high entropy layered lithium-rich positive electrode oxide, and relates to the technical field of lithium ion batteries. The method comprises the following steps: dissolving soluble salts of lithium, nickel and manganese and soluble salts of several M elements in deionized water; dissolving monohydrate citric acid in the water and stirring the water, so that the citric acid and metal ions undergo hydrolysis and condensation reactions to obtain a gel; heating the gel to fully burn the organic matter to obtain a fluffy powder, sintering, and naturally cooling to obtain a medium-entropy / high-entropy layered lithium-rich positive electrode oxide. The medium-entropy / high-entropy layered lithium-rich positive electrode material prepared by the invention has better structural stability, and the multi-element distribution reduces the local order degree in the structure, inhibits the migration of transition elements and the accompanying unfavorable structural phase change during the cycle, so that the voltage decay is slower, and the system configuration entropy is increased to reduce the activation voltage of oxygen anions in the layered lithium-rich positive electrode, and a higher discharge specific capacity is obtained at 4.5V.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lithium ion batteries, and in particular to a medium-high entropy layered lithium-rich positive electrode oxide and a preparation method thereof. Background Art

[0002] Lithium-ion batteries are currently the most widely used energy storage devices, and are used in many fields such as portable devices, grid energy storage, and electric vehicles. With the development of science and technology, people's demand for high-energy-density lithium-ion batteries is also increasing. 1+x TM 1-x O2 is a promising high specific capacity (>250mAh g -1 ) positive electrode materials, in the voltage range of 2.0-4.8V, not only the transition metal cations undergo redox to contribute capacity, but also activate oxygen anions to participate in the redox process and contribute additional capacity. However, this type of layered lithium-rich positive electrode material still has the following problems:

[0003] (1) Before 4.5V, the capacity is basically contributed by transition metal cations, while oxygen anions participate in oxidation, which requires a higher activation voltage (usually 4.5-4.8V). However, this process is generally accompanied by irreversible oxygen release. Oxygen attacks the electrolyte and produces side reactions at the interface between the positive electrode and the electrolyte. Both high voltage and oxygen release make the lithium-rich positive electrode material poorly compatible with traditional EC / DMC electrolytes, posing a safety hazard.

[0004] (2) Layered lithium-rich cathode materials + The escape and generation of oxygen vacancies can easily induce the migration and rearrangement of transition metal atoms, eventually leading to an irreversible structural phase transition from layered → spinel → rock salt phase, accompanied by the valence reduction of the transition metal, and obvious voltage decay after multiple charges and discharges.

[0005] Currently, most modification strategies focus on surface coating modification or bulk phase single doping. These efforts have slowed down the occurrence of side reactions and phase transition processes to a certain extent, but higher capacity can still be achieved at high voltage (≥4.6V). Summary of the invention

[0006] The object of the present invention is to provide a medium-high entropy layered lithium-rich positive electrode oxide and a preparation method thereof to solve the problems raised in the background technology.

[0007] To achieve the above object, the present invention provides the following technical solutions:

[0008] A medium-high entropy layered lithium-rich cathode oxide, the chemical formula of the layered lithium-rich cathode oxide is Li 1+x Ni 1-x-y- z Mny M z O2,

[0009] In the formula, the value range of x, y, and z is 0.1≤x≤0.2, 0.3≤y≤0.6, 0≤z≤0.3, 0.2≤1-xyz≤0.35;

[0010] The M element is one or a mixture of Co, Al, Ti, Zr, Nb, Mo and W elements; wherein the configuration entropy S of the layered lithium-rich positive electrode oxide is config ≥1.0R;

[0011] When the configuration entropy S config ≥1.5R is high entropy, and when 1.0R≤S config When <1.5R, it is medium entropy. When S config When <1.0R, it is low entropy.

[0012] The embodiment of the present invention also provides a method for preparing a medium-high entropy layered lithium-rich positive electrode oxide, the preparation method comprising the following steps:

[0013] S01: dissolving soluble salts of lithium, nickel and manganese and soluble salts of several M elements in deionized water to obtain a clear solution 1;

[0014] S02: dissolving the chelating agent citric acid monohydrate in the clear solution 1, and stirring thoroughly to obtain a clear solution 2;

[0015] S03: heating the clarified solution 2 in a water bath at 70°C with stirring for 2-3h to allow the citric acid and metal ions to fully undergo hydrolysis and condensation reactions to obtain a gel;

[0016] S04: Heat the gel obtained in S03 at 300°C for 2-3h to fully burn the organic matter to obtain a brown-black fluffy powder. After fully grinding the fluffy powder, place it in an alumina crucible and pre-sinter it at 450-500°C for 3h in air or oxygen atmosphere. Then continue to raise the temperature to 800-900°C for high-temperature sintering for 12h. Then naturally cool it down to obtain a medium-entropy / high-entropy layered lithium-rich positive electrode oxide.

[0017] On the basis of the above technical solution, the present invention also provides the following optional technical solution:

[0018] In an optional embodiment, the soluble salt of lithium is a mixture of one or more of lithium hydroxide, lithium nitrate and lithium acetate.

[0019] In an optional embodiment, the soluble salts of nickel and manganese are both acetates, nitrates, or a mixture of one or more thereof.

[0020] In an optional embodiment: among the soluble salts of element M, the cobalt source and the aluminum source are one or more mixtures of acetates and nitrates; the titanium source is ammonium titanium oxalate or other soluble titanium salts, the zirconium source is zirconium oxalate or other soluble zirconium salts, the niobium source is ammonium niobium oxalate or other soluble niobium salts, the molybdenum source is ammonium molybdate or other soluble molybdenum salts, and the tungsten source is ammonium tungstate or other soluble tungsten salts.

[0021] In an optional solution, the molar concentration of the lithium salt in step S01 is 5% in excess.

[0022] In an optional solution: in step S02, the molar ratio of citric acid monohydrate to metal ions is 1:1.

[0023] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0024] 1. The method of preparing medium-entropy / high-entropy layered lithium-rich cathode materials by multi-element doping has achieved a higher discharge specific capacity at 2.0-4.5V. The additional capacity beyond the theoretical capacity of metal cations can be attributed to the capacity contribution of oxygen anions. The increase in configurational entropy reduces the activation voltage of oxygen anions, reducing their charge cutoff voltage from 4.8V to 4.5V, and improving their compatibility with the electrolyte;

[0025] 2. The medium-entropy / high-entropy layered lithium-rich cathode material prepared by the present invention has better structural stability. The multi-element distribution reduces the degree of local order in the structure, inhibits the migration of transition elements and the accompanying adverse structural phase changes during the cycle, and thus has a slower voltage decay. It also increases the system configuration entropy to reduce the activation voltage of oxygen anions in the layered lithium-rich cathode, thereby obtaining a higher discharge specific capacity at 4.5V. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a powder X-ray diffraction comparison diagram of the low-entropy, medium-entropy and high-entropy layered lithium-rich positive electrodes in Example 1.

[0027] Figure 2 The low entropy, medium entropy and high entropy layered lithium-rich cathodes in Example 1 are 20 mAg in the voltage range of 2.0-4.5 V. -1 The charge and discharge curve diagram below.

[0028] Figure 3 The low entropy, medium entropy and high entropy layered lithium-rich cathodes in Example 1 are 200 mA g -1 The following cycle graph.

[0029] Figure 4 It is a cyclic voltammetry curve of the low entropy, medium entropy and high entropy layered lithium-rich positive electrode in Example 1 at 0.1 mV / s in the voltage range of 2.0-4.5V. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical scheme and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. The various embodiments listed in the present invention are only used to illustrate the present invention and are not used to limit the scope of the present invention. Any obvious modifications or changes made to the present invention do not depart from the spirit and scope of the present invention.

[0031] Example 1

[0032] Preparation of high entropy layered lithium-rich cathode material Li by citric acid combustion method 1.15 Ni 0.35 Mn 0.3 Co 0.05 Al 0.05 Ti 0.05 Mo 0.05 The O2 process includes the following steps:

[0033] S01: lithium acetate dihydrate (0.0120 mol), nickel acetate tetrahydrate (0.0035 mol), manganese acetate tetrahydrate (0.003 mol), cobalt acetate tetrahydrate (0.0005 mol), aluminum nitrate nonahydrate (0.0005 mol), ammonium titanium oxalate (0.0005 mol), and ammonium molybdate (containing Mo 0.0005 mol) were dissolved in 40 mL of deionized water in sequence to obtain a clear solution 1, wherein the molar concentration of the lithium salt was 5% excess;

[0034] S02: dissolving chelating agent citric acid monohydrate (0.0205 mol) in clear solution one, and stirring thoroughly to obtain clear solution two, wherein the molar ratio of citric acid monohydrate to metal ions is 1:1;

[0035] S03: heating the clarified solution 2 in a water bath at 70°C with stirring for 2-3h to allow the citric acid and the metal to undergo sufficient hydrolysis and condensation reaction to obtain a gel;

[0036] S04: The gel obtained in S03 is heated at 300°C for 2-3h to fully burn the organic matter to obtain a brown-black fluffy powder. After being fully ground, it is placed in an alumina crucible, placed in a muffle furnace, and heated to 500°C at a heating rate of 5°C / min in an air atmosphere for low-temperature pre-sintering for 3h, and then continued to heat to 900°C at a heating rate of 5°C / min for high-temperature sintering for 12h. The layered lithium-rich positive electrode oxide Li is obtained by naturally cooling. 1.15 Ni 0.35 Mn 0.3 Co 0.05 Al 0.05 Ti 0.05 Mo 0.05 O2.

[0037] In this embodiment, a citric acid combustion method is also provided to prepare a low entropy layered lithium-rich positive electrode material Li 1.2 Ni 0.2 Mn 0.6 O2 and intermediate entropy layered lithium-rich cathode material Li 1.2 Ni 0.3 Mn 0.4 Ti 0.05 Mo 0.05 O2; comprising the following steps:

[0038] S01: For Li 1.2 Ni 0.2 Mn 0.6 O2, lithium acetate dihydrate (0.0120 mol), nickel acetate tetrahydrate (0.0020 mol), and manganese acetate tetrahydrate (0.0060 mol) are dissolved in 40 mL of deionized water in sequence to obtain a clear solution A1, wherein the molar concentration of the lithium salt is 5% excess;

[0039] For Li 1.2 Ni 0.3 Mn 0.4 Ti 0.05 Mo 0.05 O2, lithium acetate dihydrate (0.0120 mol), nickel acetate tetrahydrate (0.0030 mol), manganese acetate tetrahydrate (0.0040 mol), ammonium titanium oxalate (0.0005 mol), and ammonium molybdate (containing Mo 0.0005 mol) were dissolved in 40 mL of deionized water in sequence to obtain a clear solution B1, wherein the molar concentration of the lithium salt was 5% excess;

[0040] S02: dissolving the chelating agent citric acid monohydrate (0.0205 mol) in the clear solutions A1 and B1, respectively, and stirring thoroughly to obtain clear solutions A2 and B21, wherein the molar ratio of citric acid monohydrate to metal ions is 1:1;

[0041] S03: The clarified solutions A2 and B2 were heated in a water bath at 70°C and stirred for 2-3 hours to allow the citric acid and the metal to undergo sufficient hydrolysis and condensation reactions to obtain gels A3 and B3, respectively;

[0042] S04: The gels A3 and B3 obtained in S03 were heated at 300°C for 2-3h to fully burn the organic matter and obtain brown-black fluffy powders. After being fully ground, they were placed in an alumina crucible and placed in a muffle furnace. In an air atmosphere, they were heated to 500°C at a heating rate of 5°C / min and pre-sintered at low temperature for 3h. Then, they were heated to 900°C at a heating rate of 5°C / min and sintered at high temperature for 12h. The low-entropy layered lithium-rich cathode materials Li 1.2 Ni 0.2Mn 0.6 O2 and intermediate entropy layered lithium-rich cathode material Li 1.2 Ni 0.3 Mn 0.4 Ti 0.05 Mo 0.05 O2.

[0043] The low-entropy, medium-entropy and high-entropy layered lithium-rich positive electrode oxides prepared in this embodiment are respectively mixed with conductive agent acetylene black and binder PVDF in a mass ratio of 8:1:1 to prepare slurry and then coated to form positive electrode sheets.

[0044] See attached Figure 1-Figure 4 The tests on the low entropy, medium entropy and high entropy layered lithium-rich cathode oxides prepared in this embodiment are as follows: Figure 1-4 middle:

[0045] a is the low entropy layered lithium-rich positive electrode oxide Li in Example 1 1.2 Ni 0.2 Mn 0.6 O2;

[0046] b is the intermediate entropy layered lithium-rich cathode oxide Li in Example 1 1.2 Ni 0.3 Mn 0.4 Ti 0.05 Mo 0.05 O2;

[0047] c is the high entropy layered lithium-rich cathode oxide Li in Example 1 1.15 Ni 0.35 Mn 0.3 Co 0.05 Al 0.05 Ti 0.05 Mo 0.0 5O2.

[0048] In the voltage range of 2.0-4.5V, 20mAg -1 The constant current charge and discharge test was carried out at a current density of 200mAg -1 The stability test was carried out with the current density of 1000 Nm.

[0049] At 20mAg -1 At a current density of 1.34 W, the discharge specific capacities of low-entropy, medium-entropy, and high-entropy lithium-rich cathodes are 119 mAh g -1 , 182mAh g -1 , 183mAh g -1 .

[0050] At 200mAg -1 At a current density of 1.34 W, the discharge specific capacity of the low-entropy, medium-entropy, and high-entropy lithium-rich cathodes is 90 mAh g-1 , 143mAh g -1 , 152mAh g -1 After 100 cycles, the capacity retention rates were 91.3%, 88.1%, and 85.5%, respectively, and the voltage decay was 1.81mV / cycle, 0.81mV / cycle, and 0.32mV / cycle.

[0051] The theoretical capacity contributed by metal cations in low-entropy, medium-entropy, and high-entropy lithium-rich cathodes is calculated to be 126 mAh g -1 , 154mAh g -1 and 181mAh g -1 When the above theoretical capacity is reached during charging, the voltages corresponding to the low-entropy, medium-entropy and high-entropy lithium-rich cathodes are 4.47V, 4.26V and 4.21V respectively. The cyclic voltammetry curves show that the medium-entropy lithium-rich cathode and the high-entropy lithium-rich cathode have an oxidation peak at around 4.3V, corresponding to the oxidation process of oxygen anions, which is not present in the low-entropy lithium-rich cathode.

[0052] Example 2

[0053] Preparation of high entropy layered lithium-rich cathode materials Li by citric acid combustion method 1.15 Ni 0.25 Mn 0.3 Co 0.1 Al 0.1 Ti 0.05 Mo 0.05 The O2 process includes the following steps:

[0054] S01: lithium acetate dihydrate (0.0120 mol), nickel acetate tetrahydrate (0.0025 mol), manganese acetate tetrahydrate (0.003 mol), cobalt acetate tetrahydrate (0.001 mol), aluminum nitrate nonahydrate (0.001 mol), ammonium titanium oxalate (0.0005 mol), and ammonium molybdate (containing Mo 0.0005 mol) were dissolved in 40 mL of deionized water in sequence to obtain a clear solution 1, wherein the molar concentration of the lithium salt was 5% excess;

[0055] S02: dissolving chelating agent citric acid monohydrate (0.0205 mol) in clear solution one, and stirring thoroughly to obtain clear solution two, wherein the molar ratio of citric acid monohydrate to metal ions is 1:1;

[0056] S03: heating the clarified solution 2 in a water bath at 70°C with stirring for 2-3h to allow the citric acid and the metal to undergo sufficient hydrolysis and condensation reaction to obtain a gel;

[0057] S04: The gel obtained in S03 is heated at 300°C for 2-3h to fully burn the organic matter to obtain a brown-black fluffy powder. After being fully ground, it is placed in an alumina crucible, placed in a muffle furnace, and heated to 450°C at a heating rate of 5°C / min in an air atmosphere for low-temperature pre-sintering for 3h, and then continued to heat to 900°C at a heating rate of 5°C / min for high-temperature sintering for 12h. The layered lithium-rich positive electrode oxide Li is obtained by naturally cooling. 1.15 Ni 0.25 Mn 0.3 Co 0.1 Al 0.1 Ti 0.05 Mo 0.05 O2.

[0058] The high entropy layered lithium-rich positive electrode oxide prepared in this example was mixed with the conductive agent acetylene black and the binder PVDF in a mass ratio of 8:1:1 and then coated to form a positive electrode sheet. -1 The constant current charge and discharge test was carried out with a current density of 185 mAh g -1 , at 200mA g -1 The discharge capacity is 138 mAh g -1 After 100 cycles, the capacity retention rate is 87.6% and the voltage decay is 0.63mV / cycle.

[0059] Example 3

[0060] Preparation of high entropy layered lithium-rich cathode materials Li by citric acid combustion method 1.2 Ni 0.3 Mn 0.3 Co 0.05 Al 0.05 Ti 0.05 Mo 0.05 The O2 process includes the following steps:

[0061] S01: lithium acetate dihydrate (0.0126 mol), nickel acetate tetrahydrate (0.003 mol), manganese acetate tetrahydrate (0.003 mol), cobalt acetate tetrahydrate (0.0005 mol), aluminum nitrate nonahydrate (0.0005 mol), ammonium titanium oxalate (0.0005 mol), and ammonium molybdate (containing Mo 0.0005 mol) were dissolved in 40 mL of deionized water in sequence to obtain a clear solution 1, wherein the molar concentration of the lithium salt was 5% excess;

[0062] S02: dissolving chelating agent citric acid monohydrate (0.0206 mol) in clear solution one, and stirring thoroughly to obtain clear solution two, wherein the molar ratio of citric acid monohydrate to metal ions is 1:1;

[0063] S03: heating the clarified solution 2 in a water bath at 70°C with stirring for 2-3h to allow the citric acid and the metal to undergo sufficient hydrolysis and condensation reaction to obtain a gel;

[0064] S04: The gel obtained in S03 is heated at 300°C for 2-3h to fully burn the organic matter to obtain a brown-black fluffy powder. After being fully ground, it is placed in an alumina crucible, placed in a muffle furnace, and heated to 500°C at a heating rate of 5°C / min in an air atmosphere for low-temperature pre-sintering for 3h, and then continued to heat to 800°C at a heating rate of 5°C / min for high-temperature sintering for 12h. The layered lithium-rich positive electrode oxide Li is obtained by naturally cooling. 1.2 Ni 0.3 Mn 0.3 Co 0.05 Al 0.05 Ti 0.05 Mo 0.05 O2.

[0065] The high entropy layered lithium-rich positive electrode oxide prepared in this example was mixed with a conductive agent, acetylene black, and a binder, PVDF, in a mass ratio of 8:1:1 to form a slurry, which was then coated to form a positive electrode sheet.

[0066] At 20mA g in the voltage range of 2.0-4.5V -1 The constant current charge and discharge test was carried out with a current density of 188 mAh g -1 , at 200mA g -1 The discharge capacity is 136 mAh g -1 After 100 cycles, the capacity retention rate is 81.6% and the voltage decay is 0.34mV / cycle.

[0067] It can be seen that the medium-entropy / high-entropy layered lithium-rich positive electrode materials prepared in the above three examples have higher discharge specific capacity, better capacity retention rate and lower voltage decay rate in the voltage range of 2.0-4.5V.

[0068] The above is only a specific implementation of the present disclosure, but the protection scope of the present disclosure is not limited thereto. Any person skilled in the art who is familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed in the present disclosure, which should be included in the protection scope of the present disclosure. Therefore, the protection scope of the present disclosure should be based on the protection scope of the claims.

Claims

1. A method for preparing a medium-high entropy layered lithium-rich cathode oxide, characterized in that: The following steps are involved: S01: 0.0120 mol lithium acetate dihydrate, 0.0035 mol nickel acetate tetrahydrate, 0.003 mol manganese acetate tetrahydrate, 0.0005 mol cobalt acetate tetrahydrate, 0.0005 mol aluminum nitrate nonahydrate, 0.0005 mol ammonium titanium oxalate, and ammonium molybdate containing 0.0005 mol of Mo were dissolved in 40 mL of deionized water in sequence to obtain a clear solution 1, in which the molar concentration of the lithium salt was 5% in excess; S02: dissolving 0.0205 mol of chelating agent citric acid monohydrate in clear solution one, and stirring thoroughly to obtain clear solution two, wherein the molar ratio of citric acid monohydrate to metal ion is 1:1; S03: heating the clarified solution 2 in a water bath at 70°C with stirring for 2-3h to allow the citric acid and the metal to undergo sufficient hydrolysis and condensation reaction to obtain a gel; S04: The gel obtained in S03 is heated at 300°C for 2-3h to fully burn the organic matter to obtain a brown-black fluffy powder. After being fully ground, it is placed in an alumina crucible, placed in a muffle furnace, and heated to 500°C at a heating rate of 5°C / min in an air atmosphere for low-temperature pre-sintering for 3h, and then continued to heat to 900°C at a heating rate of 5°C / min for high-temperature sintering for 12h. The layered lithium-rich positive electrode oxide Li is obtained by naturally cooling. 1.15 Ni 0.35 Mn 0.3 Co 0.05 Al 0.05 Ti 0.05 Mo 0.05 O2.

Citation Information

Cited By

  • Surface-modified high-entropy lithium-manganese-rich positive electrode material as well as preparation method and application thereof

    CN119764379A