A method for enhancing spin orbital moment through hydrogen ion migration based on electric field modulation

By controlling the adsorption and desorption of hydrogen ions on the surface of a heavy metal layer using an electric field, the problems of low spin current efficiency and high energy consumption in spin orbital moment devices are solved. This achieves reversible control of spin orbital moment and miniaturization of the device, resulting in low energy consumption and high reversibility.

CN115605072BActive Publication Date: 2026-11-17SHANDONG UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211275091.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-18
Publication Date
2026-11-17
Estimated Expiration
2042-10-18

AI Technical Summary

Technical Problem

Existing spin-orbit moment (SOT) devices have low spin current generation efficiency and are difficult to control, resulting in high device energy consumption, which limits their application in high-performance, low-power spintronic memories and logic devices.

Method used

By using an electric field to regulate the movement of hydrogen ions in a heterojunction device, the properties of the heavy metal layer are modified to enhance or reduce its spin orbital moment. A water-doped ionic liquid is used as a gating medium, and an electric double layer is formed by the electric field to control the adsorption and desorption of hydrogen ions on the surface of the heavy metal layer, thereby achieving reversible control of the spin orbital moment.

Benefits of technology

It improves the efficiency of spin orbital moment generation, reduces device energy consumption, achieves device miniaturization and reversibility, avoids leakage current problems of oxide gate, and has a simple process with good repeatability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115605072B_ABST
    Figure CN115605072B_ABST
Patent Text Reader

Abstract

This invention discloses a method for improving the spin-orbit moment of a heavy metal layer. It consists of a ferromagnetic layer and a heavy metal layer, which are in contact with each other. Reversible, non-volatile control of the spin-orbit moment of the heavy metal layer can be achieved through the migration of hydrogen ions under positive and negative gate voltages. A Hall device is also provided, comprising a substrate, the aforementioned thin film, a gate, a side electrode, and a gate electrode. It can be fabricated using ultraviolet lithography, argon ion etching, and magnetron sputtering techniques. This Hall device contains a heavy metal layer that is easily adsorbed by hydrogen ions; the hydrogen ion coverage on the surface of the heavy metal layer can be adjusted by regulating the gate voltage, thereby controlling the spin-orbit moment of the heavy metal layer. The gate is a water-doped ionic liquid with good dielectric properties. The device fabrication process is simple and reproducible, and it can be used for information storage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of microelectronic device fabrication, and specifically relates to a method for improving spin orbital moment. Background Technology

[0002] For decades, the control of magnetic and spin phenomena corresponding to the switching between the fundamental "0" and "1" signals in information technology has been a subject of intense interest. Early magnetoelectronic devices achieved data writing by controlling magnetization reversal through magnetic fields or current-based spin-orbit torque (STT) effects. However, both types of devices suffer from large space volumes and high energy losses. Current-induced spin-orbit torque (SOT) mediates the transfer of angular momentum from the lattice to the magnetic layer, leading to sustained magnetic oscillations or switching of magnetic structures. In heavy metal (HM) / ferromagnetic (FM) heterojunctions, an applied current can generate a spin current due to the spin Hall effect (SHE) and the interface Rashba effect (REE). The spin current flowing into the ferromagnetic layer applies SOT to the magnetic moment, which can be used to switch the magnetization direction of the ferromagnet, driving domain wall (DW) and skyrmion motion, showing great potential in magnetic storage, high-frequency magnetic devices, logic computing, and neuromorphic computing.

[0003] The current bottleneck limiting the application of SOT devices lies in the still low and difficult-to-control generation efficiency of spin current or SOT, resulting in relatively high energy consumption. In recent years, driven by the pursuit of higher performance, numerous experimental studies on SOT modulation have emerged. These studies employ methods such as annealing, intercalation with different layers, interface oxidation, and strain modulation to modulate SOT. Their main mechanisms involve adjusting the interfacial atomic mixing degree, adding additional interfaces to increase spin sources or spin transparency and reduce spin memory loss, altering the magnetic anisotropy of the FM layer, and changing the mismatch between atoms. However, all of these methods for controlling SOT alter the physical properties of the heterojunction, which is impractical after device fabrication. Another effective method for controlling magnetization is through electric field control. This is crucial for realizing high-performance, low-power spintronic memories and logic devices with reversible and non-volatile advantages. Summary of the Invention

[0004] The purpose of this invention is to provide a method for improving spin orbital moment. By using an electric field to modulate the motion of hydrogen ions, the properties of heavy metals can be modified, thereby increasing the efficiency of their spin orbital moment generation.

[0005] The heterojunction device structure provided by the present invention consists of a substrate, a heavy metal layer 1 (HM1), a heavy metal layer 2 (HM2), a ferromagnetic layer (FM), a heavy metal layer 3 (HM3), and a protective layer, from bottom to top. The heavy metal layers 1 and 2 have opposite spin Hall angles.

[0006] The specific structure of the heterojunction described in this invention includes: a substrate / HM1 / HM2 / FM / HM3 / protective layer. The substrate can be selected from Si, SiO2, and MgO. HM1 can be selected from W, Pt, Ta, Hf, and Pd, with a thickness of 0.25–5 nm. HM2 can be selected from W, Pt, Ta, Hf, and Pd, with a thickness of 0.25–5 nm. However, HM1 and HM2 must have opposite spin Hall angles, such as combinations like W / Pt, Pt / W, or Ta / Pt. The FM layer can be selected from Co, CoFeB, NiFe, and Fe, with a thickness of 0.6–30 nm. The aforementioned HM3 can be selected from W, Pt, Ta, Hf, and Pd, with a thickness of 0.1–1.24 nm. The protective layer serves to protect the underlying film from oxidation. It can be selected from one of TaN, AlOx, MgO, or SiO2, and its thickness can be 0.5-3 nm.

[0007] The working principle of the method for enhancing the spin-orbit moment of the heavy metal layer described in this invention is as follows: A water-doped ionic liquid is applied to the gate electrode and the channel of the device to form a gate. A gate voltage is applied to the thin film through the gate electrode. When hydrogen ions in the ionic liquid are adsorbed on the surface of the heavy metal layer HM3 under the action of a positive gate voltage, the spin Hall conductivity of HM3 is enhanced, thereby enhancing the spin-orbit moment of HM3. When hydrogen ions are desorbed on the surface of HM3 under the action of a negative gate voltage, the spin Hall conductivity of HM3 is reduced, thereby reducing the spin-orbit moment of HM3.

[0008] The device fabrication method provided by the present invention includes the following steps: (1) thin film deposition is performed by magnetron sputtering to obtain a heterojunction thin film with good quality; (2) the obtained sample is exposed to ultraviolet light by ultraviolet exposure to obtain a thin film sample with photoresist pattern on the surface; (3) the thin film outside the photoresist protection is etched by argon ion etching technology; (4) gate electrodes and side electrodes are fabricated by magnetron sputtering and stripping process to finally obtain Hall device, spin-orbit moment ferromagnetic resonance (ST-FMR) device and magnetic domain track device; (5) water-doped ionic liquid is dropped between the gate electrode and the device channel, and wires are led out from each electrode by ultrasonic spot welding machine; (6) SMR, critical current, second harmonic, ST-FMR and magneto-optical Kerr effect (MOKE) tests are performed.

[0009] In step (1), the conditions for preparing the thin film by the magnetron sputtering method are as follows: the background vacuum for all film depositions is better than 1.5 × 10⁻⁶. -4The deposition pressure was 0.2 Pa. All metal films were grown using low-power DC sputtering, and all oxide films were grown using RF sputtering. Low-power growth is beneficial for obtaining films with good flatness and quality. The Ar gas used in the film sputtering process had a purity of 99.99% and a flow rate of 20-40 Sccm (specifically 23 Sccm), O2 had a purity of 99.99% and a flow rate of 0.7-12 Sccm (specifically 10 Sccm), and N2 had a purity of 99.99% and a flow rate of 0.7-12 Sccm (specifically 0.7 Sccm).

[0010] In step (2), the photoresist used for ultraviolet exposure of the obtained sample is ARP-5350, and the developer is AR 300-26. The conditions for the ultraviolet exposure technique are as follows: ultraviolet light wavelength 10-400nm (specifically 365nm), power density 40-80mJ / cm². 2 (Specifically, it could be 55mJ / cm) 2 The exposure time is 4-30s (specifically 6s). The development conditions are as follows: use AR 300-26 developer to dilute at a developer:water ratio of 1:7, develop for 30s, remove and rinse with deionized water for 30s to obtain the photoresist-protected Hall device pattern, ST-FMR device pattern and magnetic domain raceway device pattern.

[0011] In step (3), the conditions for argon ion etching are as follows: argon pressure is 0.005-0.2 Pa (specifically 0.02 Pa); cathode current is 5-8 A (specifically 6.5 A); arc voltage is 45-50 V (specifically 50 V); plate voltage is 450-500 V (specifically 450 V); accelerating voltage is 180-300 V (specifically 200 V); neutralization current is 4.5-5.0 A (specifically 4.5 A); beam current is 60-200 mA (specifically 90 mA); etching time is 1 min-5 min (specifically 2 min). After argon ion etching, the sample is immersed in acetone for 10-40 minutes (15 minutes in particular), and then cleaned with an ultrasonic cleaner for 0.5-2 minutes (1 minute in particular) to obtain thin films with Hall patterns, ST-FMR patterns and magnetic domain raceway patterns.

[0012] In step (4), the gate electrode and side electrode are fabricated sequentially using ultraviolet exposure, magnetron sputtering, and lift-off processes. The magnetron sputtering conditions are as follows: the Ti magnetron sputtering growth rate is 0.03-0.05 nm / s (specifically 0.035 nm / s), and the growth time is 300-900 s (specifically 300 s); the Pt magnetron sputtering growth rate is 0.10-0.20 nm / s (specifically 0.10 nm / s), and the growth time is 300-1000 s (specifically 300 s). Both the side electrode and the gate electrode are bilayer films of Ti and Pt from bottom to top, wherein the thickness of the Ti film is 10-30 nm (specifically 10 nm), and the thickness of the Pt film is 30-100 nm (specifically 30 nm). The stripping process is as follows: immersion in acetone for 0.5-40 minutes (specifically 15 minutes), followed by ultrasonic cleaning for 0.5-2 minutes (specifically 1 minute) to remove the photoresist. This ultimately yields Hall devices, ST-FMR devices, and magnetic domain track devices.

[0013] The Hall device has a rectangular channel in the center, i.e., the Hall channel, with a width of 2-500 μm. Four symmetrical branch channels are evenly distributed on both sides of the Hall channel, connecting and combining with it. The four symmetrical branch channels have the same shape, but there are no specific requirements for their shape. Rectangular regions are connected to the ends of the Hall channel and the four symmetrical branch channels. The side length of the rectangular region connecting to the Hall channel is wider than the Hall channel. The rectangular regions are connected to each other through the Hall channel and the four symmetrical branch channels. The gate electrode is distributed on a substrate on one side of the Hall channel. The gate electrode does not contact the Hall channel, and its distance from the Hall channel in the plane is 50-200 μm, specifically 50 μm.

[0014] In step (5), the ionic liquid may be selected from N,N-diethyl-N-(2-methoxyethyl)-N-ammonium-bis-(trifluoromethylsulfonyl)-imide (DEME-TFSI) or 1-ethyl-3-methylimidazolium-bis-(trifluoromethylsulfonyl)-imide (EMIM-TFSI).

[0015] The volume ratio of the ionic liquid to water can be 1:1000–1:10 (specifically 1:100). The amount of ionic liquid used is sufficient to cover the lateral channels of the Hall device (covering the two cross-shaped structures) and most of the gate electrodes, enabling the Hall channels and gate electrodes of the Hall device to be connected through the ionic liquid. The specific amount of ionic liquid used can be 10-20 μL.

[0016] The procedure for covering the water-doped ionic liquid at the intersection of the gate electrode and the Hall channel is as follows: Water-doped ionic liquid is dropped onto the Hall channel using a probe, covering the Hall channel and the gate electrode (voltage needs to be applied to the device through the gate electrode). Wires are then led from each electrode using an ultrasonic spot welder for testing. In the device with the dropped ionic liquid, an external gate voltage V is applied. G A double electric layer is formed, thereby generating an electric field effect on the channel, allowing for hydrogen ion implantation and extraction into the thin film channel, and controlling the hydrogen ion concentration on the surface of the heavy metal layer.

[0017] In step (6), the SMR, critical current, second harmonic, ST-FMR, and MOKE tests are performed. For SMR, critical current, and second harmonic, Hall effect devices are used. For the SMR test, a current I is applied between points S and D, the SMR is measured between points C and B, and a gate voltage V is applied between points G and D. G Test R respectively CB The magnetic field and angle vary. For the critical current test, a current I is passed between points S and D, and the anomalous Hall magnetoresistance R is measured between points A and B. Hall A gate voltage V is applied between points G and D. G Test R Hall With the assistance of an external magnetic field (along the x-direction), the magnetization reversal is monitored by varying the amplitude of a pulsed current. For the second harmonic test, an alternating current I is applied between points S and D, and a lock-in amplifier SR830 is used to measure the first harmonic (V) between points A and B. ω ) and second-order (V 2ω Harmonic Hall voltage, with a gate voltage V applied between points G and D. G Test V respectively ω and V 2ω With H x and H y The changes ultimately extract the effective fields of damping-like and field-like.

[0018] In the ST-FMR test, microwave RF current is passed through points S and D, and a gate voltage V is applied between points G and D. GWhen a microwave radio frequency current is passed through the thin film, a transverse spin current is generated in the heavy metal layer and injected into the ferromagnetic layer. This exerts an oscillating spin moment on the ferromagnetic layer, causing magnetic precession. Due to the anisotropic magnetoresistance of the ferromagnetic layer, this causes oscillations in the bilayer film resistance. The oscillating resistance and radio frequency current generate a DC voltage. Measuring the change of this DC voltage with the magnetic field can be used to quantitatively analyze the spin current absorption of the ferromagnetic layer.

[0019] In the MOKE test, a current I flows between points S and D, and a gate voltage V is applied between points G and D. G First, an appropriate out-of-plane magnetic field is applied to drive the nucleation and propagation of the DW to the desired location. Second, a MOKE polarimeter is used to detect the nucleation and propagation of the DW by an out-of-plane field H in the presence of a small longitudinal current I. z The DW propagates under the influence of current flowing in the HM bar. This current generates a damping-like torque in the DW, acting similarly to an out-of-plane magnetic field H. eff =χj, where χ is the spin Hall efficiency, j is the current density, which depends on the sign of the longitudinal current, and H eff The externally applied magnetic field H can propagate Néel DW z The left-right offset causes a change in the propagation field Hp of the Néel DW. The spin Hall efficiency χ is obtained by measuring the change ΔHp in the DW propagation field and dividing it by the current j.

[0020] Compared with the prior art, the present invention has the following characteristics:

[0021] (1) The heterojunction thin film involved in this invention is at the atomic level in terms of thickness, which meets the semiconductor process's pursuit of device miniaturization.

[0022] (2) This type of switch is highly scalable. Common heavy metal materials can be modified with hydrogen ions to enhance the spin Hall effect generated by heavy metals.

[0023] (3) Controlling the hydrogen ion migration process using an electric field has the advantages of low energy consumption, good reversibility, and easy implementation.

[0024] (4) Using ionic liquid as the gate medium, the double layer formed under the action of electric field can generate a huge electric field, which is far better than that of general oxide gate.

[0025] (5) Ionic liquids have good dielectric properties and do not have the leakage problem of general oxide gates.

[0026] (6) The device fabrication process is simple and has good repeatability. Attached Figure Description

[0027] Figure 1 The thin film structure of the present invention Figure 1 (a) and Hall devices Figure 1 (b) ST-FMR devices Figure 1 (c) and magnetic domain track devices Figure 1 (d) Schematic diagram.

[0028] Figure 2 The curves of the anomalous Hall values ​​of the Hall device W(3nm) / Pt(3nm) / Co(0.7nm) / Pt(0.75nm) / TaN(0.8nm) samples prepared for this invention under different voltages as a function of pulse current are shown in the figures: (a) Curves of the anomalous Hall values ​​of the W(0.25nm) / Pt(5nm) / Co(0.7nm) / Pt(0.75nm) / TaN(0.8nm) samples under different voltages as a function of pulse current; (b) Curves of the anomalous Hall values ​​of the W(3nm) / Pt(3nm) / Co(0.7nm) / Pt(0.75nm) / TaN(0.8nm) samples under different voltages as a function of pulse current; (c) Curves of the critical current for magnetization reversal of the W(0.25nm) / Pt(5nm) / Co(0.7nm) / Pt(0.75nm) / TaN(0.8nm) samples under different voltages as a function of pulse current; (d) Curves of the critical current for magnetization reversal of the W(0.25nm) / Pt(5nm) / Co(0.7nm) / Pt(0.75nm) / TaN(0.8nm) samples under different voltages as a function of pulse current; (d) Curves of the critical current for magnetization reversal of the W(0.25nm) / Pt(5nm) / Co(0.7nm) / Pt(0.75nm) / TaN(0.8nm) samples under different voltages as a function of pulse current.

[0029] Figure 3 The time-of-flight secondary ion mass spectrometry (SIMS) test results of the thin film in the examples mainly show the change in hydrogen ion content with film thickness. Detailed Implementation

[0030] The method of the present invention will be described below through specific embodiments, but the present invention is not limited thereto.

[0031] Unless otherwise specified, the experimental methods described in the following examples are conventional methods; the reagents and materials described are commercially available unless otherwise specified.

[0032] Example:

[0033] (1) Using a magnetron sputtering apparatus, multilayer thin films with the following structures were deposited: W(3nm) / Pt(3nm) / Co(0.7nm) / Pt(0.75nm) / TaN(0.8nm) and W(0.25nm) / Pt(5nm) / Co(0.7nm) / Pt(0.75nm) / TaN(0.8nm). The background vacuum for deposition was better than 1.5 × 10⁻⁶. -4The substrate used for deposition was Si / SiO2, which was ultrasonically cleaned for 2 minutes each with acetone, alcohol, and deionized water before deposition. Deposition of W, Pt, and Co was carried out in high-purity Ar (99.99%) at 0.2 Pa with an argon flow rate of 23 sccm. Deposition of TaN was carried out in a mixture of high-purity Ar (99.99%) and high-purity N2 (99.99%) at 0.2 Pa with nitrogen and argon flow rates of 7 sccm and 23 sccm, respectively. W, Pt, Co, and TaN were all grown by DC sputtering at relatively low power outputs of 13.2 W, 11.6 W, 10.4 W, and 12.2 W, respectively.

[0034] (2) The obtained sample was subjected to ultraviolet (UV) exposure using the UV exposure method, specifically as follows: substrate cleaning treatment—spin-coating photoresist onto the substrate and baking the photoresist—exposing with a mask—development, to obtain a thin film sample with a photoresist pattern on the surface; the substrate cleaning treatment conditions were as follows: the sample was ultrasonically cleaned for 2 min each in acetone, alcohol, and deionized water. The spin-coating and baking conditions were as follows: ARP-5350 photoresist was used, spin-coated at 4000 rpm for 1 min, and pre-baked at 110℃ for 3 min. The mask exposure conditions were as follows: a mask with a Hall effect device was placed on top of the sample, and then UV exposure was performed using a UV wavelength of 365 nm and a power density of 55 mJ / cm². 2 The exposure time was 6 seconds. The development conditions were as follows: AR 300-26 developer was used to dilute the solution at a ratio of developer to water of 1:7. After development for 30 seconds, the solution was removed and rinsed with deionized water for 30 seconds to obtain a thin film covered with a photoresist pattern.

[0035] (3) The sample was etched using argon ion etching technology under the following conditions: the background vacuum during etching was better than 5 × 10⁻⁶. - 4 The etching process involves the following parameters: argon pressure of 0.005-0.2 Pa (specifically 0.02 Pa); cathode current of 5-8 A (specifically 6.5 A); arc voltage of 45-50 V (specifically 50 V); plate voltage of 450-500 V (specifically 450 V); accelerating voltage of 180-300 V (specifically 200 V); neutralization current of 4.5-5.0 A (specifically 4.5 A); beam current of 60-200 mA (specifically 90 mA); and etching time of 1-5 min (specifically 2 min). After argon ion etching, the sample is immersed in acetone for 10-40 min (specifically 15 min) and then cleaned with an ultrasonic cleaner for 0.5-2 min (specifically 1 min), yielding thin films with Hall effect patterns, ST-FMR patterns, and magnetic domain raceway patterns.

[0036] (4) Fabrication of gate and side electrodes using a substrate cleaning process—spin-coating photoresist on the substrate, baking the photoresist—exposing with a mask—development—magnetron sputtering—lift-off process: The substrate cleaning conditions are as follows: the sample is ultrasonically cleaned in acetone and alcohol for 2 min each. The photoresist coating and pre-baking conditions on the substrate are as follows: ARP-5350 photoresist is used, spin-coated at 4000 rpm for 1 min, and pre-baked at 110℃ for 3 min. The mask exposure conditions are as follows: a mask with gate and side electrodes is placed on top of the sample, and then ultraviolet exposure is performed with an ultraviolet wavelength of 365 nm and a power density of 55 mJ / cm². 2 The exposure time is 6 seconds. The development conditions are as follows: develop with AR 300-26 developer for 30 seconds, without post-baking.

[0037] The magnetron sputtering conditions are as follows: Ti sputtering growth rate is 0.035 nm / s, growth time is 300 s; Pt sputtering growth rate is 0.1 nm / s, growth time is 300 s. The stripping process conditions are as follows: acetone soaking for 15 min followed by ultrasonic cleaning for 1 min to remove the photoresist, resulting in various patterned devices.

[0038] The morphology of the obtained Hall device is as follows Figure 1 As shown in the device schematic diagram in (b), from Figure 1 (b) The schematic diagram of the Hall device shows that: the Hall device has a rectangular channel in the middle, namely the Hall channel, and four symmetrical branch channels are evenly distributed on both sides of the Hall channel, which are connected and combined with the Hall channel; the four symmetrical branch channels have the same shape, but there are no specific requirements for the shape; the ends of the Hall channel and the four symmetrical branch channels are connected to rectangular areas, and the side length of the rectangular area connected to the Hall channel is wider than the Hall channel. The rectangular areas are connected to each other through the Hall channel.

[0039] (5) Using a probe, drop a drop of water-doped ionic liquid N,N-diethyl-N-(2-methoxyethyl)-N-ammonium-bis(trifluoromethanesulfonyl)imide (DEME-TFSI) onto the gate electrode and Hall channel. The amount of liquid is 15 μL. The volume ratio of the ionic liquid to water can be 1:100. The size of the liquid covers the Hall channel of the Hall device (covering the two cross-shaped structures) and most of the gate electrode. The Hall channel and the gate electrode are connected by the ionic liquid.

[0040] (6) Measurement using lead wires from an ultrasonic spot welding machine: A current I flows between points S and D, with point S as the current input and point D as the current output; the Hall resistance R is measured between points A and B. Hall A gate voltage V is applied between points G and D. G .

[0041] A magnetic field was applied along the x-direction using a Versalab cavity, and a transport device was used to test the critical current for current-driven magnetization reversal. For example... Figure 2 As shown, for the W(3nm) / Pt(3nm) / Co(0.7nm) / Pt(0.75nm) / TaN(0.8nm) sample, gating was applied using a water-doped ionic liquid. Under a positive gate voltage, the critical current decreased, and under a negative gate voltage, the critical current recovered. For the W(0.25nm) / Pt(5nm) / Co(0.7nm) / Pt(0.75nm) / TaN(0.8nm) sample, under a positive gate voltage, the critical current increased, and under a negative gate voltage, the critical current recovered. This analysis, combined with time-of-flight secondary ion mass spectrometry (SIMS) results, further supports this trend. Figure 3 This study confirmed that hydrogen ions adsorb on the surface of the upper Pt metal under a positive gate voltage, thereby increasing the spin Hall conductivity of the upper Pt heavy metal and achieving reversible control of the spin orbital moment. Figure 2 It can be seen that only a very small gate voltage is needed to control the critical current, proving that the power consumption of this invention is very low.

[0042] according to Figure 1 The schematic diagram of the device is shown below. The main principle is analyzed as follows: W and Pt have opposite spin Hall angles. The net spin current generated depends on the relative thickness of W and Pt and the size of their relative spin Hall angles. The heavy metal Pt layer above the ferromagnetic layer will also transfer spin current to the ferromagnetic layer. Therefore, the net spin current flowing into the ferromagnetic layer depends on the relative thickness of the three heavy metal layers and the size of their relative spin Hall angles. Under a positive gate voltage, hydrogen ions in the water-doped ionic liquid adsorb onto the surface of the upper Pt layer, increasing the spin Hall conductivity of the upper Pt layer and thus increasing its spin orbital moment. Therefore, for the W(3nm) / Pt(3nm) / Co(0.7nm) / Pt(0.75nm) / TaN(0.8nm) sample (whose net spin current is dominated by the lower W and upper Pt layers), the positive gate voltage increases the net spin current flowing into the ferromagnetic layer and decreases its critical current. Conversely, for the W(0.25nm) / Pt(5nm) / Co(0.7nm) / Pt(0.75nm) / TaN(0.8nm) sample (whose net spin current is dominated by the lower Pt layer), the positive gate voltage decreases the net spin current flowing into the ferromagnetic layer and increases its critical current. In summary, this invention achieves the modulation of the spin orbital moment of the heavy metal layer through hydrogen ion migration. This invention has the advantages of being reversible and non-volatile.

[0043] The adsorption of hydrogen ions on the surface of the heavy metal Pt under a positive gate voltage can be confirmed by time-of-flight secondary ion mass spectrometry (SIMS) results, as shown in the figure below. Figure 3As shown, the hydrogen ion distribution with film depth indicates that the hydrogen ion content increases after a positive gate voltage is applied, especially on the surface of the heavy metal Pt. Furthermore, hydrogen ions and Pt elements disappear almost simultaneously, indicating that hydrogen ions are mainly adsorbed on the Pt surface.

Claims

1. A method for increasing the spin orbital moment of a heavy metal layer, characterized in that: It is composed of a substrate, heavy metal layer 1 (HM1), heavy metal layer 2 (HM2), ferromagnetic layer (FM), heavy metal layer 3 (HM3) and a protective layer. Among them, heavy metal layer 1 and heavy metal layer 2 have opposite spin Hall angles. HM1 is selected from one of W, Pt, Ta, Hf and Pd. HM2 is selected from one of W, Pt, Ta, Hf and Pd. HM3 is selected from one of W, Pt, Ta, Hf and Pd.

2. The method for increasing the spin orbital moment of a heavy metal layer as described in claim 1, characterized in that: The thickness of HM1 is 0.25–5 nm, the thickness of HM2 is 0.25–5 nm, the FM layer is selected from one of Co, CoFeB, NiFe, and Fe, and the thickness is 0.6–30 nm, and the thickness of HM3 is 0.1–1.24 nm; the protective layer is selected from one of TaN, AlOx, MgO, and SiO2 to protect the underlying film from oxidation, and its thickness is 0.5–3 nm.

3. The method for increasing the spin orbital moment of a heavy metal layer according to claim 2, characterized in that: The core component of the method for increasing the spin orbital moment of the heavy metal layer consists of heavy metal layer 1 (HM1), heavy metal layer 2 (HM2), ferromagnetic layer (FM), and heavy metal layer 3 (HM3), with the thickness of HM3 in the core component being 0.5-1.24 nm.

4. The application of the method for increasing spin orbital moment according to any one of claims 1-3 in the fabrication of microelectronic components.

5. A Hall effect device, comprising, as described in any one of claims 1-3, a substrate, a heavy metal layer 1 (HM1), a heavy metal layer 2 (HM2), a ferromagnetic layer (FM), a heavy metal layer 3 (HM3), and a protective layer, a gate, a side electrode, and a gate electrode, wherein, A Hall device is photolithographically patterned on one side of the sample, which consists of the substrate and the heavy metal layer 1 (HM1), heavy metal layer 2 (HM2), ferromagnetic layer (FM), heavy metal layer 3 (HM3) and protective layer in sequence. The Hall device has a Hall channel in the middle, which is a rectangular channel with a width of 2-500 μm. Four symmetrical branch channels are evenly distributed on both sides of the Hall channel. The four symmetrical branch channels have the same shape. The ends of the Hall channel and the four symmetrical branch channels are rectangular modules covering the side electrodes. The side length of the rectangular area connected to the Hall channel is wider than the Hall channel. The modules are connected to each other through the Hall channel and four symmetrical branch channels. The gate electrode is distributed on the substrate on one side of the Hall channel of the Hall device, and the gate electrode does not contact the Hall channel; the side electrode is distributed on the module at the end of the Hall channel and the four symmetrical branch channels; the gate covers the Hall channel and the gate electrode of the Hall device, connecting the two. The gate electrode is an ionic liquid selected from N,N-diethyl-N-(2-methoxyethyl)-N-ammonium-bis(trifluoromethanesulfonyl)imide or 1-ethyl-3-methylimidazolium-bis(trifluoromethanesulfonyl)imide; the amount of the ionic liquid used is 10-20 μL; both the side electrode and the gate electrode are bilayer films of Ti and Pt from bottom to top, wherein the thickness of the Ti film is 10-30 nm and the thickness of the Pt film is 30-100 nm; the distance between the gate electrode and the Hall channel in the Hall device in the plane is 50-200 μm.

6. A method for fabricating a Hall device, comprising fabricating the Hall device according to claim 5, characterized in that, Includes the following steps: (1) A high-quality heterojunction thin film was obtained by magnetron sputtering. (2) The obtained sample was exposed to ultraviolet light using the ultraviolet exposure method to obtain a thin film sample with a photoresist pattern on the surface; (3) Argon ion etching technology is used to etch the thin film outside the photoresist protection; (4) The door electrode and side electrode are fabricated by magnetron sputtering and stripping processes to finally obtain the Hall device.

7. The preparation method according to claim 6, characterized in that: In step (1), the conditions for preparing the thin film by magnetron sputtering are as follows: the background vacuum for all film depositions is better than 1.5 × 10⁻⁶. -4 The deposition pressure was 0.2 Pa. All metal films were grown using low-power DC sputtering, and all oxide films were grown using RF sputtering. Low-power growth is beneficial for obtaining films with good flatness and quality. The Ar gas used in the film sputtering process had a purity of 99.99% and a flow rate of 20-40 Sccm, the O2 gas had a purity of 99.99% and a flow rate of 7-12 Sccm, and the N2 gas had a purity of 99.99% and a flow rate of 7-12 Sccm. In step (2), the photoresist used for ultraviolet exposure of the obtained sample is ARP-5350, and the developer is AR 300-26. The conditions for the ultraviolet exposure technique are as follows: ultraviolet light wavelength 10-400nm, power density 40-80 mJ / cm². 2 The exposure time is 4-30 s; the development conditions are as follows: use AR 300-26 developer to dilute at a developer:water ratio of 1:7, develop for 30 s, take it out and rinse with deionized water for 30 s to obtain the Hall device pattern, ST-FMR device pattern and magnetic domain track device pattern protected by photoresist. In step (3), the conditions for argon ion etching are as follows: argon pressure is 0.005-0.2 Pa; cathode current is 5-8 A; arc voltage is 45-50 V; plate voltage is 450-500 V; accelerating voltage is 180-300 V; The neutralization current is 4.5-5.0A; the beam current is 60-200 mA; the etching time is 1 min-5 min; after argon ion etching, the sample is immersed in acetone for 10-40 min, and then cleaned with an ultrasonic cleaner for 0.5-2 min to obtain thin films with Hall patterns, ST-FMR patterns and magnetic domain raceway patterns. In step (4), during the fabrication of the gate electrode and side electrode, ultraviolet exposure technology, magnetron sputtering, and lift-off processes are used sequentially to fabricate the gate electrode and side electrode. The magnetron sputtering conditions are as follows: the growth rate of Ti magnetron sputtering is 0.03-0.05 nm / s, and the growth time is 300-900 s; the growth rate of Pt magnetron sputtering is 0.10-0.20 nm / s, and the growth time is 300-1000 s. Both the side electrode and the gate electrode are bilayer films of Ti and Pt from bottom to top, wherein the thickness of the Ti film is 10-30 nm, and the thickness of the Pt film is 30-100 nm. The lift-off process conditions are as follows: after soaking in acetone for 0.5-40 min, ultrasonic cleaning is used for 0.5-2 min to remove the photoresist. Finally, various patterned devices are obtained.

Citation Information

Patent Citations

  • Electric field regulating antiferromagnetic base Hall device and preparation method thereof

    CN104752604A

  • Spin orbit torque generating materials

    US20180166197A1