A binder for curing radiation cooling paint and radiation cooling paint
By treating epoxy resin and high-temperature free radical initiator at room temperature, an organic binder suitable for low-temperature environments is prepared, which solves the problems of low heat exchange efficiency and easy cracking of high-temperature coatings in low-temperature environments, and achieves high efficiency. The effect of heat exchange and extending coating life.
Patent Information
- Application Number
- CN202211424754.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-14
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-11-14
AI Technical Summary
Existing high-temperature radiation coatings are not suitable for low-temperature environments, resulting in low heat exchange efficiency for overhead wires in the power grid, and the coatings are prone to cracking and falling off during hot and cold shrinkage, affecting their service life.
Develop an organic binder that does not require high-temperature sintering. Through ring-opening reaction and high-temperature free radical initiator treatment at room temperature, a new unsaturated epoxy resin containing epoxy resin and unsaturated double bonds is prepared, and combined with multiple A combination of functional curing agents forms a radiation cooling coating suitable for low-temperature environments.
The binder reduces coating curing conditions, simplifies the coating process, improves the ductility and service life of the coating, and broadens the application fields of radiation coatings, including overhead wires in power grids and rapid heat transfer fields.
Smart Images

Figure CN115612064B_ABST
Abstract
Description
Technical Field
[0001] The invention discloses the technical field of polymer synthesis and radiation cooling coating preparation, and in particular relates to a binder for curing the radiation cooling coating and the radiation cooling coating. Background Art
[0002] In actual operation of overhead wires of power grids, the current passing through the wires will generate Joule heat inside, causing the temperature inside the wires to rise. Under the action of high temperature, the material properties, internal structure and various physical properties of the wires will undergo irreversible and harmful changes, such as decreased mechanical and fatigue properties and increased sag, which directly endanger the safe operation of the line. Generally speaking, the operating temperature of overhead wires should not be higher than 80°C. Therefore, the large amount of heat generated by overhead wires during operation must be dissipated in time. Existing overhead wire heat dissipation mainly relies on air circulation in the working environment. However, the efficiency of natural heat dissipation and cooling is insufficient, especially when the weather is hot and the line transmission load increases, the cooling effect is even worse.
[0003] Radiation cooling is a type of coating that can effectively accelerate the heat exchange between the coating and the surrounding environment, which can save energy and reduce consumption. It has been widely used in high-energy consumption industries such as petrochemicals and metallurgy. The existing technology mainly focuses on high-temperature radiation coatings, and the heat resistance temperature of the coating exceeds 1200°C. For example, patents CN202110441139.X and CN201910086879.9 both disclose technical methods for radiation coatings for boiler inner walls. After spraying, high-temperature radiation coatings need to be fired at a high temperature of more than 1000°C. The process is cumbersome, and due to the excessive use of inorganic binders, the coating is prone to cracking and falling off due to the influence of cold and hot shrinkage during actual application, thereby affecting the service life. For example, Table 1 in patent CN202111253565.7 lists some test data. Obviously, although high-temperature radiation coatings have good heat exchange functions, they are not suitable for heat exchange scenarios in low-temperature environments (below 200°C) such as overhead wires of power grids.
[0004] To this end, it is necessary to develop a coating with ductile binder and a radiant cooling coating suitable for low-temperature environments and with good heat exchange function. Summary of the invention
[0005] In order to solve the above problems, the present invention provides a binder for curing radiation cooling coating, and the binder is prepared by the following method:
[0006] Preparation of new unsaturated epoxy resin containing epoxy resin and unsaturated double bonds,
[0007] Preparation of multifunctional curing agents containing carboxylic acid, anhydride and unsaturated double bonds;
[0008] The novel unsaturated epoxy resin component and the multifunctional curing agent component are configured into an adhesive in a ratio of 100:30 to 100:50.
[0009] Furthermore, the novel unsaturated epoxy resin is prepared by the following method:
[0010] The carboxyl groups in the rosin structure dissolved in the reactive solvent are used to react with some epoxy groups in the epoxy resin, a catalyst is added, and a ring-opening reaction is carried out at room temperature to 60°C, and then the temperature is lowered to room temperature and a certain amount of high-temperature free radical initiator is continuously added to obtain the product.
[0011] Furthermore, a high temperature free radical initiator, an acid anhydride containing an unsaturated double bond, an alcohol containing an unsaturated double bond and a saturated acid anhydride compound are compounded in a certain ratio to obtain a multifunctional curing agent containing carboxylic acid, anhydride and unsaturated double bonds.
[0012] Furthermore, the reactive solvent is a small molecule monomer or oligomer containing unsaturated double bonds, and is soluble in rosin at room temperature to 60°C.
[0013] Furthermore, the concentration of rosin in the reactive solvent is 10% to 50%, and the weight content of the high-temperature free radical initiator in the novel epoxy resin component is 1.5% to 3%.
[0014] Furthermore, the reactive solvent is one of vinyl pyrrolidone, styrene, methyl styrene, methyl acrylate, ethyl acrylate, butyl acrylate, methyl methacrylate, ethyl methacrylate, butyl methacrylate, hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxyethyl methacrylate or hydroxypropyl methacrylate.
[0015] Furthermore, the catalyst ratio is 0.5% to 1% of the total weight of the reactants.
[0016] Furthermore, the catalyst is one of imidazole, pyridine, benzylamine or potassium hydroxide.
[0017] Furthermore, the epoxy resin is one of bisphenol A epoxy resin, novolac epoxy resin or aliphatic epoxy resin.
[0018] Furthermore, the molar number of the partially ring-opened epoxy groups accounts for 30% to 70% of the total molar number of the epoxy groups in the epoxy resin.
[0019] Furthermore, the high temperature free radical initiator is tert-butyl perbenzoate (TBPB) or dicumyl peroxide (DCP).
[0020] Furthermore, the unsaturated double-bond acid anhydride is one of maleic anhydride, dimethylmaleic anhydride, phenylmaleic anhydride or itaconic anhydride.
[0021] Furthermore, the alcohol containing an unsaturated double bond is one of hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxyethyl methacrylate or hydroxypropyl methacrylate.
[0022] Furthermore, the saturated acid anhydride is one of methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride or phthalic anhydride.
[0023] Furthermore, in the multifunctional curing agent component, the weight proportion of the multifunctional curing agent component is 25% to 50% of the unsaturated acid anhydride, 15% to 25% of the alcohol containing unsaturated double bonds, and 35% to 60% of the saturated acid anhydride.
[0024] According to another aspect of the present invention, a low-temperature radiation cooling coating is provided.
[0025] According to the mass percentage, the iron-cobalt-nickel-chromium oxide alloy powder is 30% to 60%; the graphene is 10% to 20%; and the binder described in any one of the above items is 30% to 50%.
[0026] Compared with the prior art, the adhesive and radiation coating provided by the present invention have the following advantages:
[0027] (1) Providing an organic binder that does not require high-temperature sintering, reducing the curing conditions of the coating and simplifying the coating coating process, which not only reduces the coating energy, but also lays a foundation for the application of batch coating of overhead wires in power grids;
[0028] (2) Compared with inorganic binders, organic matter naturally has good ductility and can adapt to the shrinkage or expansion of the coating in hot and cold environments without cracking or falling off, thus increasing the service life of the coating;
[0029] (3) It has broadened the application field of radiation coatings, not only providing an application basis for the heat dissipation of overhead wires and substations in power grids, but also providing possibilities for the application of many rapid heat conversion fields in the people's livelihood field, such as electric blankets, cooling clothing fabrics, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 The cooling efficiency of Example 5 is compared with that of Comparative Example 5. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0032] The binder of the present invention is an organic hybrid resin, which solves the technical problems in the prior art that radiation coatings need to be sintered at high temperatures (over 700° C.) and the coatings are prone to cracking and falling off. The binder is prepared by the following method:
[0033] The carboxyl groups in the rosin structure dissolved in the reactive solvent are used to react with some epoxy groups in the epoxy resin, and a catalyst is added to carry out a ring-opening reaction at room temperature to 60°C. The temperature is lowered to room temperature and a certain amount of high-temperature free radical initiator is continuously added to obtain a novel unsaturated epoxy resin containing epoxy resin and unsaturated double bonds.
[0034] A high temperature free radical initiator, an acid anhydride containing unsaturated double bonds, an alcohol containing unsaturated double bonds and a saturated acid anhydride compound are compounded in a certain ratio to obtain a multifunctional curing agent containing carboxylic acid, anhydride and unsaturated double bonds.
[0035] The novel unsaturated epoxy resin component and the multifunctional curing agent component are configured into an adhesive in a ratio of 100:30 to 100:50.
[0036] As an improvement of the scheme, the reactive solvent is a small molecule monomer or oligomer containing unsaturated double bonds, and is soluble in rosin at room temperature to 60°C. The reactive solvent in this scheme has the characteristics of containing double bonds and low viscosity, which can reduce the viscosity of the system before the adhesive is cured. After the adhesive is cured, it can be used as a reaction raw material to link to the polymer network through free radical copolymerization. There is no problem of non-reactive solvent volatilization during the curing process and migration to the surface after curing, thereby reducing mechanical and interfacial properties. It plays an important role in reducing VOC, improving adhesive performance and raw material utilization;
[0037] Rosin is a type of bio-based solid polymer containing carboxyl groups and double bonds with no fixed melting point. It has the advantages of a wide range of raw material sources and extremely low cost. Through the ring-opening and double-bond polymers of its carboxyl groups and some epoxy groups, the rosin can be cured into the final polymer network in a bifunctional manner. Polymers containing rosin have obvious advantages in light aging resistance, weather resistance, and outdoor application conditions.
[0038] In this application, rosin cannot be added to the system by melting or other means. The application of rosin in the entire adhesive can only be achieved by dissolving rosin in a reactive solvent.
[0039] As an improvement of the scheme, the concentration of rosin in the reactive solvent is 10% to 50%, and the weight content of the high temperature free radical initiator in the novel epoxy resin component is 1.5% to 3%. According to test results, if the concentration exceeds 50%, the excess rosin cannot be dissolved in the entire reactive solvent.
[0040] As an improvement of the scheme, the reactive solvent is one of vinyl pyrrolidone, styrene, methyl styrene, methyl acrylate, ethyl acrylate, butyl acrylate, methyl methacrylate, ethyl methacrylate, butyl methacrylate, hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxyethyl methacrylate or hydroxypropyl methacrylate. The reactive solvent should have the characteristics of functional reactive groups and good viscosity reduction effect. The functional reactive groups can ensure that all solvents are finally cured and cross-linked to the polymer network, so that there are no unreacted small molecules in the cured product, which plays an important role in improving mechanical properties and reducing VOC; good viscosity reduction effect can greatly improve the processability of adhesive preparation and the processability of the final product. All the existing commercially available reagents and industrial products that can meet the above requirements are listed, and the rest cannot meet the above requirements at the same time and cannot be applied to this technical solution.
[0041] As an improvement of the solution, the proportion of the catalyst is 0.5% to 1% of the total weight of the reactants.
[0042] As an improvement of the scheme, the catalyst is one of imidazole, pyridine, benzylamine or potassium hydroxide compounds. The selection of the catalyst in the system of the present invention should meet the following conditions: 1. Liquid or easily soluble solid, which is conducive to improving the utilization efficiency of the catalyst; 2. High catalytic efficiency, which requires that the nitrogen atom is directly connected to the benzene ring or is in a ring structure. Imidazole, pyridine and benzylamine meet the above requirements, while the other nitrogen-containing alkaline substances do not meet them. Potassium hydroxide meets the above requirements, and sodium hydroxide is also solid but easily soluble in reactive solvents, but its catalytic efficiency is not high, so it is not considered here. The other alkali metal hydroxides cannot meet the above two requirements at the same time.
[0043] As an improvement of the solution, the epoxy resin is one of bisphenol A epoxy resin, phenolic epoxy resin or aliphatic epoxy resin. The commercially available epoxy resins that can be used in the industrial field are mainly the above three types.
[0044] As an improvement of the scheme, the molar number of partially opened epoxy groups accounts for 30% to 70% of the total molar number of epoxy groups in the epoxy resin. If this value is too low, the effect of rosin cannot be fully exerted; if it is too high, the overall mechanical properties are poor.
[0045] As an improvement of the scheme, the high temperature free radical initiator is tert-butyl perbenzoate TBPB or diisopropylbenzene peroxide DCP. Free radical initiators are divided into low temperature initiators (80°C), medium temperature initiators (120°C) and high temperature initiators (180°C). The commercially available initiators suitable for high temperature are mainly the above two types, and you can choose one of them.
[0046] As an improvement of the solution, the unsaturated double-bond acid anhydride is one of maleic anhydride, dimethylmaleic anhydride, phenylmaleic anhydride or itaconic anhydride.
[0047] As an improvement of the scheme, the alcohol containing unsaturated double bonds is one of hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxyethyl methacrylate or hydroxypropyl methacrylate. The commercially available unsaturated alcohols containing double bonds are mainly the above four
[0048] As an improvement of the solution, the saturated acid anhydride is one of methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride or phthalic anhydride.
[0049] There are many types of acid anhydrides, but the acid anhydrides suitable for epoxy curing should meet two conditions. First, the acid anhydride is a cyclic acid anhydride, which is prepared by dehydration of dibasic acid molecules. After ring opening, it is a bifunctional group to improve the crosslinking degree of polymer curing; second, the acid anhydride molecule should contain a benzene ring or other cyclic structure to improve the mechanical strength of the polymer after curing. The above three types can meet the above two conditions at the same time. Acetic anhydride and the like are prepared by dehydration of monocarboxylic acid molecules, and molecules such as succinic anhydride do not have a cyclic structure, and the mechanical properties of the cured product are poor.
[0050] As an improvement of the solution, in the multifunctional curing agent component, the weight proportion of the multifunctional curing agent component is 25% to 50% of the unsaturated acid anhydride, 15% to 25% of the alcohol containing unsaturated double bonds, and 35% to 60% of the saturated acid anhydride.
[0051] The amount of unsaturated anhydride is determined based on the amount of double bonds in the entire system and the cross-linking strength after curing. The ratio of unsaturated double bond alcohol and unsaturated anhydride has a corresponding relationship, and the remaining anhydride is saturated anhydride. The high temperature free radical initiator has been added to the resin component and does not need to be added to the curing agent component.
[0052] According to another aspect of the present invention, a low-temperature radiation cooling coating is provided, and the preparation process is as follows:
[0053] According to the following mass percentages: 30% to 60% iron-cobalt-nickel-chromium oxide alloy powder; 10% to 20% graphene; 30% to 50% binder, the sintered, commercially available iron-cobalt-nickel-chromium oxide alloy powder is used as the base material of the radiation coating, a certain amount of commercially available graphene and the aforementioned binder are added, and the temperature is raised from room temperature to 180°C after ball milling and mixing. When the coating is cured in an environment of 180°C, the curing system is divided into three levels. Initially, when the temperature is below 80°C, the main reaction occurs between the unsaturated alcohol and the unsaturated anhydride with greater ring tension to generate unsaturated carboxylic acid; when the temperature rises to 80-120°C, the main cross-linking reaction occurs between the saturated anhydride and the unsaturated carboxylic acid and the epoxy group; when the temperature exceeds 120°C, the decomposition of the free radical initiator and the cross-linking curing between the unsaturated double bonds mainly occur.
[0054] Example 1
[0055] The resin component was prepared as follows:
[0056] Weigh 302g (1mol) of rosin resin and dissolve it in 302g of reactive solvent vinyl pyrrolidone, add 380g (1mol) of bisphenol A epoxy resin E51 (epoxy equivalent 190, epoxy mole number 2mol, Kunshan Nanya Company), stir evenly, continue to add 9.84g (1% of the total weight) of imidazole as a catalyst, stir and react at room temperature for 24h to obtain a light yellow transparent solution, continue to add 29.52g (3% of the total weight) of TBPB, stir evenly to obtain an unsaturated epoxy resin;
[0057] The curing agent component is prepared as follows:
[0058] Weigh 600 g of methyl hexahydrophthalic anhydride, 150 g of hydroxyethyl methacrylate, and 250 g of maleic anhydride, and stir and mix them evenly to obtain a multifunctional curing agent;
[0059] When curing or formulating the radiation coating, the resin component and the curing agent component are compounded in a weight ratio of 100:45.
[0060] Example 2
[0061] The resin component was prepared as follows:
[0062] Weigh 302g (1mol) of rosin resin and dissolve it in 2718g of reactive solvent styrene, then add 1500g of bisphenol A epoxy resin E20 (epoxy equivalent 500, epoxy mole 3mol, Kunshan Nanya Company), stir and dissolve evenly, then add 22.6g (0.5% of the total weight) of pyridine as a catalyst, stir and react at 60°C for 24h to obtain a light yellow transparent solution, then add 68.14g (1.5% of the total weight) of DCP, stir and obtain an unsaturated epoxy resin;
[0063] The curing agent component is prepared as follows:
[0064] Weigh 400 g of phthalic anhydride, 250 g of hydroxypropyl acrylate, and 350 g of dimethylmaleic anhydride, and stir and mix them evenly to obtain a multifunctional curing agent;
[0065] When curing or formulating the radiation coating, the resin component and the curing agent component are compounded in a weight ratio of 100:30.
[0066] Example 3
[0067] The resin component was prepared as follows:
[0068] Weigh 302g (1mol) of rosin resin and dissolve it in 755g of reactive solvent ethyl methacrylate, then add 250g of phenolic epoxy resin F44 (epoxy equivalent 175, epoxy mole 1.43mol, Shandong Shengquan Group), stir and dissolve evenly, then add 9.8g (0.75% total weight) of benzylamine as a catalyst, stir and react at 50°C for 24h to obtain a colorless transparent solution, then add 26.33g (2% total weight) of TBPB, stir and obtain an unsaturated epoxy resin curing agent component as follows:
[0069] Weigh 500 g of methyltetrahydrophthalic anhydride, 200 g of hydroxypropyl acrylate, and 300 g of itaconic anhydride, stir and mix them evenly to obtain a multifunctional curing agent;
[0070] When curing or formulating the radiation coating, the resin component and the curing agent component are compounded in a weight ratio of 100:50.
[0071] Example 4
[0072] The resin component was prepared as follows:
[0073] Weigh 302g (1mol) of rosin resin and dissolve it in 1208g of reactive solvent hydroxyethyl acrylate, then add 315g of aliphatic epoxy resin RMAT4221 (epoxy equivalent 126, epoxy mole 2.5mol, Shanghai Baoling Chemical Company), stir and dissolve evenly, then add 10.95g (0.6% total weight) of potassium hydroxide as a catalyst, stir and react at 30°C for 24h to obtain a colorless transparent solution, then add 33.05g (1.8% total weight) of DCP, stir and obtain an unsaturated epoxy resin curing agent component as follows:
[0074] Weigh 350 g of methyl hexahydrophthalic anhydride, 150 g of hydroxypropyl methacrylate, and 500 g of phenyl maleic anhydride, stir and mix them evenly to obtain a multifunctional curing agent; when curing or preparing radiation coatings, the resin component and the curing agent component are compounded at a weight ratio of 100:40.
[0075] Examples 5-8 are radiation coatings prepared using the adhesives of Examples 1-4, respectively, with the formulations shown in Table 1.
[0076]
[0077]
[0078] Comparative Examples 1 and 2 are commercially available inorganic binders, Comparative Examples 3 and 4 are radiation coatings prepared according to the ratio of Example 8 for Comparative Examples 1 and 2, respectively, with a curing temperature of 350° C. Comparative Examples 5 and 6 are common water-based anticorrosive coatings, with a curing temperature of 120° C. The elongation at break of the cured products of Examples 1-8 and the sintered products of Comparative Examples 1-4 were tested respectively, and the results are shown in Table 2.
[0079] Table 2 Comparison of elongation at break of adhesives
[0080] Example Elongation at break % Comparative Example Elongation at break % Example 1 3.8 Comparative Example 1 0.2 Example 2 3.6 Comparative Example 2 0.3 Example 3 3.6 Comparative Example 3 0.2 Example 4 3.2 Comparative Example 4 0.3 Example 5 2.5 Example 6 2.3 Example 7 2..4 Example 8 2.2
[0081] It can be seen from the test results in Table 2 that compared with commercially available inorganic binders, the binder prepared by the present invention has a better elongation at break; after being prepared into a radiation coating, the coating does not fall off even after being bent 90 degrees or 180 degrees, the coating has stable adhesion, can withstand thermal expansion and contraction, and is convenient for secondary processing.
[0082] The radiation heat dissipation performance test was continued for Examples 5-8 and Comparative Examples 3-6. The metal plates coated with radiation coating and of the same specifications were heated to 75°C and then cooled to 30°C at the same room temperature. The results are shown in Table 3.
[0083] Table 3 Comparison of heat dissipation performance of radiation coatings
[0084] Example Time(s) Comparative Example Time(s) Example 5 225 Comparative Example 3 269 Example 6 236 Comparative Example 4 277 Example 7 231 Comparative Example 5 348 Example 8 244 Comparative Example 6 366
[0085] It can be seen from Table 3 that in the process of cooling from the same temperature (75° C.) to room temperature in Example 5 and Comparative Example 3, the cooling rate of Example 5 always exceeds that of Comparative Example 3, indicating that the radiation coating prepared by the present invention has higher heat dissipation efficiency.
[0086] Figure 1 The cooling efficiency of Example 5 is compared with that of Comparative Example 5. Figure 1 It can be seen that the radiation coating prepared by the present invention takes less time to cool from the same temperature (75°C) to 30°C. In summary, compared with the prior art, the binder prepared by the present invention has excellent ductility and does not crack even after being bent at 180°C; its radiation heat dissipation performance is better than that of ordinary coatings and high-temperature sintered radiation coatings in the low temperature region.
[0087] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A binder for curing radiation cooling coating, characterized in that: The binder is prepared by the following method: Preparation of unsaturated epoxy resin containing epoxy resin and unsaturated double bonds, Preparation of multifunctional curing agents containing carboxylic acid, anhydride and unsaturated double bonds; The unsaturated epoxy resin component and the multifunctional curing agent component are configured into a binder according to a ratio of 100:30 to 100:50; The unsaturated epoxy resin is prepared by the following method: A catalyst is added, and at room temperature to 60°C, the carboxyl groups in the rosin structure dissolved in the reactive solvent are used to perform a ring-opening reaction on some epoxy groups in the epoxy resin, and the temperature is lowered to room temperature and a certain amount of free radical initiator is continuously added to obtain the product; A free radical initiator, an acid anhydride containing an unsaturated double bond, an alcohol containing an unsaturated double bond and a saturated acid anhydride compound are compounded in a certain ratio to obtain a multifunctional curing agent containing carboxylic acid, anhydride and unsaturated double bonds; The reactive solvent is a small molecule monomer or oligomer containing unsaturated double bonds, and is soluble in rosin at room temperature to 60°C.
2. A binder for curing radiation cooling coating according to claim 1, characterized in that: The concentration of rosin in the reactive solvent is 10% to 50%; the weight content of the free radical initiator in the epoxy resin component is 1.5% to 3%.
3. The adhesive for curing radiation cooling coating according to claim 1, characterized in that: The reactive solvent is one of vinyl pyrrolidone, styrene, methyl styrene, methyl acrylate, ethyl acrylate, butyl acrylate, methyl methacrylate, ethyl methacrylate, butyl methacrylate, hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxyethyl methacrylate or hydroxypropyl methacrylate.
4. The adhesive for curing radiation cooling coating according to claim 1, characterized in that: The catalyst ratio is 0.5% to 1% of the total weight of the reactants.
5. The adhesive for curing radiation cooling coating according to claim 1, characterized in that: The catalyst is one of imidazole, pyridine, benzylamine or potassium hydroxide.
6. A binder for curing radiation cooling paint as claimed in claim 1, characterized in that: The epoxy resin is one of bisphenol A epoxy resin, novolac epoxy resin or aliphatic epoxy resin.
7. The adhesive for curing radiation cooling paint according to claim 1, characterized in that: The molar number of partially ring-opened epoxy groups accounts for 30% to 70% of the total molar number of epoxy groups in the epoxy resin.
8. The adhesive for curing radiation cooling paint according to claim 1, characterized in that: The free radical initiator is tert-butyl perbenzoate (TBPB) or dicumyl peroxide (DCP).
9. The adhesive for curing radiation cooling paint according to claim 1, characterized in that: The unsaturated double bond anhydride is one of maleic anhydride, dimethyl maleic anhydride, phenyl maleic anhydride or itaconic anhydride.
10. The adhesive for curing radiation cooling paint according to claim 1, characterized in that: The alcohol containing unsaturated double bonds is one of hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxyethyl methacrylate or hydroxypropyl methacrylate.
11. The adhesive for curing radiation cooling paint according to claim 1, characterized in that: The saturated acid anhydride is one of methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride or phthalic anhydride.
12. The adhesive for curing radiation cooling coating according to claim 1, characterized in that: In the multifunctional curing agent component, the weight proportion of the multifunctional curing agent component is 25% to 50% of the unsaturated double bond anhydride, 15% to 25% of the unsaturated double bond-containing alcohol, and 35% to 60% of the saturated acid anhydride.
13. A low-temperature radiation cooling paint, characterized in that: The coating comprises, by mass percentage, 30% to 60% of iron-cobalt-nickel-chromium oxide alloy powder; 10% to 20% of graphene; and 30% to 50% of the binder described in any one of claims 1 to 12.
Citation Information
Patent Citations
High-temperature-resistant high-radiation coating used for furnace inner wall and preparation method of coating
CN109851335A
High-temperature high-emissivity infrared radiation coating as well as preparation method and use method thereof
CN113214685A
Infrared radiation coating and preparation method thereof
CN113755045A
Acrylic acid rosin and epoxy resin prepolymer and preparation method thereof
CN101544744A
Crylic acid rosin epoxy resin, curing method and application thereof
CN101638473A