A preparation method of micron-sized lithium ion sieve micro-H2TiO3 and a salt lake lithium extraction system using the ion sieve
By converting nano-scale lithium ion sieves into micron-scale lithium ion sieves and combining them with ultrafiltration membrane separation technology, the problems of lithium ion sieve loss and reduced adsorption performance during the lithium extraction process from salt lakes are solved, and an efficient and stable lithium ion sieve is achieved. adsorption effect.
Patent Information
- Application Number
- CN202211354430.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-01
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2042-11-01
AI Technical Summary
In the process of extracting lithium from salt lakes, existing lithium ion screens cannot be effectively used due to the small particle size of nano-scale powder, which causes sedimentation or loss. The adsorption capacity decreases after molding and cannot be effectively used. Moreover, commonly used binders will seal the nano-powder. leading to a decrease in adsorption performance.
The nano-sized lithium ion sieve precursor nano-Li2TiO3 is converted into the micron-sized lithium ion sieve precursor micro-Li2TiO3, and is acidified with hydrochloric acid to obtain the micron-sized lithium ion sieve micro-H2TiO3, which is combined with an ultrafiltration membrane for solid-liquid separation to avoid Powder loss and maintaining high adsorption capacity.
It achieves stable adsorption capacity and high utilization of the lithium ion screen, avoids powder loss, and does not cause blockage or closure of the salt lake lithium extraction system, ensuring the effectiveness and economy of the salt lake lithium extraction system.
Smart Images

Figure BDA0003920448750000071 
Figure BDA0003920448750000072 
Figure BDA0003920448750000081
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium extraction from salt lakes, in particular to a method for preparing a micron-sized lithium ion sieve micro-H2TiO3 that can be used to intercept lithium ions in water, and also relates to a salt lake lithium extraction system using the micron-sized lithium ion sieve micro-H2TiO3 obtained by the preparation method. Background Art
[0002] Lithium and its compounds are widely used in medicine, ceramics, glass, chemicals, electronics and other fields, and have attracted much attention. With the continuous expansion of demand for lithium and its compounds, terrestrial lithium resources are becoming increasingly scarce, and people have turned their attention to salt lakes that are rich in lithium resources. Due to the low concentration of lithium in salt lakes, lithium ion sieve adsorption materials have become the most promising and practical materials for lithium extraction from salt lakes, and have become a hot topic for scientists to study. Using lithium ion sieves with high adsorption capacity and high selectivity to adsorb lithium in salt lakes is a simple, easy, economical and green way to solve the shortage of lithium resources.
[0003] The existing lithium ion sieve H2TiO3 commonly used for lithium extraction from salt lakes is synthesized into nano-scale powder with an average particle size of 30-100nm. Directly adding it to the water for adsorption will cause the powder to settle and compact or lose in the water, so the powder usually needs to be molded. The general powder molding technology is to use a binder to bond and mold the nano lithium ion sieve into particles, which are filled in the adsorption column for adsorption. However, after the particles are molded, since many nano powders are wrapped or sealed by the binder, the adsorption capacity of the formed particle lithium ion sieve will decrease by about 50% compared with the powder lithium ion sieve. The decrease in adsorption capacity directly leads to a decrease in the effective utilization rate of the lithium ion sieve, an increase in the area occupied by the adsorption system and an increase in the engineering cost. If the molding process is not used, since the particle size of the lithium ion sieve powder is 30-100nm, the ultrafiltration membrane cannot be retained, and the nano-scale powder will pass through the membrane pores of the ultrafiltration membrane and lose a large amount of it. Therefore, it is impossible to directly use the "powder adsorption combined with ultrafiltration membrane separation" process to extract lithium from salt lakes.
[0004] For example, Chinese invention patent application CN 110975795A discloses a synthesis method for a lithium-extracting adsorbent, wherein the precursor of the lithium-ion sieve adsorbent Li2TiO3 is firstly obtained by calcination, and then the precursor Li2TiO3 is acid-eluted with lithium to obtain a metatitanic acid type lithium-ion sieve adsorbent H2TiO3. According to the description, the metatitanic acid type lithium-ion sieve adsorbent H2TiO3 is used in a lithium solution, and the adsorption amount is 33-39 mg / g. Obviously, this powder material has the aforementioned technical defects.
[0005] Chinese invention patent application CN 112871127A discloses a method for preparing high-porosity lithium ion sieve particles, wherein the lithium ion sieve is ground and then mixed with a pore-forming agent, a filler, and an aqueous resin emulsion, and then extruded and molded, and then dried and cured by heating, and finally acid-soaked and washed. The patent uses an aqueous resin emulsion as a binder, which can avoid the use of organic solvents, but the adsorption capacity and adsorption rate of the adsorbent after molding are lower than those of the powder, and the problem of decreased adsorption performance of the particles after molding is not solved. The adsorption amount is 12.6-18.1 mg / g.
[0006] Chinese invention patent application CN112871126A discloses a method for preparing lithium ion sieve particles with high adsorption capacity, wherein the lithium ion sieve powder is sand-ground and mixed with an inorganic binder and spray-dried, the obtained micron-sized particles are mixed with a template pore-forming agent, mixed with an aqueous resin emulsion in a granulation device for granulation, and the drying and curing process is completed by heating, and finally the particles are obtained after acid leaching and water washing. The granulation method of this patent is relatively complicated, and its adsorption capacity is about 22.2-25.1 mg / g.
[0007] Chinese invention patent application CN113996274A discloses a porous composite lithium adsorbent and a preparation method thereof, wherein an inorganic lithium adsorbent powder, a polymer skeleton material, an auxiliary agent, a volatile organic solvent, and a water-soluble organic solvent are uniformly mixed to obtain a composite lithium adsorbent precursor mixture; after granulating the precursor mixture, the mixture is placed in an atmosphere with a certain flow rate, humidity, and temperature to obtain a porous composite lithium adsorbent. The granulation process of this patent is relatively complicated, and the granules after granulation are prone to powder loss, and the problem of decreased adsorption performance of the granules after granulation cannot be solved, and the adsorption capacity is about 2 to 21 mg / g.
[0008] Chinese invention patent application CN 109266851A discloses a method for extracting lithium through a magnetic microporous lithium adsorbent, wherein the magnetic microporous lithium adsorbent is immersed in a lithium-containing solution so that at least part of the lithium ions therein are adsorbed by the magnetic microporous lithium adsorbent; the magnetic microporous lithium adsorbent is separated from the mixed system, and the lithium ions in the magnetic microporous lithium adsorbent are desorbed with water. This technology does not require granulation of the lithium ion sieve, and can retain the adsorption performance of the lithium ion sieve powder to the maximum extent. However, since the binding force between the magnetic substance and the lithium ion sieve powder is not strong enough, the magnetic substance and the lithium ion sieve powder will separate during continuous use, causing the loss of the lithium ion sieve powder and loss of magnetism, resulting in inability to continue to use. Summary of the invention
[0009] The purpose of the present invention is to overcome the defects of the prior art and provide a lithium ion sieve that can be directly added to water for adsorption without large-scale loss, without causing blockage or closure of other components in the salt lake lithium extraction system, and can be effectively recycled.
[0010] The idea of the present invention is to first convert the nano-Li2TiO3 lithium ion sieve precursor into micron-Li2TiO3 lithium ion sieve precursor, and then treat the micron-Li2TiO3 lithium ion sieve precursor with hydrochloric acid to obtain micron-H2TiO3 lithium ion sieve. Then, a salt lake lithium extraction system using the micron-H2TiO3 lithium ion sieve is designed, and a reciprocating ultrafiltration membrane is used for solid-liquid separation to verify the effective utilization rate and adsorption capacity of the lithium ion sieve, verify the adsorption capacity stability, adsorption rate change, powder utilization rate and other properties of the lithium ion sieve powder, and confirm whether the powder loss can be avoided.
[0011] In order to achieve the above object, the present invention provides a method for preparing a micron-sized lithium ion sieve micro-H2TiO3, the method comprising the following steps:
[0012] (1) Preparation of nano-scale lithium ion sieve precursor nano-Li2TiO3
[0013] Take anatase titanium dioxide and lithium carbonate powder at a molar ratio of 1:1.1-1.5, mix them thoroughly by mechanical stirring, then place the evenly mixed powder in a muffle furnace, and roast at a temperature of 700-900°C for 3-8h to obtain nano-scale lithium ion sieve precursor nano-Li2TiO3;
[0014] (2) Preparation of micron-sized lithium ion sieve precursor nano-Li2TiO3
[0015] Polyvinyl chloride, polyvinyl butyral, and polyvinylidene fluoride are used as composite binders, the mass of the composite binder is 5% to 15% of the total mass of the composite binder and the nano-scale lithium ion sieve precursor Li2TiO3, dimethylacetamide is used as an organic solvent for the composite binder, and the mass ratio of dimethylacetamide to the nano-scale lithium ion sieve precursor Li2TiO3 is 1.5 to 2:1;
[0016] Fully stir polyvinyl chloride, polyvinyl butyral, polyvinylidene fluoride, nano-scale lithium ion sieve precursor Li2TiO3 and dimethylacetamide at 50-80°C to obtain a mixed slurry, then add deionized water with a mass 4-8 times that of dimethylacetamide to the mixed slurry under high-speed stirring, and filter the slurry after full stirring to obtain a filter cake of micron-scale lithium ion sieve precursor micro-Li2TiO3;
[0017] (3) Preparation of micron-sized lithium ion sieve precursor nano-H2TiO3
[0018] The micron-sized lithium ion sieve precursor micro-Li2TiO3 obtained in step (2) is placed in 0.1-0.4 mol / L hydrochloric acid to make the molar ratio of micro-Li2TiO3 to HCl be 1:3-5. After sufficient stirring, the slurry is filtered and the filter cake obtained is the micron-sized lithium ion sieve micro-H2TiO3.
[0019] The present invention first converts a nano-scale lithium ion sieve precursor nano-Li2TiO3 into a micron-scale lithium ion sieve precursor micro-Li2TiO3, and then performs a hydrochloric acid acidification treatment on the micron-scale lithium ion sieve precursor micro-Li2TiO3 to obtain a micron-scale lithium ion sieve micro-H2TiO3. This process has two major effects: first, if the nano-Li2TiO3 powder is directly acidified, due to the small average particle size of the powder, the ultra-microfiltration membrane cannot retain these nano powders, resulting in serious powder loss. The present invention first converts nano-Li2TiO3 powder into micro-Li2TiO3 and then acidifies it, and the average particle size is large, so the lithium ion sieve and ultrafiltration membrane are used in combination in water bodies, and the ultrafiltration membrane can be used to intercept the powder, solving the problem of powder loss during application; secondly, if the nano-Li2TiO3 powder is directly granulated into 1-5mm particles and then acidified, since a large amount of nano powder is wrapped or sealed by a binder, this part of the nano powder cannot be acidified, so the utilization rate of the lithium ion sieve particles obtained by this structure is very low. The present invention first converts nano-Li2TiO3 powder into micro-Li2TiO3 powder and then acidifies it, and the average particle size of the obtained powder is 0.5-50μm, thereby avoiding the defect that a large amount of nano powder is included or sealed and cannot be acidified.
[0020] According to a preferred embodiment, the mechanical stirring time of step (1) is 1-2 hours, until the materials are fully mixed.
[0021] In the present invention, the weight ratio of polyvinyl chloride, polyvinyl butyral and polyvinylidene fluoride in step (2) is 1:1-2:1-3.
[0022] Preferably, in step (2), polyvinyl chloride, polyvinyl butyral, polyvinylidene fluoride, nanoscale lithium ion sieve precursor Li2TiO3 and dimethylacetamide are stirred at 50-80°C for 5-10 hours to obtain a mixed slurry. Deionized water is added to the mixed slurry at a flow rate of 0.1-1 L / min.
[0023] Preferably, the stirring time of step (3) is 10-20 hours.
[0024] The present invention also provides the use of the micron-sized lithium ion sieve micro-H2TiO3 obtained by the above preparation method in extracting lithium from salt lakes.
[0025] Based on this, the present invention provides a salt lake lithium extraction system using a micron-grade lithium ion sieve micro-H2TiO3, the system comprising a tank body (1), a hydrochloric acid storage tank (3), a salt lake brine storage tank (9), a hollow fiber ultrafiltration membrane (11) and a drive motor (12), the drive motor (12) being connected to the hollow fiber ultrafiltration membrane (11) and driving the hollow fiber ultrafiltration membrane (11) to reciprocate, an aeration device (2) being arranged at the bottom of the tank body (1), the hydrochloric acid storage tank (3) and the salt lake brine storage tank (9), and a driving motor (12). The water storage tank (9) is connected to the bottom of the pool body (1) through pipelines, characterized in that the pool body (1) is filled with micron-grade lithium ion sieve micro-H2TiO3 obtained by the preparation method according to any one of claims 1 to 6, the concentration of the micron-grade lithium ion sieve micro-H2TiO3 is 100g / L-200g / L, and the particle size is 0.5-50μm, and the hydrochloric acid storage tank (3) is filled with 0.1-0.4mol / L dilute hydrochloric acid as eluent.
[0026] The operation of the above-mentioned salt lake lithium extraction system is as follows:
[0027] (1) Adsorption stage
[0028] Adsorption begins: lithium-containing salt lake brine enters a pool (1) containing a micron-grade lithium ion sieve micro-H2TiO3 from a salt lake brine storage tank (9), with a hydraulic retention time of 1-5 BV / h, and the aeration device (2) is turned on to adjust the aeration volume to 100-200 L / min. When the water level of the pool (1) reaches 80%-90% of the pool height, the drive motor (12) is started to make the hollow fiber ultrafiltration membrane (11) reciprocate, and the reciprocating frequency is 0.5-5 Hz. The hollow fiber ultrafiltration membrane (11) is negatively pressured and sucked by an ultrafiltration membrane negative pressure suction device to obtain ultrafiltration membrane water production. At this time, the water inlet flow rate from the salt lake brine storage tank (9) to the pool (1) is equal to the water production flow rate of the ultrafiltration membrane;
[0029] Stop adsorption: monitor the lithium ion concentration in the water produced by the ultrafiltration membrane. When the lithium ion concentration of the produced water is 50%-80% of the lithium ion concentration of the water inlet pipe of the salt lake brine storage tank (9), it is considered that the adsorption of the micron-grade lithium ion sieve micro-H2TiO3 has reached saturation. At this time, stop the water inlet of the salt lake brine storage tank (9) to the pool body (1), stop the ultrafiltration membrane negative pressure suction device to stop the hollow fiber ultrafiltration membrane (11) from producing water, stop aeration, stop the reciprocating motion of the hollow fiber ultrafiltration membrane (11), and after natural sedimentation for 5-10 minutes, open the ultrafiltration membrane negative pressure suction device to suck the brine in the pool body (1) through the hollow fiber ultrafiltration membrane (11). When the water level of the pool body (1) drops to 20%-30% of the pool height, stop the ultrafiltration membrane negative pressure suction device;
[0030] (2) Elution stage
[0031] The dilute hydrochloric acid tank of the hydrochloric acid storage tank (3) is introduced into the pool body (1), and the ultrafiltration membrane negative pressure suction device is started. The hydraulic retention time is 1-3BV / h. The pH value of the ultrafiltration membrane produced water is monitored. When the pH value is the same as the pH value of the dilute hydrochloric acid in the hydrochloric acid storage tank (3), the introduction of the eluent is stopped, and the ultrafiltration membrane negative pressure suction device is started to cause the hollow fiber ultrafiltration membrane (11) to begin negative pressure suction. When the water level of the pool body (1) drops to 20%-30% of the pool height, the negative pressure suction device is stopped. At this time, the elution stage ends and the adsorption stage is re-entered.
[0032] The present invention starts from the nano-Li2TiO3, a precursor of the lithium ion sieve, to obtain the micron-H2TiO3 lithium ion sieve, and the specific surface area and pore volume of the obtained micron-H2TiO3 are significantly smaller than those of nano-Li2TiO3. The salt lake lithium extraction system designed based on the ion sieve material verifies the effective utilization rate and adsorption capacity of the lithium ion sieve, confirming that the lithium ion sieve powder has a stable adsorption capacity, a high powder utilization rate, and can effectively avoid powder loss. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 It is a SEM photo of the nano-scale lithium ion sieve precursor nano-Li2TiO3 and the micron-scale lithium ion sieve micro-H2TiO3 of Example 1;
[0034] Figure 2 It is a SEM photo of the nano-scale lithium ion sieve precursor nano-Li2TiO3 and the micron-scale lithium ion sieve micro-H2TiO3 of Example 2;
[0035] Figure 3 This is a schematic diagram of the structure of the salt lake lithium extraction system of Example 1. DETAILED DESCRIPTION
[0036] The following examples are used to explain the technical solutions of the present invention in a non-limiting manner.
[0037] In the present invention, unless otherwise specified, "%" used to describe concentration refers to mass percentage, and ":" refers to mass ratio.
[0038] Example 1
[0039] Preparation of nano-scale lithium ion sieve precursor nano-Li2TiO3:
[0040] The molar ratio of anatase titanium dioxide and lithium carbonate powder is 1:1.1, and the powder is placed in a blender for mechanical stirring and mixing for 1 hour. Then the evenly mixed powder is placed in a muffle furnace and calcined at 700°C for 3 hours to obtain a nano-scale lithium ion sieve precursor nano-Li2TiO3.
[0041] Preparation of micron-sized lithium ion sieve precursor micro-Li2TiO3:
[0042] Weigh equal amounts of polyvinyl chloride (PVC), polyvinyl butyral (PVB) and polyvinylidene fluoride (PVDF) as composite binders, and control the mass ratio of the composite binder to the nanoscale lithium ion sieve precursor Li2TiO3 to be 5:95. Weigh dimethylacetamide (DMAc) as the organic solvent of the composite binder, and control the mass ratio of DMAc to the nanoscale lithium ion sieve precursor Li2TiO3 to be 1.5:1. Stir polyvinyl chloride (PVC), polyvinyl butyral (PVB), polyvinylidene fluoride (PVDF), nanoscale lithium ion sieve precursor Li2TiO3 and dimethylacetamide (DMAc) at 50°C for 5h until they are uniformly mixed to obtain a mixed slurry. Weigh 4 times the mass of DMAc in deionized water, and then add the deionized water to the mixed slurry under high-speed stirring, control the flow rate of the deionized water so that all the deionized water is added to the mixed slurry within 1h, and then continue stirring for another 1h. After stopping stirring, the mixture is filtered, and the obtained filter cake is micron-grade lithium ion sieve precursor micro-Li2TiO3.
[0043] Preparation of micron-sized lithium ion sieve micro-H2TiO3: Measure hydrochloric acid with a concentration of 0.1 mol / L, the molar ratio of micro-Li2TiO3 to HCl is 1:3, place the micron-sized lithium ion sieve precursor micro-Li2TiO3 in the hydrochloric acid, stir for 10 hours to ensure that the materials are evenly mixed, filter the mixture, and the resulting filter cake is the micron-sized lithium ion sieve micro-H2TiO3.
[0044] The obtained nano-scale lithium ion sieve precursor nano-Li2TiO3 and micron-scale lithium ion sieve micro-H2TiO3 were characterized by using a BET fully automatic specific surface and porosity analyzer (Micromeritics ASAP2020HD88, USA), and the data in Table 1 were obtained. It can be seen that the specific surface area and pore volume of micro-H2TiO3 are significantly smaller than those of nano-Li2TiO3.
[0045] Table 1 BET characterization of nano-Li2TiO3 and micro-H2TiO3
[0046]
[0047] The nano-scale lithium ion sieve precursor nano-Li2TiO3 and the micron-scale lithium ion sieve micro-H2TiO3 were characterized by using LS-609 laser particle size analyzer (Europe and America Instruments Co., Ltd.), and the data in Table 2 were obtained. It can be seen that the particle size of the nano-scale lithium ion sieve precursor nano-Li2TiO3 is about 10-60nm, and the particle size of the micron-scale lithium ion sieve micro-H2TiO3 is about 5-40μm.
[0048] Table 2 BET characterization of nano-Li2TiO3 and micro-H2TiO3
[0049]
[0050] SEM photos of nano-Li2TiO3, a precursor of nano-lithium ion sieve, and micro-H2TiO3, a micron-lithium ion sieve, are shown in Figure 2. Figure 1 shown.
[0051] Verify the lithium ion adsorption capacity of nano-H2TiO3 (obtained by acidification of nano-Li2TiO3) and micro-H2TiO3:
[0052] 1g of powdered nano-H2TiO3 and micro-H2TiO3 were respectively put into 1L of lithium hydroxide aqueous solution, the lithium ion concentration in the solution was 300mg / L, and stirred for 3h. The water sample was taken to analyze the concentration of lithium ions, and the adsorption capacity of the two materials was calculated by the concentration difference of lithium ions to obtain the data in Table 3. It can be calculated that the adsorption capacity of micro-H2TiO3 in this embodiment is 93.2% of the adsorption capacity of nano-H2TiO3.
[0053] Table 3 BET characterization of nano-Li2TiO3 and micro-H2TiO3
[0054]
[0055] Experiment on lithium extraction from brine of micro-H2TiO3:
[0056] Set as Figure 3In the system shown, a uniformly distributed microporous aeration net 2 is arranged at the bottom of the stainless steel tank body 1, and the tank body has good uniform aeration. The hydrochloric acid storage tank 3 and the salt lake brine storage tank 9 are connected through the hydrochloric acid pipeline and the brine pipeline respectively. The hydrochloric acid pipeline is provided with a hydrochloric acid inlet pipe pH online detector 4 and a hydrochloric acid inlet pipe suction pump 5. The brine pipeline is provided with a salt lake brine inlet pipe suction pump 7 and a salt lake brine inlet pipe lithium ion concentration online monitor 8. The two pipelines are finally connected to the tank body liquid inlet 6 located at the bottom of the tank. A U-shaped hollow fiber ultrafiltration membrane 11 is installed in the stainless steel tank body 1, and the membrane is installed on the ultrafiltration membrane water production plate frame 17. The reciprocating swing of the ultrafiltration membrane in the tank body is realized by the swing power bracket 16 and the swing ultrafiltration membrane power motor device 12 connected to the bracket. The water production pipeline 15 of the ultrafiltration membrane is provided with a water production pipe lithium ion concentration online monitor 13 and a water production pipe pH online detector 14.
[0057] The cell body is loaded with micron-sized lithium ion sieve micro-H2TiO3, and the loading amount is 100g / L based on the total solvent in the cell body. During the operation stage, the liquid level in the cell body is usually maintained at 80-90% of the cell height.
[0058] The hydrochloric acid storage tank 3 is loaded with 0.1 mol / L dilute hydrochloric acid.
[0059] The salt lake brine storage tank 9 is loaded with the salt lake brine to be processed.
[0060] During operation, the salt lake brine in the salt lake brine storage tank 9 enters the pool body, the hydraulic retention time is 2BV / h, the aeration device is turned on so that the ratio of aeration volume to membrane filament water production (gas-water ratio) is 30:1, when the water level of the pool body reaches 80%-90% of the pool height, the motor is started to make the hollow fiber ultrafiltration membrane reciprocate, the reciprocating frequency is 1Hz, the hollow fiber ultrafiltration membrane is negatively sucked by the ultrafiltration membrane negative pressure suction device to obtain ultrafiltration membrane water production, and the water inlet flow rate of the salt lake brine storage tank (9) to the pool body 1 is controlled to be equal to the water production flow rate of the ultrafiltration membrane.
[0061] When the lithium ion concentration online monitor 13 of the water production pipe detects that the lithium ion concentration of the produced water is 50% of the lithium ion concentration of the water inlet pipe of the salt lake brine storage tank 9, it is considered that the adsorption of the micron-grade lithium ion sieve micro-H2TiO3 has reached saturation, and at this time, the water inlet from the salt lake brine storage tank (9) to the pool body (1) is stopped, and the ultrafiltration membrane negative pressure suction device is stopped to stop the hollow fiber ultrafiltration membrane (11) from producing water, aeration is stopped, and the reciprocating motion of the hollow fiber ultrafiltration membrane (11) is stopped. After natural sedimentation for 5-10 minutes, the ultrafiltration membrane negative pressure suction device is opened to suck the brine in the pool body (1) through the hollow fiber ultrafiltration membrane (11). When the water level of the pool body (1) drops to 20%-30% of the pool height, the ultrafiltration membrane negative pressure suction device is stopped;
[0062] The dilute hydrochloric acid tank of the hydrochloric acid storage tank (3) is introduced into the pool body (1), and the ultrafiltration membrane negative pressure suction device is started. The hydraulic retention time is 1 BV / h. The pH value of the ultrafiltration membrane produced water is monitored. When the pH value is the same as the pH value of the dilute hydrochloric acid in the hydrochloric acid storage tank (3), the introduction of the eluent is stopped, and the ultrafiltration membrane negative pressure suction device is started to cause the hollow fiber ultrafiltration membrane (11) to begin negative pressure suction. When the water level of the pool body (1) drops to 20%-30% of the pool height, the negative pressure suction device is stopped.
[0063] The brine of a salt lake in Tibet was tested as an experiment, and the inlet concentration and output water concentration of each component in the brine were tested, as shown in Table 4.
[0064] Table 4 Analysis of component concentration in lithium extraction process
[0065]
[0066] The experimental results show that the system can achieve the selective extraction of lithium ions from brine, with a lithium extraction rate of up to 96.7%. In addition, the titanium element was analyzed for the produced water after the membrane filament was filtered, and it was found that there was no titanium element in the produced water, proving that there was no dissolved titanium element in the produced water, and there were no powder particles that could pass through the membrane filament, that is, no powder loss.
[0067] Example 2
[0068] Preparation of nano-scale lithium ion sieve precursor nano-Li2TiO3:
[0069] The molar ratio of anatase titanium dioxide and lithium carbonate powder is 1:1.5, and the powder is placed in a blender for mechanical stirring and mixing for 3 hours. Then the evenly mixed powder is placed in a muffle furnace and calcined at 850°C for 4 hours to obtain a nano-scale lithium ion sieve precursor nano-Li2TiO3.
[0070] Preparation of micron-sized lithium ion sieve precursor micro-Li2TiO3:
[0071] Weigh equal amounts of polyvinyl chloride (PVC), polyvinyl butyral (PVB) and polyvinylidene fluoride (PVDF) as composite binders, and control the mass ratio of the composite binder to the nanoscale lithium ion sieve precursor Li2TiO3 to be 15:85. Weigh dimethylacetamide (DMAc) as the organic solvent of the composite binder, and control the mass ratio of DMAc to the nanoscale lithium ion sieve precursor Li2TiO3 to be 2:1. Stir polyvinyl chloride (PVC), polyvinyl butyral (PVB), polyvinylidene fluoride (PVDF), nanoscale lithium ion sieve precursor Li2TiO3 and dimethylacetamide (DMAc) at 60°C until they are uniformly mixed to obtain a mixed slurry. Weigh 5 times the mass of DMAc in deionized water, and then add the deionized water to the mixed slurry under high-speed stirring, control the flow rate of the deionized water so that all the deionized water is added to the mixed slurry within 1 hour, and then continue stirring for another 1 hour. After stopping stirring, the mixture is filtered, and the obtained filter cake is micron-grade lithium ion sieve precursor micro-Li2TiO3.
[0072] Preparation of micron-sized lithium ion sieve micro-H2TiO3: Measure hydrochloric acid with a concentration of 0.2 mol / L, the molar ratio of micro-Li2TiO3 to HCl is 1:5, place the micron-sized lithium ion sieve precursor micro-Li2TiO3 in the hydrochloric acid, stir for 10 hours to ensure that the materials are evenly mixed, filter the mixture, and the resulting filter cake is the micron-sized lithium ion sieve micro-H2TiO3.
[0073] The specific surface area and pore volume of the obtained lithium ion sieve were measured.
[0074] Table 5 BET characterization of nano-Li2TiO3 and micro-H2TiO3
[0075]
[0076] The particle size of the obtained lithium ion sieve was measured.
[0077] Table 6 BET characterization of nano-Li2TiO3 and micro-H2TiO3
[0078]
[0079] SEM photos of nano-Li2TiO3, a precursor of nano-lithium ion sieve, and micro-H2TiO3, a micron-lithium ion sieve, are shown in Figure 2. Figure 2 shown.
[0080] Similarly, using the example 1 and Figure 3The system shown in the figure is verified, the difference is that the cell body is filled with micron-sized lithium ion sieve micro-H2TiO3 with a loading amount of 200g / L based on the total solvent in the cell body. The hydrochloric acid storage tank 3 is loaded with 0.2mol / L dilute hydrochloric acid. During operation, when the lithium ion concentration of the produced water is monitored to be 80% of the lithium ion concentration of the water inlet pipe of the salt lake brine storage tank 9, it is considered that the adsorption of the micron-sized lithium ion sieve micro-H2TiO3 has reached saturation.
[0081] The brine from a salt lake in Tibet was tested as an experiment to detect the influent concentration and produced water concentration of each component in the brine, as shown in Table 7.
[0082] Table 7 Analysis of component concentrations during lithium extraction
[0083]
[0084] The experimental results show that the system can achieve the selective extraction of lithium ions from brine, with a lithium extraction rate of up to 96.2%. In addition, the titanium element was analyzed for the produced water after the membrane filaments were filtered, and it was found that there was no titanium element in the produced water, proving that there was no dissolved titanium element in the produced water, and there were no powder particles that could pass through the membrane filaments, that is, no powder loss.
Claims
1. A salt lake lithium extraction system using a micron-grade lithium ion sieve micro-H2TiO3, the system comprising a tank body (1), a hydrochloric acid storage tank (3), a salt lake brine storage tank (9), a hollow fiber ultrafiltration membrane (11) and a drive motor (12), the drive motor (12) being connected to the hollow fiber ultrafiltration membrane (11) and driving the hollow fiber ultrafiltration membrane (11) to reciprocate, an aeration device (2) being arranged at the bottom of the tank body (1), the hydrochloric acid storage tank (3) and the salt lake brine storage tank (9) being connected to the bottom of the tank body (1) via pipelines, characterized in that The cell body (1) is filled with micron-grade lithium ion sieve micro-H2TiO3, the concentration of the micron-grade lithium ion sieve micro-H2TiO3 is 100g / L-200g / L based on the total volume of the cell body, and the particle size is 0.5-50μm, and the hydrochloric acid storage tank (3) is filled with 0.1-0.4mol / L dilute hydrochloric acid as an eluent; The preparation method of the micron-sized lithium ion sieve micro-H2TiO3 comprises the following steps: (1) Preparation of nano-Li2TiO3, a lithium ion sieve precursor Take anatase titanium dioxide and lithium carbonate powder in a molar ratio of 1:1.1-1.5, mix them thoroughly by mechanical stirring, then place the evenly mixed powder in a muffle furnace, and roast it at a temperature of 700-900°C for 3-8h to obtain nano-scale lithium ion sieve precursor nano-Li2TiO3; (2) Preparation of micron-sized lithium ion sieve precursor nano-Li2TiO3 Polyvinyl chloride, polyvinyl butyral, and polyvinylidene fluoride are used as composite binders, the mass of the composite binder is 5% to 15% of the total mass of the composite binder and the nanoscale lithium ion sieve precursor Li2TiO3, dimethylacetamide is used as an organic solvent for the composite binder, and the mass ratio of dimethylacetamide to the nanoscale lithium ion sieve precursor Li2TiO3 is 1.5 to 2:1; Fully stir polyvinyl chloride, polyvinyl butyral, polyvinylidene fluoride, nano-scale lithium ion sieve precursor Li2TiO3 and dimethylacetamide at 50-80°C to obtain a mixed slurry, then add deionized water with a mass 4-8 times that of dimethylacetamide to the mixed slurry under high-speed stirring, and filter the slurry after full stirring to obtain a filter cake of micron-scale lithium ion sieve precursor micro-Li2TiO3; (3) Preparation of micron-sized lithium ion sieve precursor nano-H2TiO3 The micron-sized lithium ion sieve precursor micro-Li2TiO3 obtained in step (2) is placed in 0.1-0.4 mol / L hydrochloric acid, so that the molar ratio of micro-Li2TiO3 to HCl is 1:3-5. After sufficient stirring, the slurry is filtered and the filter cake obtained is the micron-sized lithium ion sieve micro-H2TiO3.
2. The salt lake lithium extraction system according to claim 1, characterized in that The mechanical stirring time of step (1) is 1-2h.
3. The salt lake lithium extraction system according to claim 1, characterized in that In step (2), the composite binder is polyvinyl chloride, polyvinyl butyral and polyvinylidene fluoride in a weight ratio of 1:1-2:1-3.
4. The salt lake lithium extraction system according to claim 1, characterized in that In step (2), polyvinyl chloride, polyvinyl butyral, polyvinylidene fluoride, nano-scale lithium ion sieve precursor Li2TiO3 and dimethylacetamide are stirred at 50-80°C for 5-10 hours to obtain a mixed slurry.
5. The salt lake lithium extraction system according to claim 1, characterized in that In step (2), deionized water is added to the mixed slurry at a constant flow rate within 1-3 hours.
6. The salt lake lithium extraction system according to claim 1, characterized in that The stirring time of step (3) is 10-20 hours.
7. The salt lake lithium extraction system according to claim 1, characterized in that The system operates as follows: (1) Adsorption stage Adsorption begins: lithium-containing salt lake brine enters a pool (1) equipped with a micron-grade lithium ion sieve micro-H2TiO3 from a salt lake brine storage tank (9), with a hydraulic retention time of 1-5 BV / h. The aeration device (2) is turned on to make the volume ratio of aeration volume to membrane fiber water production volume 20:1-35:
1. When the water level of the pool (1) reaches 80%-90% of the pool height, the drive motor (12) is started to make the hollow fiber ultrafiltration membrane (11) reciprocate, and the reciprocating motion frequency is 0.5-5 Hz. The hollow fiber ultrafiltration membrane (11) is negatively pressured by the ultrafiltration membrane negative pressure suction device to obtain ultrafiltration membrane water production. At this time, the water inlet flow rate from the salt lake brine storage tank (9) to the pool (1) is equal to the water production flow rate of the ultrafiltration membrane; Stop adsorption: monitor the lithium ion concentration in the water produced by the ultrafiltration membrane. When the lithium ion concentration of the produced water is 50%-80% of the lithium ion concentration of the water inlet pipe of the salt lake brine storage tank (9), it is considered that the adsorption of the micron-grade lithium ion sieve micro-H2TiO3 has reached saturation. At this time, stop the water inlet from the salt lake brine storage tank (9) to the pool body (1), stop the ultrafiltration membrane negative pressure suction device to stop the hollow fiber ultrafiltration membrane (11) from producing water, stop aeration, stop the reciprocating motion of the hollow fiber ultrafiltration membrane (11), and after natural sedimentation for 5-10 minutes, open the ultrafiltration membrane negative pressure suction device to suck the brine in the pool body (1) through the hollow fiber ultrafiltration membrane (11). When the water level of the pool body (1) drops to 20%-30% of the pool height, stop the ultrafiltration membrane negative pressure suction device; (2) Elution stage The dilute hydrochloric acid tank of the hydrochloric acid storage tank (3) is introduced into the pool body (1), and the ultrafiltration membrane negative pressure suction device is started. The hydraulic retention time is 1-3 BV / h. The pH value of the ultrafiltration membrane produced water is monitored. When the pH value is the same as the pH value of the dilute hydrochloric acid in the hydrochloric acid storage tank (3), the introduction of the eluent is stopped, and the ultrafiltration membrane negative pressure suction device is started to cause the hollow fiber ultrafiltration membrane (11) to begin negative pressure suction. When the water level of the pool body (1) drops to 20%-30% of the pool height, the negative pressure suction device is stopped. At this time, the elution stage ends and the adsorption stage is re-entered.