Solar cell and method for preparing the same
By simplifying the process flow in N-type monocrystalline IBC solar cells and forming boron-doped polysilicon layers and phosphorus-doped polysilicon layers through boron diffusion, the issues of manufacturing complexity and high cost are solved, and efficient solar cell preparation and performance are achieved. promote.
Patent Information
- Application Number
- CN202211479670.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-24
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-11-24
AI Technical Summary
The manufacturing process of N-type monocrystalline IBC solar cells is complex, the technical threshold is high, and the manufacturing cost is high, which limits its mass production application.
By sequentially forming a first silicon oxide layer, an intrinsic amorphous silicon layer, a phosphosilicate glass layer and a second silicon oxide layer on the back of the n-type silicon substrate, and removing the phosphosilicate glass layer and the second silicon oxide layer in some areas, the process is performed. Boron is diffused to form a boron-doped polysilicon layer and a phosphorus-doped polysilicon layer, and isolation trenches are formed at their junctions to simplify the process and reduce costs.
It simplifies the solar cell preparation process, reduces production costs, improves passivation performance, and increases the open circuit voltage of solar cells.
Smart Images

Figure CN115692548B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solar cells, and in particular to a solar cell and a preparation method thereof. Background Art
[0002] N-type single crystal IBC (Interdigitated back contact) solar cells usually use a diffusion process to form a heavily doped emitter and back field region on the back of the silicon wafer, which can effectively solve the problem of light blocking by metal grid lines and can significantly increase the short-circuit current density.
[0003] Compared with traditional crystalline silicon solar cells, N-type single crystal IBC solar cells have the following advantages in actual outdoor photovoltaic power stations and system applications: 1. High photoelectric conversion efficiency; 2. No light-induced degradation (LID) and high stability; 3. Good weak light response and low temperature coefficient; 4. Beautiful components, no grid line blocking the front, more beautiful appearance than traditional components, can be widely used in photovoltaic building integration; 5. Long service life.
[0004] However, the manufacturing process of N-type single crystal IBC solar cells is relatively complex, with high technical barriers and high manufacturing costs, which are important factors restricting the mass production of N-type single crystal IBC solar cells. Therefore, how to simplify the preparation process of N-type single crystal IBC solar cells and reduce the manufacturing cost is an important research direction in this field. Summary of the invention
[0005] Based on this, it is necessary to provide a solar cell and a preparation method thereof with a relatively simple preparation process and a low production cost.
[0006] According to one aspect of the present invention, there is provided a method for preparing a solar cell, comprising the following steps:
[0007] forming a first silicon oxide layer, an intrinsic amorphous silicon layer, a phosphosilicate glass layer and a second silicon oxide layer in sequence on the back side of the n-type silicon substrate;
[0008] Removing the phosphosilicate glass layer and the second silicon oxide layer from a portion of the back side of the n-type silicon substrate;
[0009] Performing boron diffusion on the back side of the n-type silicon substrate so that the intrinsic amorphous silicon layer in the region where the phosphosilicate glass layer and the second silicon oxide layer are removed is converted into a boron-doped polysilicon layer, and the intrinsic amorphous silicon layer in the region where the phosphosilicate glass layer and the second silicon oxide layer are not removed is converted into a phosphorus-doped polysilicon layer;
[0010] forming an isolation groove at the junction of the boron-doped polysilicon layer and the phosphorus-doped polysilicon layer;
[0011] A first electrode connected to the boron-doped polysilicon layer and a second electrode connected to the phosphorus-doped polysilicon layer are prepared.
[0012] In some embodiments, the boron diffusion is performed on the back side of the n-type silicon substrate, comprising the following steps:
[0013] The back side of the n-type silicon substrate is subjected to diffusion treatment using a boron source at a temperature of 900° C. to 1050° C. for 1 h to 3 h.
[0014] In some embodiments, the boron source is one or more of BCl3 or BBr3.
[0015] In some embodiments, the volume proportion of the boron source in the boron diffusion atmosphere is 5% to 30%.
[0016] In some embodiments, removing the phosphosilicate glass layer and the second silicon oxide layer from a portion of the back side of the n-type silicon substrate comprises the following steps:
[0017] forming a patterned blocking layer in a partial area of the surface of the second silicon oxide layer;
[0018] Using a solution containing HF to remove the phosphosilicate glass layer and the second silicon oxide layer in the area on the back side of the n-type silicon substrate where the patterned barrier layer is not formed;
[0019] The patterned blocking layer is removed.
[0020] In some embodiments, the patterned barrier layer is a waxy resin material.
[0021] In some embodiments, the patterned barrier layer is removed using an alkaline solution containing hydrogen peroxide.
[0022] In some embodiments, forming an isolation trench at the interface between the boron-doped polysilicon layer and the phosphorus-doped polysilicon layer comprises the following steps:
[0023] Laser grooves are formed at the interface between the boron-doped polysilicon layer and the phosphorus-doped polysilicon layer, and the laser grooves are etched with an alkaline solution.
[0024] In some of the embodiments, after forming the isolation trench and before preparing the first electrode and the second electrode, the preparation method further includes a step of removing a wrap-around coating on the front surface of the n-type silicon substrate.
[0025] In some of the embodiments, after forming the isolation trench and before removing the wrap-around plating layer on the front side of the n-type silicon substrate, the preparation method further includes the step of forming a third silicon oxide layer in the isolation trench.
[0026] In some of the embodiments, after removing the coating on the front side of the n-type silicon substrate and before preparing the first electrode and the second electrode, the preparation method further includes the steps of texturing the front side of the n-type silicon substrate and cleaning the n-type silicon substrate with a mixed solution of hydrofluoric acid and hydrochloric acid.
[0027] In some embodiments, after cleaning the n-type silicon substrate and before preparing the first electrode and the second electrode, the preparation method further includes the following steps:
[0028] forming an aluminum oxide layer on the front and back sides of the n-type silicon substrate;
[0029] forming a passivation anti-reflection layer on the aluminum oxide layer on the front and back sides of the n-type silicon substrate;
[0030] A hole is opened in the passivation anti-reflection layer on the back side of the n-type silicon substrate to form a first electrode contact hole connected to the boron-doped polysilicon layer and a second electrode contact hole connected to the phosphorus-doped polysilicon layer.
[0031] In some embodiments, the first electrode is prepared in the first electrode contact hole by screen printing; and the second electrode is prepared in the second electrode contact hole by screen printing.
[0032] According to another aspect of the present invention, a solar cell is provided. The solar cell is prepared by the above-mentioned method for preparing a solar cell of the present invention.
[0033] According to another aspect of the present invention, there is provided a solar cell, the solar cell comprising:
[0034] n-type silicon substrate;
[0035] A first silicon oxide layer is provided on the back side of the n-type silicon substrate;
[0036] a boron-doped polysilicon layer, disposed on the first silicon oxide layer;
[0037] a phosphorus-doped polysilicon layer, disposed on the first silicon oxide layer and separated from the boron-doped polysilicon layer by an isolation trench;
[0038] an aluminum oxide layer, disposed on the front surface of the n-type silicon substrate, on the boron-doped polysilicon layer, on the phosphorus-doped polysilicon layer and in the isolation trench;
[0039] A passivation anti-reflection layer is disposed on the aluminum oxide layer;
[0040] A first electrode, passing through the passivation anti-reflection layer and the aluminum oxide layer on the back side of the n-type silicon substrate and connected to the boron-doped polysilicon layer;
[0041] The second electrode is connected to the phosphorus-doped polysilicon layer through the passivation anti-reflection layer and the aluminum oxide layer on the back side of the n-type silicon substrate.
[0042] Compared with the prior art, the present invention has the following beneficial effects:
[0043] The boron-doped polysilicon layer and the phosphorus-doped polysilicon layer are formed in one step on the back of the n-type silicon substrate by removing the phosphorus-silicon glass layer and the second silicon oxide layer in a partial area of the back of the n-type silicon substrate and then performing boron diffusion. The preparation method can simultaneously prepare the boron-doped polysilicon layer and the phosphorus-doped polysilicon layer through only one high-temperature process (boron diffusion), greatly simplifying the preparation process of solar cells and reducing production costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 is a schematic diagram of an n-type silicon substrate;
[0045] Figure 2 It is a schematic diagram after forming a first silicon oxide layer, an intrinsic amorphous silicon layer, a phosphosilicate glass layer and a second silicon oxide layer on the back side of an n-type silicon substrate;
[0046] Figure 3 is a schematic diagram after a patterned barrier layer is formed on a partial area of the second silicon oxide layer;
[0047] Figure 4 is a schematic diagram after the phosphosilicate glass layer and the second silicon oxide layer in the area where no barrier layer is provided are removed;
[0048] Figure 5 is a schematic diagram after removing the patterned barrier layer;
[0049] Figure 6 Schematic diagram after boron diffusion;
[0050] Figure 7 A schematic diagram of the laser grooving to form an isolation groove;
[0051] Figure 8 It is a schematic diagram after chain acid polishing treatment;
[0052] Fig. 9 This is a schematic diagram after velveting and cleaning;
[0053] Fig.10 is a schematic diagram after an aluminum oxide layer is formed on the front and back sides of an n-type silicon substrate;
[0054] Fig.11 is a schematic diagram after a passivation anti-reflection layer is formed on the front and back sides of an n-type silicon substrate;
[0055] Fig.12It is a schematic diagram after a hole is opened in the passivation anti-reflection layer on the back side of the n-type silicon substrate;
[0056] Fig.13 FIG. 4 is a schematic diagram of a solar cell according to an embodiment of the present invention.
[0057] Description of reference numerals:
[0058] 1. n-type silicon substrate; 2. first silicon oxide layer; 3. intrinsic amorphous silicon layer; 4. phosphosilicate glass layer; 5. second silicon oxide layer; 6. patterned barrier layer; 7. boron-doped polysilicon layer; 8. borosilicate glass; 9. phosphorus-doped polysilicon layer; 10. isolation groove; 11. winding coating; 12. aluminum oxide layer; 13. passivation anti-reflection layer; 14. first electrode; 15. second electrode; 100. solar cell. DETAILED DESCRIPTION
[0059] In order to make the above-mentioned purpose, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.
[0060] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.
[0061] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0062] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0063] See also Figures 1 to 13 An embodiment of the present invention provides a method for preparing a solar cell 100, the method comprising the following steps S1 to S14:
[0064] Step S1: Provide an n-type silicon substrate 1, and use an alkaline solution to remove damage to the n-type silicon substrate 1, and then perform a cleaning process. The structure of the n-type silicon substrate 1 is as follows: Figure 1 shown.
[0065] In some embodiments, the n-type silicon substrate 1 is subjected to a damage removal treatment using a sodium hydroxide solution to remove a damaged layer on the surface of the n-type silicon substrate 1 after mechanical processing; and then the surface of the n-type silicon substrate 1 is cleaned by water washing.
[0066] Step S2: On the back side of the n-type silicon substrate 1 ( Figure 1 The first silicon oxide layer 2, the intrinsic amorphous silicon layer 3, the phosphosilicate glass layer 4 and the second silicon oxide layer 5 are sequentially formed on the lower surface of the n-type silicon substrate 1. The structure after forming the first silicon oxide layer 2, the intrinsic amorphous silicon layer 3, the phosphosilicate glass layer 4 and the second silicon oxide layer 5 is as shown in FIG. Figure 2 shown.
[0067] In some embodiments, LPCVD (Low Pressure Chemical Vapor Deposition) or PECVD (Plasma Enhanced Chemical Vapor Deposition) is used to first deposit a first silicon oxide layer 2 on the back side of the n-type silicon substrate 1, and then deposit an intrinsic amorphous silicon layer 3 on the first silicon oxide layer 2. The first silicon oxide layer 2 has a thickness of 1 nm to 2 nm, and the intrinsic amorphous silicon layer 3 has a thickness of 50 nm to 500 nm.
[0068] In some embodiments, APCVD (Atmospheric Pressure Chemical Vapor Deposition) is used to sequentially deposit a phosphosilicate glass layer 4 (PSG) and a second silicon oxide layer 5 on the intrinsic amorphous silicon layer 3. The thickness of the phosphosilicate glass layer 4 is 30nm to 100nm, and the mass ratio of phosphorus (P) in the phosphosilicate glass layer 4 is less than or equal to 50%; the thickness of the second silicon oxide layer 5 is 30nm to 100nm.
[0069] Step S3: forming a patterned barrier layer 6 in a partial area on the surface of the second silicon oxide layer 5. The structure after forming the patterned barrier layer 6 is as follows: Figure 3 shown.
[0070] In some embodiments, the barrier layer slurry is graphically printed on a partial area of the surface of the second silicon oxide layer 5 according to a preset pattern and dried to form the above-mentioned patterned barrier layer 6. The barrier layer slurry has the following characteristics: the formed barrier layer can be dissolved in alkali but insoluble in acid.
[0071] In some embodiments, the patterned barrier layer 6 is a wax-like resin material.
[0072] In some of the embodiments, the printed line spacing of the patterned barrier layer 6 formed after printing is 500 μm to 2000 μm.
[0073] Step S4: using a solution containing HF (hydrofluoric acid) to remove the phosphosilicate glass layer 4 and the second silicon oxide layer 5 in the area where the patterned barrier layer 6 is not formed on the back side of the n-type silicon substrate 1. The structure after removing the phosphosilicate glass layer 4 and the second silicon oxide layer 5 in the area where the barrier layer is not provided is as follows: Figure 4 shown.
[0074] In some embodiments, a hydrofluoric acid solution is used to remove the phosphosilicate glass layer 4 and the second silicon oxide layer 5 in the region where the patterned barrier layer 6 is not formed, and the first silicon oxide layer 2 is retained. In the region where the patterned barrier layer 6 is provided on the back side of the n-type silicon substrate 1, the phosphosilicate glass layer 4 and the second silicon oxide layer 5 on the inner side thereof will not be removed due to the presence of the patterned barrier layer 6.
[0075] Step S5: removing the patterned barrier layer 6. The structure after removing the patterned barrier layer 6 is as follows: Figure 5 shown.
[0076] In some embodiments, a mixed solution of sodium hydroxide and hydrogen peroxide (H2O2) is used to remove the patterned barrier layer 6, and after removing the patterned barrier layer 6, the n-type silicon substrate 1 is cleaned with a mixed solution of hydrochloric acid (HCl) and H2O2.
[0077] It can be understood that after the patterned barrier layer 6 is removed, the phosphosilicate glass layer 4 and the second silicon oxide layer 5 are retained at corresponding positions of the patterned barrier layer 6 .
[0078] It should be noted that the purpose of the above steps S3, S4 and S5 is to form a stacked structure having a phosphorus silicon glass layer 4 and a second silicon oxide layer 5 in a partial area on the back of the n-type silicon substrate 1, while only the first silicon oxide layer 2 and the intrinsic amorphous silicon layer 3 are formed in other areas on the back of the n-type silicon substrate 1. Steps S3 to S5 are achieved by setting a patterned barrier layer 6 as a mask layer. It is understandable that other methods can be used to achieve the above purpose in some other embodiments of the present invention, as long as a stacked structure having a phosphorus silicon glass layer 4 and a second silicon oxide layer 5 can be formed in a partial area on the back of the n-type silicon substrate 1.
[0079] Step S6: Boron diffusion is performed on the back side of the n-type silicon substrate 1. The structure after the boron diffusion is as follows: Figure 6 shown.
[0080] During the high-temperature treatment of boron diffusion, the intrinsic amorphous silicon layer 3 in the area where the phosphosilicate glass layer 4 and the second silicon oxide layer 5 are removed from the back of the n-type silicon substrate 1 can be converted into a boron-doped polysilicon layer 7, the outer layer of which will diffuse to form borosilicate glass 8 (BSG); while the intrinsic amorphous silicon layer 3 in the area where the phosphosilicate glass layer 4 and the second silicon oxide layer 5 are not removed from the back of the n-type silicon substrate 1 (i.e., the corresponding area where the patterned barrier layer 6 is set), due to the high temperature, the phosphorus in the phosphosilicate glass layer 4 is diffused into the intrinsic amorphous silicon layer 3, and crystallized and annealed to form a phosphorus-doped polysilicon layer 9. Since the second silicon oxide layer 5 is blocked on the outside of this area, boron will not be doped into the intrinsic amorphous silicon layer 3 in this area. In this way, the preparation of the boron-doped polysilicon layer 7 and the phosphorus-doped polysilicon layer 9 can be achieved simultaneously through a one-step high-temperature process (boron diffusion), which greatly simplifies the preparation process of the solar cell 100 and reduces the production cost of the solar cell 100.
[0081] The region corresponding to the boron-doped polysilicon layer 7 is the p-region, and the region corresponding to the phosphorus-doped polysilicon layer 9 is the n-region.
[0082] In some embodiments, the n-type silicon substrate 1 is placed in a boron diffusion furnace, and a boron source (boron trichloride (BCl3) and / or boron tribromide (BBr3)) is used to perform a boron diffusion treatment at a temperature of 900°C to 1050°C for 1h to 3h, and the volume ratio of the boron source in the boron diffusion atmosphere in the boron diffusion furnace is 5% to 30%. It can be understood that the temperature of the boron diffusion can be but not limited to 900°C, 920°C, 950°C, 980°C, 1000°C, 1020°C, 1050°C, etc.; the time of the boron diffusion can be but not limited to 1h, 1.5h, 2h, 2.5h, 3h, etc.; the volume ratio of the boron source in the boron diffusion atmosphere can be but not limited to 5%, 8%, 10%, 12%, 15%, 18%, 20%, 22%, 25%, 28%, 30%, etc.
[0083] Step S7: Use laser to perform laser grooving on the region at the junction of the boron-doped polysilicon layer 7 and the phosphorus-doped polysilicon layer 9, and then perform etching with an alkaline solution to form an isolation groove 10. The structure after laser grooving to form the isolation groove 10 is as follows: Figure 7 shown.
[0084] In some of the embodiments, a laser is used to perform laser grooving on the boundary area between the boron-doped polysilicon layer 7 and the phosphorus-doped polysilicon layer 9 to remove the polysilicon layer at the grooving location, and then an alkaline solution (such as a sodium hydroxide solution) is used to etch the grooving location to separate the boron-doped polysilicon layer 7 and the phosphorus-doped polysilicon layer 9 so that they are not directly connected to each other.
[0085] Step S8: removing the coating layer 11 on the front side of the n-type silicon substrate 1.
[0086] In some of the embodiments, a chain acid polishing (HF+HNO3) device is used to remove the silicon oxide layer, phosphosilicate glass, polysilicon layer, borosilicate glass and other winding layers 11 that are wound on the front side of the n-type silicon substrate 1. By using the chain acid polishing (HF+HNO3) device, the silicon oxide layer, phosphosilicate glass, polysilicon layer and borosilicate glass that are wound on the front side can be removed all at once, thereby avoiding leakage and appearance problems of the solar cell 100 caused by incomplete removal of the winding layer 11. While removing the front winding layer 11, the phosphosilicate glass layer 4, the second silicon oxide layer 5 and the borosilicate glass 8 on the back side of the n-type silicon substrate 1 are also removed. The schematic diagram after the chain acid polishing treatment is shown in FIG. Figure 8 shown.
[0087] In some of the embodiments, before removing the winding coating 11 on the front side of the n-type silicon substrate 1, APCVD is used to deposit a silicon oxide film in the isolation groove 10, and then the n-type silicon substrate 1 is placed in a chain acid polishing device to remove the winding coating 11. In this way, the silicon oxide film can protect the isolation groove 10 area on the back side of the n-type silicon substrate 1 from being textured in the subsequent texture process, maintain the surface morphology, reduce the carrier recombination in this area, and thus improve the overall passivation performance of the back side of the n-type silicon substrate 1.
[0088] Step S9: The front side of the n-type silicon substrate 1 is textured and cleaned. The structure after the texture and cleaning is as follows: Fig. 9 shown.
[0089] In some embodiments, the n-type silicon substrate 1 is sent to a tank cleaning machine, and sodium hydroxide is used to texturize the front side of the n-type silicon substrate 1. The back side of the n-type silicon substrate 1 will not be etched by the alkaline solution (texturizing solution) due to the protection of phosphosilicate glass and borosilicate glass. After the texturizing is completed, a mixed solution of HF and HCl (hydrochloric acid) is used for cleaning.
[0090] Step S10: forming an aluminum oxide layer 12 on the front and back sides of the n-type silicon substrate 1. The structure after forming the aluminum oxide layer 12 is as follows: Fig.10 shown.
[0091] In some embodiments, ALD (Atomic Layer Deposition) is used to form aluminum oxide layers 12 on the front and back sides of the n-type silicon substrate 1. The thickness of the aluminum oxide layers 12 on the front and back sides of the n-type silicon substrate 1 is 3 nm to 10 nm respectively.
[0092] Step S11: forming a passivation anti-reflection layer 13 on the aluminum oxide layer 12 on the front and back sides of the n-type silicon substrate 1. The structure after forming the passivation anti-reflection layer 13 is as follows: Fig.11 shown.
[0093] In some of the embodiments, a passivation anti-reflection layer 13 is first deposited on the aluminum oxide layer 12 on the front side of the n-type silicon substrate 1 by PECVD, and the thickness of the passivation anti-reflection layer 13 on the front side is 60nm-100nm; then a passivation anti-reflection layer 13 is deposited on the aluminum oxide layer 12 on the back side of the n-type silicon substrate 1 by PECVD, and the thickness of the passivation anti-reflection layer 13 on the back side is 80nm-150nm.
[0094] Step S12: Opening a hole in the passivation anti-reflection layer 13 on the back side of the n-type silicon substrate 1. The structure after opening the hole is as follows: Fig.12 shown.
[0095] In some embodiments, a laser is used to open a hole in the passivation anti-reflection layer 13 on the back side of the n-type silicon substrate 1, and a first electrode contact hole connected to the boron-doped polysilicon layer 7 and a second electrode contact hole connected to the phosphorus-doped polysilicon layer 9 are formed. In this way, electrodes connected to the boron-doped polysilicon layer 7 and the phosphorus-doped polysilicon layer 9 can be prepared in the first electrode contact hole and the second electrode contact hole, respectively.
[0096] Step S13: Prepare the first electrode 14 and the second electrode 15 in the first electrode contact hole and the second electrode contact hole respectively. The structure of the obtained solar cell 100 is as follows: Fig.13 shown.
[0097] In some embodiments, a first electrode 14 is prepared in a first electrode contact hole by screen printing, and the first electrode 14 is connected to the boron-doped polysilicon layer 7; a second electrode 15 is prepared in a second electrode contact hole by screen printing, and the second electrode 15 is connected to the phosphorus-doped polysilicon layer 9.
[0098] Step S14: light injection.
[0099] Light injection equipment is used to inject light into the prepared solar cell 100 .
[0100] In general, the method for preparing the solar cell 100 of the present invention forms a boron-doped polysilicon layer 7 and a phosphorus-doped polysilicon layer 9 in one step on the back side of the n-type silicon substrate 1 by removing the phosphosilicate glass layer 4 and the second silicon oxide layer 5 in a partial area of the back side of the n-type silicon substrate 1 and then performing boron diffusion. The preparation method can simultaneously prepare the boron-doped polysilicon layer 7 and the phosphorus-doped polysilicon layer 9 through only one high-temperature process (boron diffusion), which greatly simplifies the preparation process of the solar cell 100 and reduces the production cost.
[0101] In addition, by forming a patterned barrier layer 6 in a partial area on the surface of the second silicon oxide layer 5, the back side of the n-type silicon substrate 1 is patterned, so that the phosphosilicate glass layer 4 and the second silicon oxide layer 5 in a partial area on the back side of the n-type silicon substrate 1 can be easily removed, and the phosphosilicate glass layer 4 and the second silicon oxide layer 5 in a partial area are retained. The preparation method of the solar cell 100 of the present invention forms a first silicon oxide layer 2 and a boron-doped polysilicon layer 7 in the p-region on the back side of the n-type silicon substrate 1, and forms a first silicon oxide layer 1 and a phosphorus-doped polysilicon layer 9 in the n-region, which greatly improves the passivation performance of the solar cell 100, thereby facilitating the improvement of the open circuit voltage (Voc) of the solar cell 100.
[0102] See also Fig.13In one embodiment of the present invention, a back-contact solar cell 100 is provided. The solar cell 100 includes an n-type silicon substrate 1, a first silicon oxide layer 2, a boron-doped polysilicon layer 7, a phosphorus-doped polysilicon layer 9, an aluminum oxide layer 12, a passivation anti-reflection layer 13, a first electrode 14 and a second electrode 15.
[0103] Among them, the first silicon oxide layer 2 is arranged on the back side of the n-type silicon substrate 1; the boron-doped polysilicon layer 7 is arranged on the first silicon oxide layer 2; the phosphorus-doped polysilicon layer 9 is arranged on the first silicon oxide layer 2, and is separated from the boron-doped polysilicon layer 7 by the isolation groove 10; an aluminum oxide layer 12 is arranged on the front side of the n-type silicon substrate 1, on the boron-doped polysilicon layer 7, on the phosphorus-doped polysilicon layer 9 and in the isolation groove 10; a passivation anti-reflection layer 13 is arranged on each aluminum oxide layer 12; a first electrode 14 passes through the passivation anti-reflection layer 13 and the aluminum oxide layer 12 on the back side of the n-type silicon substrate 1, and is connected to the boron-doped polysilicon layer 7; a second electrode 15 passes through the passivation anti-reflection layer 13 and the aluminum oxide layer 12 on the back side of the n-type silicon substrate 1, and is connected to the phosphorus-doped polysilicon layer 9.
[0104] In some embodiments, the passivation anti-reflection layer 13 is a silicon nitride layer, and the first electrode 14 and the second electrode 15 are metal gate electrodes.
[0105] The present invention will be further described below in conjunction with specific embodiments and comparative examples, but they should not be construed as limiting the scope of protection of the present invention.
[0106] Embodiment 1:
[0107] A preparation process of an n-type full back electrode solar cell 100 comprises the following steps:
[0108] Providing an n-type silicon substrate 1, and performing a damage removal treatment and cleaning on the n-type silicon substrate 1 using a sodium hydroxide (NaOH) alkaline solution;
[0109] A first silicon oxide layer 2 with a thickness of 1 nm and an intrinsic amorphous silicon layer 3 with a thickness of 200 nm are sequentially deposited on the back side of an n-type silicon substrate 1 by LPCVD;
[0110] A phosphosilicate glass layer 4 (PSG) and a second silicon oxide layer 5 are sequentially deposited on the intrinsic amorphous silicon layer 3 by APCVD; wherein the thickness of the phosphosilicate glass layer 4 is 50 nm, the mass proportion of phosphorus (P) in the phosphosilicate glass layer 4 is 30%, and the thickness of the second silicon oxide layer 5 is 50 nm;
[0111] A corrosion-resistant slurry is printed on a partial area of the second silicon oxide layer 5 on the back of the n-type silicon substrate 1, and dried to form a patterned barrier layer 6; the corrosion-resistant slurry is a waxy resin material, and the characteristics of the corrosion-resistant slurry are that it is acid-resistant but not alkali-resistant; the printed line spacing of the patterned barrier layer 6 is 1200 μm;
[0112] The phosphosilicate glass layer 4 and the second silicon oxide layer 5 in the region where the patterned barrier layer 6 is not formed are removed by using an HF solution, and then the patterned barrier layer 6 is removed by using a mixed solution of NaOH and H2O2, and then cleaned by using a mixed solution of HCl and H2O2;
[0113] The n-type silicon substrate 1 is placed in a boron diffusion furnace, and BCl3 is used as a boron source (the volume proportion of the boron source in the atmosphere is 20%), and the back side of the n-type silicon substrate 1 is subjected to boron diffusion at 980°C for 2 hours to form p-type B-doped polysilicon (i.e., boron-doped polysilicon layer 7), and BSG (borosilicate glass) is diffused in the outer layer of the boron-doped polysilicon layer 7; and the area where the phosphosilicate glass layer 4 and the second silicon oxide layer 5 are retained, due to the high temperature, the phosphorus in the phosphosilicate glass layer 4 is pushed into the intrinsic amorphous silicon layer 3 to form n-type P-doped polysilicon (i.e., phosphorus-doped polysilicon layer 9), and in this area, due to the blocking of the outer second silicon oxide layer 5, boron will not be doped into the intrinsic amorphous silicon layer 3;
[0114] A laser is used to ablate the interface between the p-region (i.e., the region with the boron-doped polysilicon layer 7) and the n-region (i.e., the region with the phosphorus-doped polysilicon layer 9), and then the interface is etched in a NaOH solution to form an isolation groove 10 that separates the boron-doped polysilicon layer 7 from the phosphorus-doped polysilicon layer 9;
[0115] A chain acid polishing (HF+HNO3) device is used to remove silicon oxide, phosphosilicate glass, polysilicon and borosilicate glass coated on the front side of the n-type silicon substrate 1, and then the n-type silicon substrate 1 is texturized on the front side using NaOH in a tank cleaning machine. The back side will not be etched by alkali due to the protection of the phosphosilicate glass layer 4 and the borosilicate glass layer, and finally cleaned with a mixed solution of HF and HCl;
[0116] An aluminum oxide layer 12 (AlOx) is prepared on the front and back sides of the n-type silicon substrate 1 by ALD, and the thickness of the aluminum oxide layer 12 is 5 nm;
[0117] A silicon nitride (SiNx) passivation anti-reflection layer 13 is prepared on the front and back sides of the n-type silicon substrate 1 by using a tubular PECVD method; wherein the thickness of the passivation anti-reflection layer 13 on the front side of the n-type silicon substrate 1 is 75 nm, and the thickness of the passivation anti-reflection layer 13 on the back side of the n-type silicon substrate 1 is 100 nm;
[0118] A hole is opened on the passivation anti-reflection layer 13 on the back side of the n-type silicon substrate 1 by using a laser to form a first electrode contact hole connected to the boron-doped polysilicon layer 7 and a second electrode contact hole connected to the phosphorus-doped polysilicon layer 9 respectively;
[0119] A first electrode 14 is formed at the first electrode contact hole, and a second electrode 15 is formed at the second electrode contact hole by screen printing; the first electrode 14 is connected to the boron-doped polysilicon layer 7, and the second electrode 15 is connected to the phosphorus-doped polysilicon layer 9;
[0120] Light is injected into the prepared solar cell 100 to obtain an n-type full back electrode solar cell 100 .
[0121] Embodiment 2:
[0122] The preparation method of the solar cell 100 of this embodiment is basically the same as that of the embodiment 1, except that: this embodiment adopts the PECVD method to sequentially form the first silicon oxide layer 2 and the intrinsic amorphous silicon layer 3 on the back side of the n-type silicon substrate 1. By adopting the above preparation method, the winding coating 11 on the front side of the n-type silicon substrate 1 is less and easier to remove, which is beneficial to improving the appearance and yield of the solar cell 100.
[0123] Embodiment 3:
[0124] The preparation method of the solar cell 100 of this embodiment is basically the same as that of Example 1, with the only difference being that in this embodiment, the mass proportion of phosphorus (P) in the phosphosilicate glass layer 4 deposited on the intrinsic amorphous silicon layer 3 by APCVD is reduced from 30% in Example 1 to 20% in this embodiment.
[0125] That is, the doping concentration of the n-region of the solar cell 100 prepared in this embodiment is reduced, the concentration of phosphorus in the phosphorus-doped polysilicon layer 9 is reduced, and the carrier recombination in the n-region is reduced, thereby improving the passivation performance of the n-region.
[0126] Embodiment 4:
[0127] The preparation method of the solar cell 100 of this embodiment is basically the same as that of Example 1, with the only difference being that in this embodiment, after forming the isolation trench 10, an APCVD method is used to deposit a third silicon oxide layer in the isolation trench 10, and the thickness of the third silicon oxide layer is 50nm to 200nm; and then the chain acid polishing, winding plating and texturing are performed in step 8.
[0128] The preparation method of this embodiment, by depositing a third silicon oxide layer in the isolation groove 10, can protect the laser grooved area on the back side of the n-type silicon substrate 1 from being textured, maintain the morphology of the polished surface on the back side of the n-type silicon substrate, reduce the carrier recombination in this area, and thus improve the overall passivation performance of the back side of the n-type silicon substrate 1.
[0129] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0130] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the attached claims, and the description and drawings can be used to interpret the content of the claims.
Claims
1. A method for preparing a solar cell, characterized in that: The steps include: forming a first silicon oxide layer, an intrinsic amorphous silicon layer, a phosphosilicate glass layer and a second silicon oxide layer in sequence on the back side of the n-type silicon substrate; forming a patterned blocking layer in a partial area of the surface of the second silicon oxide layer; removing the phosphosilicate glass layer and the second silicon oxide layer in the area on the back side of the n-type silicon substrate where the patterned barrier layer is not formed; removing the patterned blocking layer; Performing boron diffusion on the back side of the n-type silicon substrate so that the intrinsic amorphous silicon layer in the region where the phosphosilicate glass layer and the second silicon oxide layer are removed is converted into a boron-doped polysilicon layer, and the intrinsic amorphous silicon layer in the region where the phosphosilicate glass layer and the second silicon oxide layer are not removed is converted into a phosphorus-doped polysilicon layer; forming an isolation groove at the junction of the boron-doped polysilicon layer and the phosphorus-doped polysilicon layer; A first electrode connected to the boron-doped polysilicon layer and a second electrode connected to the phosphorus-doped polysilicon layer are prepared.
2. The method for preparing a solar cell according to claim 1, characterized in that: Boron diffusion is performed on the back side of the n-type silicon substrate, comprising the following steps: The back side of the n-type silicon substrate is diffused by using a boron source at a temperature of 900°C to 1050°C for 1 h to 3 h.
3. The method for preparing a solar cell according to claim 2, characterized in that: The boron source is one or more of BCl3 or BBr3.
4. The method for preparing a solar cell according to claim 2, characterized in that: The volume proportion of the boron source in the boron diffusion atmosphere is 5% to 30%.
5. The method for preparing a solar cell according to claim 1, characterized in that: The phosphosilicate glass layer and the second silicon oxide layer in the area on the back side of the n-type silicon substrate where the patterned barrier layer is not formed are removed by using a solution containing HF.
6. The method for preparing a solar cell according to claim 1, characterized in that: The patterned barrier layer is a waxy resin material.
7. The method for preparing a solar cell according to claim 1, characterized in that: The patterned blocking layer is removed by using an alkaline solution containing hydrogen peroxide.
8. The method for preparing a solar cell according to claim 1, characterized in that: Forming an isolation trench at the junction of the boron-doped polysilicon layer and the phosphorus-doped polysilicon layer comprises the following steps: Laser grooves are formed at the interface between the boron-doped polysilicon layer and the phosphorus-doped polysilicon layer, and the laser grooves are etched with an alkaline solution.
9. The method for preparing a solar cell according to any one of claims 1 to 8, characterized in that: After forming the isolation groove and before preparing the first electrode and the second electrode, the preparation method further includes a step of removing the wrap-around coating on the front side of the n-type silicon substrate.
10. The method for preparing a solar cell according to claim 9, characterized in that: After forming the isolation groove and before removing the wrap-around plating layer on the front side of the n-type silicon substrate, the preparation method further includes the step of forming a third silicon oxide layer in the isolation groove.
11. The method for preparing a solar cell according to claim 9, characterized in that: After removing the coating on the front side of the n-type silicon substrate and before preparing the first electrode and the second electrode, the preparation method further includes the steps of texturing the front side of the n-type silicon substrate and cleaning the n-type silicon substrate with a mixed solution of hydrofluoric acid and hydrochloric acid.
12. The method for preparing a solar cell according to claim 11, characterized in that: After cleaning the n-type silicon substrate and before preparing the first electrode and the second electrode, the preparation method further includes the following steps: forming an aluminum oxide layer on the front and back sides of the n-type silicon substrate; forming a passivation anti-reflection layer on the aluminum oxide layer on the front and back sides of the n-type silicon substrate; A hole is opened in the passivation anti-reflection layer on the back side of the n-type silicon substrate to form a first electrode contact hole connected to the boron-doped polysilicon layer and a second electrode contact hole connected to the phosphorus-doped polysilicon layer.
13. The method for preparing a solar cell according to claim 12, characterized in that: The first electrode is prepared in the first electrode contact hole by screen printing; and the second electrode is prepared in the second electrode contact hole by screen printing.
14. A solar cell, characterized in that: The solar cell is prepared by the method for preparing a solar cell according to any one of claims 1 to 13.
15. The solar cell according to claim 14, characterized in that: include: n-type silicon substrate; A first silicon oxide layer is provided on the back side of the n-type silicon substrate; a boron-doped polysilicon layer, disposed on the first silicon oxide layer; a phosphorus-doped polysilicon layer, disposed on the first silicon oxide layer and separated from the boron-doped polysilicon layer by an isolation trench; an aluminum oxide layer, disposed on the front surface of the n-type silicon substrate, on the boron-doped polysilicon layer, on the phosphorus-doped polysilicon layer and in the isolation trench; A passivation anti-reflection layer is disposed on the aluminum oxide layer; A first electrode, passing through the passivation anti-reflection layer and the aluminum oxide layer on the back side of the n-type silicon substrate and connected to the boron-doped polysilicon layer; The second electrode is connected to the phosphorus-doped polysilicon layer through the passivation anti-reflection layer and the aluminum oxide layer on the back side of the n-type silicon substrate.