A method for preparing silicon-based negative electrode material for lithium-ion battery

By using a composite binder modified by sodium carboxymethyl cellulose and polyacrylamide, the problems of volume expansion and insufficient bonding force of silicon-based negative electrode materials are solved, and the battery performance and cycle life of lithium-ion batteries are significantly improved. Efficient battery performance improvement is achieved.

CN115763770BActive Publication Date: 2024-10-25KUNMING UNIV OF SCI & TECH
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202310000476.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-03
Publication Date
2024-10-25
Estimated Expiration
2043-01-03

AI Technical Summary

Technical Problem

The volume expansion of silicon-based negative electrode materials in lithium-ion batteries leads to powdering and SEI film rupture, which affects the specific capacity and cycle life of the battery. Existing binders such as PVDF and CMC have insufficient adhesion, and the organic solvents used are toxic. , polyacrylamide has poor dispersion.

Method used

A composite binder prepared by composite modification of sodium carboxymethylcellulose and polyacrylamide. The mass percentage of sodium carboxymethylcellulose is 30~50wt% and the mass percentage of polyacrylamide is 50~70wt%. Through magnetic force After stirring and grinding evenly, it is mixed with silicon powder and conductive carbon black to form a uniform slurry and coated to form a negative electrode piece.

Benefits of technology

It significantly improves the first Coulombic efficiency and cycle life of lithium-ion batteries, enhances the rate performance, suppresses the volume expansion and powdering of silicon particles, and the process is simple and easy to produce on a large scale.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 230102185352
    Figure 230102185352
  • Figure 230102185357
    Figure 230102185357
  • Figure 230102185405
    Figure 230102185405
Patent Text Reader

Abstract

The present invention discloses a method for preparing a silicon-based negative electrode material for a lithium-ion battery, and belongs to the technical field of new energy materials. The method described in the present invention is to form a new binder for use as a silicon negative electrode material for a lithium-ion battery by reacting sodium carboxymethyl cellulose, an aqueous binder commonly used for silicon negative electrode materials for lithium-ion batteries, with polyacrylamide at room temperature. The composite modified binder contains a catechol structure that can form a double hydrogen bond with silicon. When silicon particles are present in the active substance, the adhesion of the active substance can be increased, and the volume change of the silicon-based negative electrode material can be better suppressed. At the same time, the adhesion of the active substance to the current collector is increased, so that the silicon-based negative electrode material is not easy to pulverize and fall off. The use of the composite binder in the present invention significantly increases the cycle stability of the lithium-ion battery, and also exhibits excellent rate performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention discloses a method for preparing a silicon-based negative electrode material for a lithium-ion battery, and belongs to the technical field of new energy materials. Background Art

[0002] With the rapid development of my country's automobile and electronics industries, environmental pollution has increased while the energy shortage crisis has gradually emerged. In order to solve these problems, the research on new energy is important and meaningful. Lithium-ion batteries have many advantages such as high specific capacity, excellent cycle effect, and no memory effect. Research on high-specific-capacity lithium-ion batteries plays a decisive role in the development of renewable energy and electric vehicles.

[0003] As one of the key components of lithium-ion batteries, negative electrode materials have a great impact on the specific capacity, rate performance, and cycle life of lithium-ion batteries. The theoretical specific capacity of silicon materials used as negative electrodes for lithium-ion batteries is as high as 4200mAh / g, which is more than ten times the specific capacity of commercial graphite. At the same time, silicon materials also have the advantages of low lithium insertion potential, abundant reserves, low cost, and environmental friendliness. However, after the silicon-based negative electrode material is fully embedded with lithium, the volume expansion is as high as 300%. The accumulated stress from multiple charge and discharge cycles will cause the silicon-based negative electrode material to pulverize. At the same time, the volume expansion will also cause the SEI film to rupture. The repeated generation of the SEI film will consume lithium ions, reduce the specific capacity of the battery, and shorten the cycle life. In order to limit the volume expansion of silicon-based negative electrode materials, the role of the binder is crucial.

[0004] Commonly used binders for lithium-ion batteries are polyvinylidene fluoride (PVDF) and sodium carboxymethyl cellulose (CMC). However, the organic solvent N-methylpyrrolidone (NMP) used in polyvinylidene fluoride is toxic. At the same time, the bonding force of PVDF and CMC is not strong enough, and they are not suitable for silicon-based negative electrode materials with large volume changes. Polyacrylamide (PAM) is a binder with strong bonding force, but its dispersibility is poor. When used as a silicon-based negative electrode material, it is easy to cause silicon particles to agglomerate. Based on the above-mentioned silicon embedded lithium volume expansion problem, relevant workers have done a lot of research, and many of them have modified sodium carboxymethyl cellulose as a binder, such as compounding sodium carboxymethyl cellulose with styrene-butadiene rubber.

[0005] The present invention is to compound and modify two binders, CMC and PAM, to produce a new binder. In this composite binder, CMC is for better dispersibility and PAM is for stronger adhesion. Therefore, in order to limit the volume expansion of silicon-based materials, the mass ratio of PAM is required to be higher than that of CMC. This composite binder is used as a silicon-based negative electrode material for lithium-ion batteries, which significantly improves the first coulomb efficiency and cycle life of the battery. Summary of the invention

[0006] The object of the present invention is to provide a method for preparing a silicon-based negative electrode material for a lithium ion battery, wherein the silicon-based negative electrode material for a lithium ion battery is prepared by using a modified composite binder, wherein the binder is prepared by composite modification of sodium carboxymethyl cellulose and polyacrylamide, wherein the mass percentage of sodium carboxymethyl cellulose in the binder is 30-50wt%, and the mass percentage of polyacrylamide is 50-70wt%.

[0007] The composite binder of the present invention is used as a silicon-based negative electrode material for lithium-ion batteries, which significantly improves the initial coulombic efficiency and cycle life of lithium-ion batteries.

[0008] As a further preferred embodiment of the present invention, the method for preparing the silicon-based negative electrode material for lithium-ion batteries of the present invention specifically comprises the following steps:

[0009] (1) Sodium carboxymethyl cellulose powder is placed in deionized water, sealed, and then magnetically stirred to obtain a sodium carboxymethyl cellulose solution.

[0010] (2) Weigh silicon powder as the active material and conductive carbon black as the conductive agent, put them into a mortar and grind them, drop sodium carboxymethyl cellulose solution into the ground powder, and grind them evenly.

[0011] (3) Add polyacrylamide particles to the uniformly ground slurry obtained in step (2), continue grinding and add an appropriate amount of deionized water to allow the two binders to react with each other until the slurry is uniformly ground and the polyacrylamide particles completely disappear.

[0012] (4) The ground slurry is coated onto the current collector by a coating machine and placed in a high-temperature drying oven for drying to form a negative electrode sheet for a lithium-ion battery.

[0013] Preferably, the sodium carboxymethyl cellulose described in the present invention is a cellulose derivative with a glucose polymerization degree of 100-2000, a relative molecular mass of 242.16, a stirring temperature of 20° C. to 80° C., and a stirring time of 2 to 8 hours.

[0014] Preferably, the polyacrylamide of the present invention is non-ionic and has a molecular weight between 2 million and 14 million.

[0015] Preferably, in step (2) of the present invention, the purity of the silicon powder is 100% and the particle size is 30 nm to 50 nm.

[0016] Preferably, the active material of the present invention accounts for 60wt% of the silicon-based negative electrode material of the lithium-ion battery, the conductive agent accounts for 20wt% of the silicon-based negative electrode material of the lithium-ion battery, and the binder accounts for 20wt% of the silicon-based negative electrode material of the lithium-ion battery.

[0017] Preferably, the slurry of the present invention is coated on the current collector to a thickness of 10 to 20 microns, and the obtained negative electrode plate is dried in a high-temperature drying oven at a temperature of 60 to 80° C. for a drying time of 12 to 24 hours.

[0018] Beneficial effects of the present invention:

[0019] The sodium carboxymethyl cellulose (CMC) and polyacrylamide (PAM) in the present invention are both relatively cheap and easy to obtain, and the preparation method of the composite binder is simple, easy to operate, and can be mass-produced.

[0020] The composite binder in the present invention can not only make silicon particles evenly dispersed and prevent agglomeration, but also effectively inhibit the volume expansion of silicon when lithium is inserted; it significantly improves the initial coulombic efficiency, rate performance and cycle life of lithium-ion batteries, and has great development prospects.

[0021] The composite modified binder of the present invention contains a catechol structure that can form a double hydrogen bond with silicon. When the active material exists in silicon particles, the adhesion of the active material can be increased, and the volume change of the silicon-based negative electrode material can be better suppressed. At the same time, the adhesion of the active material to the current collector is increased, making the silicon-based negative electrode material not easy to pulverize and fall off. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 1 is a charge and discharge cycle curve diagram of the lithium ion batteries in Example 1, Comparative Example 1, Comparative Example 2, and Comparative Example 3.

[0023] Figure 2 It is a charge and discharge rate curve diagram of the lithium ion battery in Example 1, Comparative Example 1, Comparative Example 2, and Comparative Example 3.

[0024] Figure 3 This is a test curve of the charge and discharge performance of the lithium-ion battery in Example 1.

[0025] Figure 4 This is a cyclic voltammetry test curve of the lithium ion battery in Example 1.

[0026] Figure 5 This is the electrochemical impedance diagram of the lithium ion battery in Example 1. DETAILED DESCRIPTION

[0027] The present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments, but the protection scope of the present invention is not limited to the contents described above.

[0028] In the embodiment of the present invention, 30nm silicon powder is mainly used as the active material, conductive carbon black is used as the conductive agent, and then different types of binders are used to make lithium ion battery negative electrode plates at a mass ratio of 6:2:2 to compare the electrochemical properties of lithium ion batteries with different binders, so as to highlight the advantages of the composite binder of the present invention. Specific examples are as follows.

[0029] Example 1

[0030] In this example, 50wt% sodium carboxymethyl cellulose (CMC) and 50wt% polyacrylamide (PAM) are compounded into a composite binder as a binder for lithium-ion battery silicon-based negative electrode materials. The specific steps for making lithium-ion battery silicon-based negative electrode plates are as follows:

[0031] (1) Weigh 0.05 g of sodium carboxymethyl cellulose powder on a balance and place it in a 10 ml beaker. Use a dropper to add 3 ml of deionized water to the beaker. Place a magnet in the beaker and cover with plastic wrap. Place the beaker on a magnetic stirrer at room temperature and stir for 2 h to allow the sodium carboxymethyl cellulose powder to completely dissolve in the deionized water.

[0032] (2) Weigh 0.3 g of 30 nm silicon powder and 0.1 g of conductive carbon black on a balance. Put them into a mortar and grind them for 20 min to mix them evenly.

[0033] (3) Using a dropper, drop the sodium carboxymethyl cellulose solution stirred in step (1) into the powder mixed evenly in step (2), and continue grinding for 20 minutes to grind the slurry evenly so that the silicon particles are evenly dispersed.

[0034] (4) Weigh 0.05 g of polyacrylamide particles on a balance and add them to the slurry ground evenly in step (3). Continue grinding for 20 min to allow the two different binders to react with each other. Use a dropper to add an appropriate amount of deionized water to make the slurry have a moderate viscosity (ready to be coated) and the polyacrylamide particles completely dissolved. Then, coat it on a coating machine.

[0035] (5) During coating, first stick the copper foil as the current collector on the coater and clean the surface with alcohol. Then adjust the scraper height to 10 μm and start coating so that the slurry thickness is 10 μm.

[0036] (6) After coating, the electrode is placed in a high-temperature drying oven at 80°C for 24 hours and then cut to make a negative electrode for a lithium-ion battery.

[0037] Example 2

[0038] In this example, 40wt% sodium carboxymethyl cellulose (CMC) and 60wt% polyacrylamide (PAM) are compounded into a composite binder as a binder for lithium-ion battery silicon-based negative electrode materials. The specific steps for making lithium-ion battery silicon-based negative electrode plates are as follows:

[0039] (1) Weigh 0.04 g of sodium carboxymethyl cellulose powder on a balance and place it in a 10 ml beaker. Use a dropper to add 2.5 ml of deionized water to the beaker. Place a magnetic bar in the beaker and cover with plastic wrap. Place the beaker on a magnetic stirrer at room temperature and stir for 2 h to allow the sodium carboxymethyl cellulose powder to completely dissolve in the deionized water.

[0040] (2) Weigh 0.3 g of 30 nm silicon powder and 0.1 g of conductive carbon black on a balance. Put them into a mortar and grind them for 20 min to mix them evenly.

[0041] (3) Using a dropper, drop the sodium carboxymethyl cellulose solution stirred in step (1) into the powder mixed evenly in step (2), and continue grinding for 20 minutes to grind the slurry evenly so that the silicon particles are evenly dispersed.

[0042] (4) Weigh 0.06 g of polyacrylamide particles on a balance and add them to the slurry that has been ground evenly in step (3). Continue grinding for 20 min to allow the two different binders to react with each other. Use a dropper to add an appropriate amount of deionized water to make the slurry have a moderate viscosity and the polyacrylamide particles completely dissolved. Then apply the slurry on a coating machine.

[0043] (5) During coating, first stick the copper foil as the current collector on the coater and clean the surface with alcohol. Then adjust the scraper height to 10 μm and start coating so that the slurry thickness is 10 μm.

[0044] (6) After coating, the electrode is placed in a high-temperature drying oven at 80°C for 24 hours and then cut to make a negative electrode for a lithium-ion battery.

[0045] Example 3

[0046] In this example, 30wt% sodium carboxymethyl cellulose (CMC) and 70wt% polyacrylamide (PAM) are compounded into a composite binder as a binder for lithium-ion battery silicon-based negative electrode materials. The specific steps for making lithium-ion battery silicon-based negative electrode plates are as follows:

[0047] (1) Weigh 0.03 g of sodium carboxymethyl cellulose powder on a balance and place it in a 10 ml beaker. Use a dropper to add 2 ml of deionized water to the beaker, put in a magnet, cover with plastic wrap, and place the beaker on a magnetic stirrer at room temperature for 2 h to allow the sodium carboxymethyl cellulose powder to completely dissolve in the deionized water.

[0048] (2) Weigh 0.3 g of 30 nm silicon powder and 0.1 g of conductive carbon black on a balance. Put them into a mortar and grind them for 20 min to mix them evenly.

[0049] (3) Using a dropper, drop the sodium carboxymethyl cellulose solution stirred in step (1) into the powder mixed evenly in step (2), and continue grinding for 20 minutes to grind the slurry evenly so that the silicon particles are evenly dispersed.

[0050] (4) Weigh 0.07 g of polyacrylamide particles on a balance and add them to the slurry that has been ground evenly in step (3). Continue grinding for 20 min to allow the two different binders to react with each other. Use a dropper to add an appropriate amount of deionized water to make the slurry have a moderate viscosity and the polyacrylamide particles completely dissolved. Then apply the slurry on a coating machine.

[0051] (5) During coating, first stick the copper foil as the current collector on the coater and clean the surface with alcohol. Then adjust the scraper height to 10 μm and start coating so that the slurry thickness is 10 μm.

[0052] (6) After coating, the electrode is placed in a high-temperature drying oven at 80°C for 24 hours and then cut to make a negative electrode for a lithium-ion battery.

[0053] Comparative Example 1

[0054] This example uses polyvinylidene fluoride (PVDF) as a binder for silicon-based negative electrode materials for lithium-ion batteries. The specific steps for making silicon-based negative electrode plates for lithium-ion batteries are as follows:

[0055] (1) Weigh 0.1 g of polyvinylidene fluoride (PVDF) powder on a balance and place it in a 10 ml beaker. Use a dropper to add 3 ml of N-methylpyrrolidone (NMP) as an organic solvent into the beaker. Place a magnetic bar in the beaker and cover with plastic wrap. Place the beaker on a magnetic stirrer and stir at 80 °C for 15 min to fully dissolve the polyvinylidene fluoride powder in the N-methylpyrrolidone organic solvent.

[0056] (2) Weigh 0.3 g of 30 nm silicon powder and 0.1 g of conductive carbon black on a balance. Put them into a mortar and grind them for 20 min to mix them evenly.

[0057] (3) Use a dropper to drip the solution stirred in step (1) into the powder mixed evenly in step (2), and continue grinding for 20 minutes. You can drip appropriate amount of N-methylpyrrolidone to grind the slurry evenly so that the silicon particles are evenly dispersed and the slurry has a moderate viscosity, and then apply it on a coater.

[0058] (4) During coating, first stick the copper foil as the current collector on the coater and clean the surface with alcohol. Then adjust the scraper height to 10 μm and start coating so that the slurry thickness is 10 μm.

[0059] (5) After coating, the electrode is placed in a high-temperature drying oven at 80°C for 24 hours and then cut to make a negative electrode for a lithium-ion battery.

[0060] Comparative Example 2

[0061] This example uses sodium carboxymethyl cellulose (CMC) as a binder for silicon-based negative electrode materials for lithium-ion batteries. The specific steps for making silicon-based negative electrode sheets for lithium-ion batteries are as follows:

[0062] (1) Weigh 0.1 g of sodium carboxymethyl cellulose (CMC) powder on a balance and place it in a 10 ml beaker. Use a dropper to add 3 ml of deionized water as a solvent to the beaker. Place a magnetic bar in the beaker and cover with plastic wrap. Place the beaker on a magnetic stirrer and stir at room temperature for 2 h to allow the sodium carboxymethyl cellulose powder to fully dissolve in the deionized water.

[0063] (2) Weigh 0.3 g of 30 nm silicon powder and 0.1 g of conductive carbon black on a balance. Put them into a mortar and grind them for 20 min to mix them evenly.

[0064] (3) Use a dropper to drop the sodium carboxymethyl cellulose solution stirred in step (1) into the powder mixed evenly in step (2), and continue grinding for 20 minutes. Appropriate amount of deionized water can be dropped to grind the slurry evenly so that the silicon particles are evenly dispersed and the slurry has a moderate viscosity, and then apply it on a coater.

[0065] (4) During coating, first stick the copper foil as the current collector on the coater and clean the surface with alcohol. Then adjust the scraper height to 10 μm and start coating so that the slurry thickness is 10 μm.

[0066] (5) After coating, the electrode is placed in a high-temperature drying oven at 80°C for 24 hours and then cut to make a negative electrode for a lithium-ion battery.

[0067] Comparative Example 3

[0068] In this example, polyacrylamide (PAM) is used as a binder for silicon-based negative electrode materials for lithium-ion batteries. The specific steps for making silicon-based negative electrode sheets for lithium-ion batteries are as follows:

[0069] (1) Weigh 0.1 g of polyacrylamide (PAM) particles on a balance and place it in a 10 ml beaker. Use a dropper to add 3 ml of deionized water as a solvent to the beaker. Place a magnet in the beaker and cover with plastic wrap. Place the beaker on a magnetic stirrer and stir at room temperature for 2 h to allow the polyacrylamide particles to fully dissolve in the deionized water to form a viscous binder.

[0070] (2) Weigh 0.3 g of 30 nm silicon powder and 0.1 g of conductive carbon black on a balance. Put them into a mortar and grind them for 20 min to mix them evenly.

[0071] (3) Use a medicine spoon to add the polyacrylamide binder stirred in step (1) into the powder mixed evenly in step (2), and continue grinding for 20 minutes. You can drop appropriate amount of deionized water to grind the slurry evenly so that the silicon particles are evenly dispersed and the slurry has a moderate viscosity, and then apply it on the coater.

[0072] (4) During coating, first stick the copper foil as the current collector on the coater and clean the surface with alcohol. Then adjust the scraper height to 10 μm and start coating so that the slurry thickness is 10 μm.

[0073] (5) After coating, the electrode is placed in a high-temperature drying oven at 80°C for 24 hours and then cut to make a negative electrode for a lithium-ion battery.

[0074] The negative electrode plates of the lithium-ion batteries in the embodiment and the comparative embodiment are assembled into a battery; the CR2025 button battery is selected in the present invention, the battery separator is the celgard2500 separator, the electrolyte is 1 mol / L LiPF6 dissolved in a mixed solution of EC / DEC with a volume ratio of 1:1, and 10% FEC is added as an additive; after the battery is packaged, it is left to stand for 24 hours, and then the charge and discharge cycle test and the rate performance test are carried out on the battery test system.

[0075] Lithium-ion battery cycle performance test table

[0076]

[0077] From the lithium-ion battery cycle performance test table and Figure 1 It can be seen that the first discharge specific capacity, first coulomb efficiency and cycle stability of the lithium ion battery assembled by the composite binder in Example 1 are better than those of the lithium ion batteries assembled by the other three binders in Comparative Example 1, Comparative Example 2 and Comparative Example 3; Figure 2 It can be seen that the rate performance of the lithium-ion battery assembled using the composite binder in Example 1 is also stronger than that of the lithium-ion batteries assembled using the other three binders.

[0078] Figure 3 This is a test curve diagram of the charge and discharge performance of the lithium-ion battery in Example 1. From the diagram, it can be analyzed that the lithium-ion battery exhibits typical charge and discharge behavior of silicon materials.

[0079] Figure 4 This is a cyclic voltammetry test curve of the lithium ion battery in Example 1. The reaction mechanism of the lithium ion battery can be analyzed from the figure, indicating that it has good electrochemical performance.

[0080] Figure 5 This is the electrochemical impedance diagram of the lithium-ion battery in Example 1. It can be seen from the figure that the charge transfer impedance of the negative electrode of the lithium-ion battery is only 60Ω, which has good conductivity.

[0081] The composite binder in the present invention significantly increases the adhesion of silicon-based negative electrode materials for lithium-ion batteries, and can also make silicon particles evenly dispersed during the production of electrode plates, thereby increasing the initial coulombic efficiency and cycle stability of lithium-ion batteries, enhancing its rate performance, and having great development prospects.

Claims

1. A method for preparing a silicon-based negative electrode material for a lithium-ion battery, It is characterized in that The modified composite binder is used to prepare a lithium-ion battery silicon-based negative electrode material, wherein the binder is prepared by composite modification of sodium carboxymethyl cellulose and polyacrylamide, wherein the mass percentage of sodium carboxymethyl cellulose in the binder is 30-50wt%, and the mass percentage of polyacrylamide is 50-70wt%, and the specific steps include: (1) placing sodium carboxymethyl cellulose powder into deionized water, sealing the solution, and then performing magnetic stirring to obtain a sodium carboxymethyl cellulose solution; (2) Weigh silicon powder as the active material and conductive carbon black as the conductive agent, put the two into a mortar and grind them, drop sodium carboxymethyl cellulose solution into the ground powder, and grind them evenly; (3) Adding polyacrylamide particles to the uniformly ground slurry obtained in step (2), continuing to grind and adding an appropriate amount of deionized water to allow the two binders to react with each other until the slurry is uniformly ground and the polyacrylamide particles completely disappear; (4) The ground slurry is coated onto the current collector by a coating machine and placed in a high-temperature drying oven for drying to form a negative electrode sheet for a lithium-ion battery; The sodium carboxymethyl cellulose is a cellulose derivative with a glucose polymerization degree of 100-2000, a relative molecular mass of 242.16, a stirring temperature of 20°C to 80°C, and a stirring time of 2 to 8 hours; The polyacrylamide is non-ionic and has a molecular weight between 2 million and 14 million; In step (2), the purity of silicon powder is 100% and the particle size is 30nm~50nm; The active material described in step (3) accounts for 60wt% of the lithium-ion battery silicon-based negative electrode material, the conductive agent accounts for 20wt% of the lithium-ion battery silicon-based negative electrode material, and the binder accounts for 20wt% of the lithium-ion battery silicon-based negative electrode material; The thickness of the slurry coated on the current collector is 10-20 microns, and the obtained negative electrode plate is dried in a high-temperature drying oven at a temperature of 60-80°C for a drying time of 12-24 hours.

Citation Information

Patent Citations

  • Lithium ion battery negative electrode slurry and preparation method thereof

    CN109659552A

  • Novel battery pole piece enhancing method and corresponding pole piece

    CN110247023A

  • Cross-linking type aqueous binder for lithium ion battery and electrode prepared from cross-linking type aqueous binder

    CN111106352A

  • Modification method and application of silicon-based binder for negative electrode material of lithium ion battery

    CN112322223A

  • Negative plate, battery and preparation method

    CN114122323A