Infrared nonlinear optical crystal with diamond-like grid structure, preparation method and use thereof

By developing the infrared nonlinear optical crystal material ACd3Ga5S11 with a diamond-like grid structure, the problems of low laser damage threshold and two-photon absorption of existing infrared nonlinear optical crystal materials have been solved, and a balance between high laser damage threshold and strong frequency doubling response has been achieved. , which enhances the application value of the material.

CN115772705BActive Publication Date: 2024-10-01FUJIAN INST OF RES ON THE STRUCTURE OF MATTER CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111039955.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-09-06
Publication Date
2024-10-01
Estimated Expiration
2041-09-06

AI Technical Summary

Technical Problem

Existing infrared nonlinear optical crystal materials have defects in laser damage threshold and two-photon absorption, which limit their application prospects.

Method used

An infrared nonlinear optical crystal material ACd3Ga5S11 with a diamond-like grid structure was developed. It was prepared by a high-temperature solid-state method. The material has excellent second-order nonlinear optical properties and high laser damage threshold. The powder frequency doubling strength reaches 2 times that of the commercial material AgGaS2. -3 times.

Benefits of technology

It achieves phase matching in the infrared band, has a wide light transmission range and strong frequency doubling response, and the laser damage threshold is 35-40 times that of AgGaS2 crystal, significantly improving the application potential of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115772705B_ABST
    Figure CN115772705B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of inorganic nonlinear optical materials, and specifically discloses an infrared nonlinear optical crystal with a diamond-like grid structure, a preparation method and use thereof. The molecular formula of the optical crystal of the present invention is: ACd3Ga5S 11 ; Wherein, A is an alkali metal element, the alkali metal element is selected from K, Rb or Cs, and its crystal structure belongs to the orthorhombic system, and the space group is Pna21. The optical crystal of the present invention has excellent second-order nonlinear optical properties, can achieve phase matching in the infrared band, has a wide light transmittance range, and a strong infrared double frequency response. Its powder double frequency intensity can reach 2-3 times that of the commercial material AgGaS2, and its laser damage threshold is 35-40 times that of the AgGaS2 crystal. It has important application value in high-tech fields such as laser frequency conversion, near-infrared probes, and photorefractive information processing, especially for infrared detectors and infrared lasers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of inorganic nonlinear optical materials, and in particular relates to an infrared nonlinear optical crystal with a diamond-like grid structure, and a preparation method and application thereof. Background Art

[0002] Nonlinear optical crystals are a very important type of functional material, which are widely used in laser communications, optical information processing, integrated circuits and military technology. Generally speaking, an ideal nonlinear optical crystal must meet the following conditions: (1) a large second-order harmonic frequency coefficient; (2) a high laser damage threshold; (3) an appropriate birefringence; (4) a wide optical transmission range; (5) good physical, chemical and mechanical properties. Nonlinear optical materials can be divided into inorganic materials, organic materials, polymer materials and organometallic complex materials according to their physical and chemical properties. At present, the vast majority of nonlinear optical crystals on the market are inorganic materials. According to their different application bands, they can be divided into three categories: ultraviolet band, visible band and infrared band. Among them, nonlinear optical crystal materials in the ultraviolet and visible bands can already meet the requirements of practical applications.

[0003] The nonlinear optical crystal materials in the infrared band are mainly semiconductor materials with ABC2-type chalcopyrite structure, such as AgGaS2, AgGaSe2, ZnGeP2, etc. These compounds have large nonlinear optical coefficients and high mid- and far-infrared transmittance, but they also have serious disadvantages such as low laser damage threshold and two-photon absorption, which limits their application. Therefore, exploring new infrared nonlinear optical crystal materials with application prospects is a difficulty and hot spot in the current research field of nonlinear optical materials. Summary of the invention

[0004] The present invention aims to provide an infrared nonlinear optical crystal with a diamond-like grid structure, a preparation method and use thereof. The optical crystal material has excellent second-order nonlinear optical properties, can achieve phase matching in the infrared band, and its powder frequency doubling intensity can reach 2-3 times that of the commercial material AgGaS2, and its laser damage threshold is 35-40 times that of the AgGaS2 crystal, achieving a good balance between a large second-order frequency doubling coefficient and a high laser damage threshold.

[0005] The present invention provides the following technical solutions:

[0006] The present invention provides an optical crystal, wherein the molecular formula of the optical crystal is ACd3Ga5S 11 ; wherein A is an alkali metal element, and the alkali metal element is selected from K, Rb or Cs.

[0007] According to an embodiment of the present invention, the structure of the optical crystal belongs to the orthorhombic system, the space group is Pna21, and its unit cell parameters are α=β=γ=90°.

[0008] Exemplarily, the optical crystal is KCd3Ga5S 11 , the unit cell parameters are α=β=γ=90°.

[0009] Exemplarily, the optical crystal is RbCd3Ga5S 11 , the unit cell parameters are α=β=γ=90°.

[0010] Exemplarily, the optical crystal is CsCd3Ga5S 11 , the unit cell parameters are α=β=γ=90°.

[0011] According to an embodiment of the present invention, the optical crystal has a three-dimensional diamond-like grid structure, and the three-dimensional diamond-like grid structure is mainly composed of [Cd3S9] and [Ga5S 14 ] The hyperpolyhedron is used as the basic structural unit and is connected to each other through common vertices S; the alkali metal ions A are dispersed and filled in the three-dimensional diamond-like grid structure as a charge balance.

[0012] Preferably, the structure of the optical crystal is as follows Figure 1 shown.

[0013] According to an embodiment of the present invention, the optical crystal KCd3Ga5S 11 Basically Figure 2 X-ray crystal diffraction pattern shown in a.

[0014] According to an embodiment of the present invention, the optical crystal is an infrared nonlinear optical crystal.

[0015] According to an embodiment of the present invention, the powder frequency doubling intensity of the optical crystal is 2-3 times that of the commercial material AgGaS2 crystal.

[0016] According to an embodiment of the present invention, the laser damage threshold of the optical crystal is 35-40 times that of the commercial material AgGaS2 crystal.

[0017] The present invention also provides a method for preparing the above optical crystal, comprising the following steps: mixing raw materials uniformly, and preparing the optical crystal by a high-temperature solid phase method;

[0018] The raw materials include: alkali metal halide AX, gallium oxide (Ga2O3), single substance Cd, single substance S and single substance B.

[0019] According to an embodiment of the present invention, in the alkali metal halide AX, A is selected from K, Rb or Cs, and X is selected from Cl, Br or I.

[0020] According to an embodiment of the present invention, the molar ratio of AX, Ga2O3, Cd, S and B is (1-10):5:6:(20-25):10, preferably (2-5):5:6:(21-23):10; for example, the molar ratio can be 3:5:6:22:10, or AX:Ga2O3:Cd:S:B=4:5:6:23:10.

[0021] According to an embodiment of the present invention, the high temperature solid phase method specifically comprises: putting the raw materials into a sealed container and placing it in a heating device, heating up, keeping the high temperature, and cooling down to room temperature to obtain the optical crystal.

[0022] Preferably, the high temperature solid phase method is carried out under vacuum conditions. Further preferably, the sealed container has a vacuum environment, for example, the vacuum pressure is 10 -4 -10 -3 Pa.

[0023] Preferably, the sealed container is a sealed quartz reaction tube.

[0024] Preferably, the heating refers to heating to a holding temperature, and the holding temperature is selected from 800 to 1200°C, preferably 900 to 1100°C, such as 950-1050°C.

[0025] Preferably, the high temperature insulation time is not less than 50 hours, preferably 50-100 hours.

[0026] Exemplarily, the high temperature insulation refers to insulation at 950° C. for 120 hours, or insulation at 1000° C. for 100 hours.

[0027] Preferably, the cooling includes cooling to 400° C. and then naturally cooling to room temperature. Further preferably, the cooling is performed at a rate of no more than 2° C. / hour.

[0028] Preferably, the preparation method further comprises washing and drying the product obtained by naturally cooling to room temperature to obtain the optical crystal, for example, washing with water (such as deionized water) and drying with ethanol.

[0029] The present invention also provides an optical crystal prepared by the method.

[0030] The present invention also provides uses of the optical crystal, such as infrared detectors, infrared lasers, photorefractive information processing, etc.

[0031] The present invention also provides use of the optical crystal, for example, for laser frequency conversion.

[0032] The present invention also provides use of the optical crystal, for example, in a near-infrared probe.

[0033] The present invention also provides an infrared detector, which contains the optical crystal.

[0034] The invention also provides an infrared laser, which contains the optical crystal.

[0035] Beneficial effects of the present invention:

[0036] The present invention provides an infrared nonlinear optical crystal material with a diamond-like grid structure, which has excellent second-order nonlinear optical properties, namely, phase matching can be achieved in the infrared band, has a moderate birefringence, a wide light transmittance range, and a strong frequency doubling response. The frequency doubling intensity can reach 2-3 times that of the commercial material AgGaS2, and the laser damage threshold is 35-40 times that of the AgGaS2 crystal, thus achieving a good balance between a large second-order frequency doubling coefficient and a high laser damage threshold.

[0037] This infrared nonlinear optical crystal has important application value in high-tech fields such as laser frequency conversion, near-infrared probes, and photorefractive information processing, especially in infrared detectors and infrared lasers. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 ACd3Ga5S 11 Schematic diagram of the crystal structure.

[0039] Figure 2 The sample KCd3Ga5S prepared in Example 1 11 X-ray diffraction pattern of . DETAILED DESCRIPTION

[0040] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.

[0041] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.

[0042] Example 1

[0043] KI, Ga2O3, Cd, S and B were mixed in a molar ratio of 3:5:6:22:10 to obtain raw materials. The raw materials were placed in a quartz crucible, and the quartz crucible containing the raw materials was placed in a quartz reaction tube, and vacuum was drawn to 10 -3 Pa and melt the sealed quartz reaction tube with hydrogen-oxygen flame. Place the quartz reaction tube in a tube furnace with a temperature controller, heat it to 1000°C, and keep it warm for 100 hours. Then cool it to 400°C at a rate of no more than 2°C / hour, stop heating, and cool it naturally to room temperature. The product is washed with deionized water and dried with ethanol to obtain the infrared nonlinear optical crystal KCd3Ga5S 11 , recorded as sample 1.

[0044] Example 2

[0045] The difference between this embodiment and embodiment 1 is that KI is replaced with RbI, and the infrared nonlinear optical crystal RbCd3Ga5S is obtained according to the molar ratio of 4:5:6:24:10. 11 , recorded as sample 2.

[0046] Example 3

[0047] The difference between this embodiment and embodiment 1 is that KI is replaced with CsI, and the infrared nonlinear optical crystal CsCd3Ga5S is obtained according to the molar ratio of 4:5:6:23:10. 11 , recorded as sample 3.

[0048] Test Example 1

[0049] (1) Structural characterization of samples

[0050] The samples of Examples 1-3 were subjected to X-ray single crystal diffraction tests, under the following test conditions: on a Saturn 724 single crystal diffractometer, Mo target, Kα radiation source (λ=0.07107nm), and test temperature 293K. The samples were structurally analyzed by Shelx-2014. The crystallographic data results of the samples are shown in Table 1, and the crystal structure diagram is shown in Figure 1 shown.

[0051] Table 1 Sample ACd3Ga5S 11 Crystallographic data of (A=K,Rb,Cs)

[0052]

[0053] like Figure 1 As shown, the obtained crystal is mainly composed of [Cd3S9] and [Ga5S 14] Hyperpolyhedrons serve as basic structural units, which are interconnected through shared vertices S to form a three-dimensional diamond-like grid structure, and alkali metal ions A, which serve as charge balance, are dispersed and filled in the three-dimensional grid structure.

[0054] X-ray powder diffraction phase analysis (XRD) was performed on Sample 1. The test conditions were: on a Rigaku MiniFlex II X-ray diffractometer, Cu target, Kα radiation source (λ = 0.154184 nm). The powder XRD pattern of Sample 1 was fitted with the single crystal diffraction data as shown in the figure below: Figure 2 As shown. Figure 2 It can be seen that the XRD pattern of sample 1 is fitted with the XRD spectrum obtained by single crystal diffraction data. Figure 1 This indicates that the sample obtained in Example 1 has high crystallinity and purity.

[0055] (2) Characterization of optical properties of samples

[0056] The optical properties of samples 1-3 were tested under the following conditions: characterization on a Perkin-Elmer FT-IR infrared spectrometer and a Perkin-Elmer Lambda 950 UV-visible (near infrared) absorption or diffuse reflectance spectrometer. The light transmission properties, frequency doubling properties, laser damage threshold and optical band gap of samples 1-3 are shown in Table 2.

[0057] Table 2 Optical properties of samples

[0058]

[0059] The exemplary embodiments of the present invention are described above. However, the present invention is not limited to the above embodiments. Any modification, equivalent substitution, improvement, etc. made by those skilled in the art within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. An optical crystal, characterized in that: The molecular formula of the optical crystal is ACd3Ga5S 11 ; Wherein, A is an alkali metal element, and the alkali metal element is selected from K, Rb or Cs; The structure of the optical crystal belongs to the orthorhombic system, the space group is Pna21, and its unit cell parameters are α=β=γ=90°; The optical crystal has a three-dimensional diamond-like grid structure, and the three-dimensional diamond-like grid structure is mainly composed of [Cd3S9] and [Ga5S 14 ] Hyperpolyhedrons are used as basic structural units and are connected to each other through common vertices S; alkali metal ions A are dispersed and filled in the three-dimensional diamond-like grid structure as a charge balance.

2. The optical crystal according to claim 1, characterized in that: The optical crystal is KCd3Ga5S 11 , the unit cell parameters are α=β=γ=90°; Or, the optical crystal is RbCd3Ga5S 11 , the unit cell parameters are α=β=γ=90°; Or, the optical crystal is CsCd3Ga5S 11 , the unit cell parameters are α=β=γ=90°.

3. The optical crystal according to claim 1, characterized in that: The optical crystal is an infrared nonlinear optical crystal; The powder frequency-doubled intensity of the optical crystal is 2-3 times that of the commercial material AgGaS2 crystal; The laser damage threshold of the optical crystal is 35-40 times that of the commercial material AgGaS2 crystal.

4. The method for preparing an optical crystal according to any one of claims 1 to 3, characterized in that: The preparation method comprises the following steps: mixing the raw materials uniformly, and preparing the optical crystal by a high temperature solid phase method; The raw materials include: alkali metal halide AX, gallium oxide, single substance Cd, single substance S and single substance B; In the alkali metal halide AX, A is selected from K, Rb or Cs, and X is selected from Cl, Br or I; The molar ratio of AX, Ga2O3, Cd, S and B is (1-10):5:6:(20-25):

10.

5. The preparation method according to claim 4, characterized in that: The molar ratio of AX, Ga2O3, Cd, S and B is (2-5):5:6:(21-23):

10.

6. The preparation method according to claim 4, characterized in that: The high temperature solid phase method specifically comprises: putting the raw material into a sealed container and placing it in a heating device, heating it up, keeping it at a high temperature, and cooling it down to room temperature to obtain the optical crystal; The high temperature solid phase method is carried out under vacuum conditions; the closed container has a vacuum environment, and the vacuum pressure is 10 -4 -10 - 3 Pa; The sealed container is a sealed quartz reaction tube; The heating refers to heating to a holding temperature, wherein the holding temperature is selected from 800 to 1200° C.; The high temperature insulation time is not less than 50 hours; The cooling includes cooling to 400°C and then naturally cooling to room temperature; the cooling is performed at a rate not exceeding 2°C / hour; The preparation method further comprises washing and drying the product obtained by naturally cooling to room temperature to obtain the optical crystal.

7. The preparation method according to claim 6, characterized in that: The insulation temperature is 900-1100° C.; the high temperature insulation time is 50-100 hours.

8. Use of the optical crystal according to any one of claims 1 to 3 for infrared detectors, infrared lasers or photorefractive information processing.

9. Use of the optical crystal according to any one of claims 1 to 3 for laser frequency conversion.

10. Use of the optical crystal according to any one of claims 1 to 3 for near-infrared probes.

11. An infrared detector, characterized in that: The infrared detector comprises the optical crystal according to any one of claims 1 to 3.

12. An infrared laser, characterized in that: The infrared laser comprises the optical crystal according to any one of claims 1 to 3.