A low-noise, high-response Ga2O3-based avalanche photodiode and its preparation method
By preparing a Ga2O3 film with a multi-layer doped structure, using the MOCVD process and high-temperature oxygen annealing, the problem of low response of Ga2O3-based UV detectors is solved, a low-noise, high-response Ga2O3-based SAM-APD is achieved, and the process flow is simplified. And improve the signal-to-noise ratio of the device.
Patent Information
- Application Number
- CN202211630179.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-19
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-12-19
AI Technical Summary
The existing Ga2O3-based UV detectors have low responsivity and complex processes, making it difficult to prepare low-noise, high-response Ga2O3-based avalanche photodiodes (APD).
The Ga2O3 film using a multi-layer doped structure is prepared by the MOCVD process, using a p-type Si substrate and multi-layer Ga2O3 film epitaxy, combined with high-temperature oxygen annealing, to form a low-noise, high-response Ga2O3-based heterojunction separated absorption and multiplication region ( SAM) structure.
The responsivity of the Ga2O3 ultraviolet detector is improved, the noise is reduced, the signal-to-noise ratio is improved, the process flow is simplified, and the practical application of the device is promoted.
Smart Images

Figure CN115810694B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of semiconductor photoelectric detectors, and in particular relates to a low-noise, high-response Ga2O3-based avalanche photodiode (APD) and a preparation method thereof. Background Art
[0002] Gallium oxide (Ga2O3) is an emerging ultra-wide bandgap (UWBG) semiconductor material. With an ultra-wide bandgap of 4.2 to 4.9 eV, it basically covers the entire solar-blind ultraviolet band; its high breakdown electric field strength and high thermal stability make it an ideal material in the field of solar-blind ultraviolet detection. Current Ga2O3-based ultraviolet solar-blind detectors, such as photoconductive and PN junction types, have low responsivity and are difficult to apply in practice. Avalanche photodiodes (APDs) use the high electric field in the depletion region of the PN junction to achieve internal current gain, greatly improving the responsivity, which also makes APDs more sensitive to weaker ultraviolet signals. Another important parameter of APDs is noise. APDs often show stronger shot noise as the reverse bias increases, thereby reducing the signal-to-noise ratio of the device. This problem can be effectively solved by using a heterojunction separated absorption and multiplication region (SAM) structure. In SAM-APDs, narrow-bandgap and wide-bandgap semiconductors are used as absorption and multiplication regions, respectively, to reduce noise while reducing tunnel current and improving the signal-to-noise ratio of the device. At present, SAM-APD has been widely used in InGaAsP and AlGaN-based APDs.
[0003] However, for Ga2O3, which is UWBG and has not yet achieved p-type doping, the preparation of SAM-APD devices based on the heterojunction formed by n-Ga2O3 and other p-type materials (such as Si) becomes a feasible option. By adjusting the thickness and doping concentration of the Ga2O3 epitaxial layer, an electric field distribution similar to that of SAM-APD can be obtained in Ga2O3, achieving the effect of absorption and multiplication separation. This puts forward technical requirements for the preparation of Ga2O3 films and the regulation of electrical properties. Secondly, point defects and surface states in the heteroepitaxial growth of Ga2O3 films have a great influence on surface barriers and leakage currents, and the quality of the films also urgently needs to be improved. As the main means of industrializing epitaxial films, the MOCVD process has advantages in Ga2O3 film epitaxy and property regulation. Based on the above problems, the present invention proposes a low-noise, high-response Ga2O3-based SAM-APD and a preparation method thereof. Summary of the invention
[0004] The purpose of the present invention is to provide a Ga2O3-based SAM-APD with a multi-layer doping structure, low noise and high response and a preparation method thereof through a MOCVD process.
[0005] The present invention adopts heavily doped p-type Si as substrate and utilizes the current mature MOCVD process to firstly epitaxially grow a low-thickness n-Ga2O3 film on the upper surface of the p-Si substrate as a multiplication layer; then epitaxially grow a high-thickness UID-Ga2O3 film (unintentionally doped Ga2O3 film) on the low-thickness n-Ga2O3 film as a light absorption layer; then epitaxially grow a layer of heavily doped n-Ga2O3 on the high-thickness UID-Ga2O3 film. + -Ga2O3 ohmic contact layer; after the epitaxy is completed, in-situ annealing is performed in an oxygen atmosphere to reduce the defect density, and finally ohmic contact electrodes are deposited on the lower surface of the Si substrate and the ohmic contact layer, respectively, so as to prepare the device described in the present invention. The present invention obtains a Reed diode-like electric field distribution through multiple layers of Ga2O3 films with different doping concentrations, and the direction of the electric field is from the Ga2O3 layer to the Si substrate, thereby realizing a SAM structure. At the same time, the advantages of low cost, high thermal conductivity and easy p-type doping of the p-type Si substrate are utilized, and point defects in the film are reduced by thermal annealing, thereby proposing a Ga2O3-based SAM-APD with a multi-layer doping structure, low noise and high response.
[0006] The low-noise, high-response Ga2O3-based avalanche photodiode of the present invention comprises, in sequence, a p-Si substrate 1, a low-thickness n-Ga2O3 film 2 epitaxially grown on the substrate 1, a high-thickness UID-Ga2O3 film 3 epitaxially grown on the low-thickness n-Ga2O3 film 2, and an n-Ga2O3 film epitaxially grown on the UID-Ga2O3 film 3. + -Ga2O3 ohmic contact layer 4, ohmic contact electrode 5 deposited on the lower surface of Si substrate and ohmic contact layer (such as Figure 1 shown).
[0007] The method for preparing a low-noise, high-response Ga2O3-based SAM-APD described in the present invention comprises the following steps:
[0008] A. Substrate 1 is a p-Si substrate obtained by the CZ method, with a thickness of 430-450 μm and a hole concentration of 1×10 19 cm -3 ~1×10 20 cm -3 , ultrasonically clean with toluene, acetone, ethanol, and deionized water for 5 to 10 minutes in sequence before use;
[0009] B. Low-thickness n-Ga2O3 film 2 is epitaxially grown on the p-Si substrate in step A using MOCVD process. The reaction sources are trimethylgallium and high-purity oxygen, the n-type dopant is silane (SiH4), the epitaxial temperature is 750-900°C, the pressure is 30-40 mbar, the epitaxial time is 10-12 min, the film thickness is 100-120 nm, and the electron concentration is 1×1018 cm -3 ~1×10 19 cm -3 .
[0010] C. The high-thickness UID-Ga2O3 film 3 is epitaxially grown on the low-thickness n-Ga2O3 film 2 using the MOCVD process. The reaction sources are trimethylgallium (TMGa) and high-purity oxygen. The epitaxial temperature is 750-900°C, the pressure is 30-40 mbar, the epitaxial time is 30-40 min, the film thickness is 300-400 nm, and the electron concentration is 1×10 15 cm -3 ~1×10 17 cm -3 ;
[0011] D、n + The -Ga2O3 ohmic contact layer 4 is epitaxially grown on the high-thickness UID-Ga2O3 film 3 using the MOCVD process; the reaction sources are trimethylgallium and high-purity oxygen, the n-type dopant is silane (SiH4), the epitaxial temperature is 750-900°C, the pressure is 30-40mbar, the epitaxial time is 2-3min, and the thickness is 20-30nm; after the epitaxy is completed, the temperature is raised to 900-950°C, and high-temperature oxygen annealing is continued in the MOCVD reaction chamber, the annealing time is 0.8-1.2 hours, and the oxygen flow rate is 400-500sccm; finally, it is cooled to room temperature; the electron concentration is 1×10 19 cm -3 ~1×10 20 cm -3 .
[0012] E. In step D, an Au electrode with a thickness of 300 to 400 nm is evaporated on the lower surface of the p-Si substrate 1 of the device; + -The upper surface of the Ga2O3 ohmic contact layer 4 is evaporated by hard mask electron beam to form a Ti electrode with a thickness of 20 to 30 nm and an Au electrode with a thickness of 50 to 100 nm, respectively, to form a Ti / Au composite electrode; then annealed at 450 to 550°C for 2 to 5 minutes in a nitrogen atmosphere to form a good ohmic contact electrode 5, thereby preparing the low-noise, high-response Ga2O3-based SAM-APD described in the present invention.
[0013] Effects and benefits of the present invention:
[0014] The present invention solves the problem of low response of current Ga2O3 ultraviolet detectors and overcomes the problems of low current density and complex process of current horizontal structure Ga2O3 ultraviolet detectors; the present invention proposes a preparation method of a Ga2O3-based SAM-APD with low noise and high response, which can effectively improve the responsiveness of Ga2O3 ultraviolet detectors and promote their practical application. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 : Schematic diagram of the device structure prepared by the present invention;
[0016] Figure 2 In Example 1, the Si substrate is composed of a low-thickness n-Ga2O3 film 2, a high-thickness UID-Ga2O3 film 3, and an n + -Ga2O3 ohmic contact layer 4, the horizontal axis is the 2Theta angle, and the vertical axis is the diffraction line intensity. The test results show that under the condition of large lattice mismatch and thermal mismatch between Ga2O3 and Si, the prepared Ga2O3 film is polycrystalline, indicating that the film still has high crystal quality, which is beneficial to reduce device leakage current.
[0017] Figure 3 :The IV curve of the device in Example 1 under different UV power, the horizontal axis is the reverse bias voltage applied to the device, the vertical axis is the current of the device, Figure a and Figure b are linear and logarithmic coordinate IV curves respectively. The test results show that the device has a strong response to ultraviolet light, which is specifically manifested in the photocurrent increasing with the UV power and the continuously decreasing avalanche voltage. The current and avalanche voltage of the device under different UV power have a large difference, which has a high degree of differentiation. The device shows a dramatic current gain at the avalanche breakdown voltage, showing an obvious avalanche effect. The responsiveness and detection rate of the device can reach 1×10 4 A / W and 3×10 16 Jones. DETAILED DESCRIPTION
[0018] Embodiment 1:
[0019] A Ga2O3-based SAM-APD with low noise and high response, the structural diagram of which is shown in Figure 1 As shown, the structure is composed of a p-Si substrate 1, a low-thickness n-Ga2O3 film 2 epitaxially grown on the surface of the substrate 1, a high-thickness UID-Ga2O3 film 3 epitaxially grown on the low-thickness n-Ga2O3 film 2, and a high-thickness n-Ga2O3 film epitaxially grown on the UID-Ga2O3 film 3. + -Ga2O3 ohmic contact layer 4, and ohmic contact electrode 5 deposited on the lower surface of Si substrate and the ohmic contact layer.
[0020] The above-mentioned method for preparing a Ga2O3-based SAM-APD with low noise and high response has the following steps:
[0021] The substrate used for epitaxy is a high-quality p-Si single crystal prepared by the CZ method with a thickness of 440μm. First, the substrate is cleaned in toluene, acetone, ethanol and deionized water in an ultrasonic state for 5 minutes respectively, then the substrate is blown dry with high-purity nitrogen and placed in the reaction chamber. + -Ga2O3 ohmic contact layer 4 is obtained by MOCVD process epitaxy, the reaction sources are TMGa and high-purity oxygen, and silane (SiH4) is used as n-type dopant. During the entire epitaxy process, the electron concentration of the film is regulated by adjusting the SiH4 flow rate. The TMGa and high-purity oxygen flow rates are 15sccm and 600sccm, respectively, and the epitaxy temperature and pressure are 750℃ and 40mbar, respectively. During the epitaxy of low-thickness n-Ga2O3 film 2, the SiH4 flow rate is set to 15scmm to achieve a higher electron concentration (about 1×10 18 cm -3 ), the epitaxial growth time is 10min. When epitaxially growing high-thickness UID-Ga2O3 film 3, the SiH4 flow rate is set to 0scmm, and the epitaxial growth time is 30min. + -Ga2O3 ohmic contact layer 4 (electron concentration is 1×10 20 cm -3 ), the SiH4 flow rate was set to 20scmm, and the epitaxial time was set to 3min. After the epitaxy was completed, the reaction chamber temperature was raised to 900°C, and a high-temperature oxygen annealing treatment was performed for 1h in an oxygen atmosphere of 600scmm. Then the temperature was lowered to room temperature for sampling. In terms of device preparation, a 300nm Au electrode was first deposited on the lower surface of the p-Si substrate 1, and then a hard mask was used to deposit a 300nm Au electrode on the n-Si substrate 1. + -A circular Ti / Au composite electrode array is deposited on the Ga2O3 ohmic contact layer 4, with an electrode diameter of 1mm, a circle center spacing of 1.6mm, and a Ti / Au thickness of 20nm / 150nm respectively. Finally, an ohmic contact electrode 5 is formed by annealing at 500℃ in a nitrogen atmosphere, and a Ga2O3-based SAM-APD with low noise and high response designed by the present invention is obtained by laser cutting into independent devices. The effective area of each device is about 1.775mm 2 .
[0022] In order to study the effect of the preparation method on improving the crystal quality of Ga2O3 thin film, we used Ultima IV X-ray diffractometer to test the crystal quality of Ga2O3 thin film in this embodiment and conducted a light response test on the device. The results are as follows:
[0023] 1. Crystal quality analysis of samples in the examples
[0024] Figure 2 This is the XRD 2Theta diagram of the Ga2O3 film in Example 1. Under the condition that there is a large lattice mismatch and thermal mismatch between Ga2O3 and Si, the prepared Ga2O3 film exhibits a polycrystalline state, indicating that the film still has a high crystal quality.
[0025] 2. Photoresponse analysis of the device in the embodiment
[0026] Figure 3 The photoresponse IV curve of the device in Example 1 shows a strong response to ultraviolet light, which is manifested by an increasing photocurrent and a decreasing avalanche voltage as the light power increases. The device has a huge photocurrent gain after the avalanche, thus obtaining a gain of more than 1×10 4 A / W responsivity and 3×10 16 Jones's detection rate.
Claims
1. A method for preparing a low-noise, high-response Ga2O3-based SAM-APD, the steps of which are as follows: A. ultrasonically clean the p-Si substrate (1) with toluene, acetone, ethanol, and deionized water for 5 to 10 minutes, and then blow dry with high-purity nitrogen; B. epitaxially growing a low-thickness n-Ga2O3 thin film (2) on the surface of the p-Si substrate (1) in step A using a MOCVD process, wherein the reaction sources are trimethylgallium and high-purity oxygen, the n-type dopant is silane, the epitaxial temperature is 750-900° C., the pressure is 30-40 mar, and the epitaxial time is 10-12 min; C. epitaxially growing a thick UID-Ga2O3 film (3) on a thin n-Ga2O3 film (2) using a MOCVD process, wherein the reaction sources are trimethylgallium (TMGa) and high-purity oxygen, the epitaxial temperature is 750-900°C, the pressure is 30-40mar, and the epitaxial time is 30-40min; D. Using MOCVD process to grow n on high thickness UID-Ga2O3 film (3) + -Ga2O3 ohmic contact layer (4), the reaction sources are trimethylgallium and high-purity oxygen, the n-type dopant is silane, the epitaxial temperature is 750-900°C, the pressure is 30-40mar, and the epitaxial time is 2-3min; after the epitaxy is completed, the temperature is raised to 900-950°C, and high-temperature oxygen annealing is continued in the MOCVD reaction chamber, the annealing time is 0.8-1.2 hours, and the oxygen flow rate is 400-500sccm; finally, the temperature is lowered to room temperature; E. Evaporating Au electrode on the lower surface of the p-Si substrate (1) of the device obtained in step D; + A Ti / Au composite electrode is evaporated on the upper surface of the Ga2O3 ohmic contact layer (4) by hard mask electron beam; then annealed at 450-550°C for 2-5 minutes in a nitrogen atmosphere to form a good ohmic contact electrode (5), which is then cut into independent devices by laser to prepare a low-noise, high-response Ga2O3-based SAM-APD.
2. The method for preparing a low-noise, high-response Ga2O3-based SAM-APD according to claim 1, characterized in that: The thickness of the p-Si substrate (1) is 430-450 μm, and the hole concentration in the p-Si substrate (1) is 1×10 19 cm -3 ~1×10 20 cm -3 .
3. The method for preparing a low-noise, high-response Ga2O3-based SAM-APD according to claim 1, characterized in that: The thickness of the low-thickness n-Ga2O3 film (2) is 100-120 nm, and the electron concentration in the low-thickness n-Ga2O3 film (2) is 1×10 18 cm -3 ~1×10 19 cm -3 .
4. The method for preparing a low-noise, high-response Ga2O3-based SAM-APD according to claim 1, characterized in that: The thickness of the high-thickness UID-Ga2O3 film (3) is 300-400 nm, and the electron concentration in the high-thickness UID-Ga2O3 film (3) is 1×10 15 cm -3 ~1×10 17 cm -3 .
5. The method for preparing a low-noise, high-response Ga2O3-based SAM-APD according to claim 1, characterized in that: n + -Ga2O3 ohmic contact layer (4) has a thickness of 20 to 30 nm, n + -The electron concentration in the Ga2O3 ohmic contact layer (4) is 1×10 19 cm -3 ~1×10 20 cm -3 .
6. The method for preparing a low-noise, high-response Ga2O3-based SAM-APD according to claim 1, characterized in that: The thickness of the Au electrode on the lower surface of the p-Si substrate (1) is 300-400 nm. + - In the Ti / Au composite electrode on the upper surface of the Ga2O3 ohmic contact layer (4), the thickness of the Ti electrode is 20 to 30 nm, and the thickness of the Au electrode is 50 to 100 nm.
7. A low-noise, high-response Ga2O3-based SAM-APD, characterized by: The method is prepared by any one of claims 1 to 6.
Citation Information
Patent Citations
Gallium oxide MIS structured ultraviolet detector
CN109980040A
Self-assembled crystal / amorphous gallium oxide phase junction photoelectric detector and manufacturing method thereof
CN110350043A