A diaphragm, an electrical device including the diaphragm and a method for preparing the same

By applying an organic-inorganic hybrid composite compound coating to the rechargeable battery separator, the problem of multiple performance requirements of existing separators in the high-tech field is solved, and high energy density, mechanical strength and electrochemical reaction performance are improved. , suppressing the gas generation inside the battery.

CN115812263BActive Publication Date: 2024-10-22CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080102780.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-07-28
Filing Date
2020-09-25
Publication Date
2024-10-22
Estimated Expiration
2040-09-25

AI Technical Summary

Technical Problem

Existing rechargeable battery separators in high-tech fields are difficult to meet multiple performance requirements such as high energy density, low mass per unit area, high air permeability, high mechanical strength and wear resistance, and are difficult to effectively suppress gas generation inside the battery and improve electrochemistry. reaction performance.

Method used

A coating containing an organic-inorganic hybrid composite compound is used to form a polymer substrate layer with a mesoporous or microporous structure through periodic assembly of metal cations and ligands, thereby improving the energy density, mechanical strength and electrical properties of the separator. Chemical reaction properties and applied in batteries to improve performance.

Benefits of technology

It significantly improves the energy density, air permeability, mechanical strength and electrochemical reaction performance of the separator, extends the cycle life of the battery and suppresses the generation of gas inside the battery, meeting the stringent requirements of the high-tech field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115812263B_ABST
    Figure CN115812263B_ABST
Patent Text Reader

Abstract

A diaphragm, an electrical device comprising the diaphragm, and a method for preparing the same. The diaphragm has multiple improved properties due to a coating containing an organic-inorganic hybrid composite compound, wherein the organic-inorganic hybrid composite compound is formed by periodically assembling basic units shown in Formula I. Also provided are a battery (10) and an electrical device comprising the diaphragm, methods for preparing the same, and a method and use of the organic-inorganic hybrid composite compound for improving diaphragm performance. x (M a C b ) y ·A z Formula I.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Cross-references

[0002] This application claims priority to Chinese patent application No. 202010734845.9, entitled “A diaphragm, an electronic device including the diaphragm, and a method for preparing the same,” filed on July 28, 2020 by the same applicant, Contemporary Amperex Technology Co., Ltd., the entire text of which is incorporated into this application by reference. Technical Field

[0003] The present application relates to the field of electrical devices, and in particular to a diaphragm used in electrical devices, a battery and other electrical devices including the diaphragm, an electrical device including the battery and other electrical devices, and methods for manufacturing the same. Background Art

[0004] Electrical devices are widely used in all aspects of modern society. In many electrical devices, diaphragms are needed to achieve physical and electrical separation. Rechargeable batteries are the most well-known electrical devices that require diaphragms. The working principle of rechargeable batteries is to use reversible electrochemical reactions to achieve repeated charging and discharging. One or more diaphragms are often used inside to separate the anode side from the cathode side, providing selective permeation or blocking of substances of different types, sizes and charges in the system. For example, the diaphragm is insulated from electrons, physically isolating the positive and negative active materials of the secondary battery, preventing internal short circuits and forming an electric field in a certain direction, while allowing the ions in the battery to pass through the diaphragm and move between the positive and negative electrodes. With the development of related fields in recent years, rechargeable batteries have been increasingly used in high-tech, high-intensity, and high-demand fields such as new energy vehicles, aerospace, ships, and heavy machinery, and are even used as the main power and energy supply equipment in these fields. Compared with conventional rechargeable batteries used in small daily consumer products over the past few decades, these high-tech fields have put forward unprecedented stringent requirements for rechargeable batteries, many of which are closely related to the performance of the diaphragm in the battery. For example, depending on the specific use, people may urgently hope that the newly developed membrane can achieve at least one of the following effects: it is conducive to improving at least one of the battery energy density, ion transport performance and cycle performance; it is extremely light in weight, has excellent air permeability and has extremely high mechanical strength, wear resistance and peeling resistance; it has good affinity with the liquid used in the battery system and can achieve excellent electrolyte retention rate and electrolyte wettability; it can effectively inhibit the generation and accumulation of gas inside the battery system and prevent bulging of the battery or battery cell; it has a good promoting effect on the electrochemical reaction in the battery and significantly inhibits any adverse effects on the electrochemical reaction; it has excellent thermal properties and thermal stability, etc.

[0005] To this end, researchers in this field have conducted a lot of research and made many experimental improvements to the materials of the diaphragm, such as designing the polymer composition of the substrate in the diaphragm, or depositing organic polymer particles or inorganic ceramic material particles on the substrate, but no satisfactory diaphragm has been developed so far. Summary of the invention

[0006] The diaphragm of the present application has a coating containing a specially designed organic-inorganic hybrid composite compound, and thus exhibits extremely high energy density, low mass per unit area, high air permeability, high mechanical strength, excellent electrolyte wetting performance and retention rate, gas absorption, electrochemical reaction promotion, thermal stability and required thermal parameters, etc., and the performance of batteries and other electrical devices using the diaphragm, such as rate performance and cycle performance, is greatly improved.

[0007] A first aspect of the present application provides a diaphragm, the diaphragm comprising:

[0008] a polymer substrate layer, and

[0009] A coating applied to at least one surface of the polymer substrate layer, the coating comprising an organic-inorganic hybrid composite compound, wherein the organic-inorganic hybrid composite compound is composed of basic units represented by formula I periodically assembled along at least one spatial direction:

[0010] L x (M a C b ) y ·A z Formula I

[0011] In Formula I, M is a cation of one or more metals selected from the group consisting of Zn, Co, Cu, Fe, Cd, Mn, Ag, Rh, Ru, Be, Mg, Al, Sc, Cr, Ni, Y, Ti, Zr, Hf, Li, Na, K, In, Ca, Sr, Pb, lanthanide metals, actinide metals, and a is a value of 0.1-10;

[0012] C is one or more atoms, atomic groups, small molecules or anions selected from the following: O, =O, O 2- , S 2- , Cl - Br - ,I - , CO, -OH, OH - , H2O, b is a value from 0 to 20;

[0013] y is a value from 1 to 50;

[0014] When M is cations of two or more metals, the product of a and y represents the number of all metal cations in the basic unit represented by the single formula I;

[0015] L is one or more ligands selected from the following: imidazole, porphyrin, pyridine, pyrazole, pyrimidine, piperidine, pyrrolidine, furan, thiophene, piperazine, pyridazine, indole, quinoline, carbazole, morpholine, and salts, acid radicals, esters, amides, anhydrides, dimers or trimers of the above ligands, and one or more hydrogen atoms in the above ligands (e.g., hydrogen atoms directly connected to carbon atoms or hydrogen atoms directly connected to nitrogen atoms) can be optionally substituted by one or more substituents selected from the following: cyano, nitro, amino, aldehyde, carboxyl, halogen (e.g., one or more of F, Cl, Br and I), C1-C8 alkyl, hydroxy C1-C8 alkyl, C1-C8 alkoxy, C2-C8 alkenyl, C2-C8 alkynyl, C3-C8 16 Cycloalkyl, C6-C 20 Aryl, C6-C 20 heteroaryl, or any combination thereof, x is a value from 1 to 50;

[0016] A is an atom or cation of one or more metal elements selected from the group consisting of Li, Na, K, Rb, Cs, Be, Sr, Zn, Al, Mg and Ca, or is one or more molecules selected from the group consisting of H2, O2, H2O, CO2, NH3, CH4, methyl formate, ethyl acetate, propylene carbonate, and z is a value from 0 to 100.

[0017] According to one embodiment of the first aspect, in the organic-inorganic hybrid composite compound, the number of basic units shown in formula I periodically assembled along at least one spatial direction is an integer from 3 to 10,000. According to one embodiment of the first aspect, the number of basic units shown in formula I periodically assembled along at least one spatial direction of the X direction, Y direction and Z direction of the Cartesian coordinate system is an integer from 3 to 10,000. According to another embodiment of the first aspect, the extension direction of the periodic assembly of the basic units shown in formula I is along at least one of the three spatial directions X', Y' and Z', and the number of periodic assemblies is an integer from 3 to 10,000, and the three directions X', Y' and Z' are respectively at an angle of 0 to 75 degrees, for example, 5 to 60 degrees, with the X direction, Y direction and Z direction of the Cartesian coordinate system. According to another embodiment of the first aspect, 0.5≤x∶y≤6. According to another embodiment of the first aspect, when b is not zero, 0.5≤a∶b≤8. According to another embodiment of the first aspect, the organic-inorganic hybrid composite compound has the following structure: the metal cation M, the ligand L and optionally C together constitute a basic unit, and the basic unit is periodically assembled along at least one spatial direction to constitute the organic-inorganic hybrid composite compound having a multi-mesoporous or multi-microporous structure. According to another embodiment of the first aspect, M is a cation of one or more metals selected from the following: Co and Zn; and L is one or more ligands selected from the following: 2-methylimidazole (acid root / ester), benzimidazole (acid root / ester), 4-cyanoimidazole (acid root / ester), 5-chlorobenzimidazole (acid root / ester), 2-formaldehydeimidazole (acid root / ester) and 2-nitroimidazole (acid root / ester). According to another embodiment of the first aspect, the basic unit shown in formula I in the organic-inorganic hybrid composite compound is selected from one or more of the following: (mIm)2Co, (mIm)2Zn, (bIm)2Zn, (cnIm)2Zn, (cbIm) 39 [Zn 20 (OH)], (cbIm)(nIm)Zn, (Ica)2Zn and (cbIm)2Zn. According to another embodiment of the first aspect, the coating further comprises one or more components selected from the following: adhesives, inorganic particles, stabilizers, wetting agents, defoamers, thickeners, rheology modifiers, pH regulators and preservatives. According to another embodiment of the first aspect, the inorganic particles are selected from at least one of the following: boehmite, zeolite, molecular sieves, alumina, aluminum oxide, silica, aluminum nitride, silicon carbide, MgO, CaO, ZnO, ZrO2, TiO2, and mixtures thereof. According to another embodiment of the first aspect, the weight ratio of the organic-inorganic hybrid composite compound to the inorganic particles is 1:5 to 5:1.

[0018] The second aspect of the present application provides a battery, the battery comprising the separator according to any one of the above embodiments. According to one embodiment, the battery further comprises an electrode and an electrolyte. According to one embodiment, the battery is a secondary battery.

[0019] The third aspect of the present application provides an electrical device, the electrical device comprising the diaphragm described in any one of the above embodiments, the electrical device is selected from a rechargeable lithium ion battery, a rechargeable sodium ion battery, a lithium sulfur battery, a magnesium battery, a zinc battery and a supercapacitor. According to one embodiment, the electrical device is selected from a secondary lithium ion battery, a secondary sodium ion battery, a secondary lithium sulfur battery, a secondary magnesium battery, and a secondary zinc battery.

[0020] A fourth aspect of the present application provides an electrical device, which includes the battery or electrical device described in any one of the embodiments of the second or third aspects above.

[0021] The fifth aspect of the present application provides a method for manufacturing a diaphragm, the method comprising: providing a polymer substrate layer, and forming a coating comprising an organic-inorganic hybrid composite compound on at least one surface of the polymer substrate layer, wherein the organic-inorganic hybrid composite compound is as described in any one of the embodiments of the first aspect above.

[0022] The sixth aspect of the present application provides a method for improving the performance of a diaphragm, the method comprising: providing a polymer substrate layer, and a coating comprising the organic-inorganic hybrid composite compound of the present application on at least one surface of the polymer substrate layer; the improved diaphragm performance is selected from at least one of the following: (1) affinity of the diaphragm for the electrolyte; (2) air permeability, gas capacity and expansion resistance of the diaphragm; (3) surface density, energy density and mechanical strength of the diaphragm; (4) heat resistance, flame retardancy and explosion resistance of the diaphragm; (5) ionic conductivity of the diaphragm; (6) rate performance and cycle performance of a battery cell made using the diaphragm.

[0023] The seventh aspect of the present application provides a use of the organic-inorganic hybrid composite compound for improving the performance of a diaphragm; the improved diaphragm performance is selected from at least one of the following: (1) affinity of the diaphragm for the electrolyte; (2) air permeability, gas capacity and expansion resistance of the diaphragm; (3) surface density, energy density and mechanical strength of the diaphragm; (4) heat resistance, flame retardancy and explosion resistance of the diaphragm; (5) ion conductivity of the diaphragm; (6) rate performance and cycle performance of a battery cell made using the diaphragm.

[0024] According to any embodiment of the present application, the coating of the present application can achieve performance improvement, and the performance is selected from at least one of the following: energy density, ion transport performance, cycle performance, weight, air permeability, mechanical strength, wear resistance, peeling resistance, anti-bulging property, electrochemical reaction promotion, thermal properties, and thermal stability.

[0025] In the following detailed description, the design details of the diaphragm, electrical device, and manufacturing method thereof designed in the present application are described in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 Scanning electron microscopy (SEM) spectrum of an organic-inorganic hybrid composite compound synthesized according to one embodiment of the present application;

[0027] Figure 2A-2B A car according to one embodiment of the present application is shown, wherein a battery of the car includes the separator of the present application;

[0028] Figure 3A shows an exploded schematic diagram of a battery according to one embodiment of the present application;

[0029] Figure 3B-3C Shows Figure 3A A three-dimensional schematic diagram of a battery. DETAILED DESCRIPTION

[0030] "Range" disclosed herein is in the form of lower limit and upper limit. It can be one or more lower limits, and one or more upper limits respectively. A given range is defined by selecting a lower limit and an upper limit. The selected lower limit and upper limit define the boundaries of a particular range. All ranges that can be defined in this way are inclusive and combinable, i.e. any lower limit can be combined with any upper limit to form a range. For example, for a particular parameter, a range of 60-120 and 80-110 is listed, and it is understood that a range of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following ranges can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5.

[0031] In this application, unless otherwise specified, the numerical range "ab" represents an abbreviation of any real number combination between a and b, where a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" have been listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0032] If not specifically stated, the term "two" used in this specification means "at least two".

[0033] In this application, unless otherwise specified, all the embodiments mentioned herein can be combined with each other to form a new technical solution.

[0034] In this application, unless otherwise specified, all technical features mentioned herein can be combined with each other to form a new technical solution.

[0035] In this application, unless otherwise specified, all steps mentioned herein may be performed sequentially or randomly. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may also include step (c), which means that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0036] In this application, if there is no special explanation, the "including" mentioned herein means open or closed. For example, the "including" may mean that other components not listed may also be included, or only the listed components may be included.

[0037] In the present application, when describing the spatial relationship of a specific component or object relative to other components or objects, the terms "inside", "outside", "above", "below", etc. are used to indicate that the former is located inside, outside, above or below the latter, and the two may be in direct contact, or may be separated by a certain distance or separated by a third component or object.

[0038] According to one embodiment of the present application, the organic-inorganic hybrid composite compound can be prepared in a very simple manner, specifically, a metal cation soluble or insoluble salt, a ligand, a solvent, and optionally one or more other additives (such as a pH regulator, a surfactant, an oxidant, a reductant, a solubilizer, a seed, and the raw materials of A and C in Formula I, etc.) are formed into a mixed system according to a set ratio, the system is sealed, and aged at a specific temperature for a specific time, so that the metal cation M, the ligand L, and the optional A and C are spontaneously assembled (sometimes also regarded as orderly coprecipitation) to form the organic-inorganic hybrid composite compound of the present application. According to some embodiments of the present application, the small molecule represented by C can be introduced by adsorption after the synthesis of the organic-inorganic hybrid composite compound of the present application.

[0039] In the present application, the ligand contained in the organic-inorganic hybrid composite compound is selected from at least one of the following: imidazole, porphyrin, pyridine, pyrazole, pyrimidine, piperidine, pyrrolidine, furan, thiophene, piperazine, pyridazine, indole, quinoline, carbazole, morpholine, and salts, acid radicals, esters, amides, anhydrides, dimers or trimers of the above ligands, and one or more hydrogen atoms in the above ligands (for example, hydrogen atoms directly connected to carbon atoms or hydrogen atoms directly connected to nitrogen atoms) can be optionally substituted by one or more substituents selected from the following: cyano, nitro, amino, aldehyde, carboxyl, halogen (for example, one or more of F, Cl, Br and I), C1-C8 alkyl, hydroxy C1-C8 alkyl, C1-C8 alkoxy, C2-C8 alkenyl, C2-C8 alkynyl, C3-C8 16 Cycloalkyl, C6-C 20 Aryl, C6-C 20 Heteroaryl, or any combination thereof, x is a value from 1 to 50. In the composite compound of the present application, M and C (and optionally A, when A is not methane, methyl formate, ethyl acetate, propylene carbonate) provide contributions to the inorganic part, and L and optionally A (when A is methane, methyl formate, ethyl acetate, propylene carbonate) provide contributions to the organic part.

[0040] "Periodic assembly", "ordered assembly" and "periodic ordered assembly" can be used interchangeably in this application to indicate that basic units are repeated along at least one specified direction, such as one, two or three specified directions, and adjacent basic units are regularly connected by common points, edges or faces.

[0041] One of the most important improvements of the present application is to form a coating containing a specially designed organic-inorganic hybrid composite compound on a polymer substrate. In the following, for the purpose of simplification, the term "organic-inorganic hybrid composite compound" is referred to as "composite compound". That is to say, in the full text of the present application, the terms "organic-inorganic hybrid composite compound", "composite compound", and "organic-inorganic hybrid composite compound periodically assembled from the basic units shown in Formula I" can be used interchangeably. In addition, in the full text of the present application, the terms "pore", "channel" and "hole" can be used interchangeably to represent the micropores, mesopores, macroporous structures, or any combination thereof present in the composite oxide of the present application.

[0042] The composite compound specially designed in the present application has a microstructure that is very different from conventional metal organic complexes. Specifically, in the composite compound used in the present application, the metal cation represented by M and the ligand represented by L coordinate with each other, and optionally C and A are added to form the smallest structural unit (basic unit) shown in formula I, and then multiple such structural units are periodically assembled along at least one of the three directions of X, Y and Z of the Cartesian coordinate system (or along at least one of the directions of X', Y', and Z' that deviate from 0 to 75 degrees relative to the X, Y and Z directions of the Cartesian coordinate system) to form a porous material with a periodic porous mesh skeleton, and the pore size of the pores in the skeleton can be nanometer-level (for example, several nanometers, tens of nanometers, tens of nanometers or hundreds of nanometers), and the pores with such size can be called "nanopores", and the composite compound with pores with such size can be called "nanoscale composite compound" or "nanocomposite compound". The pore size of the pores in the skeleton can also be micrometer-level (e.g., several micrometers, tens of micrometers, tens of micrometers, or hundreds of micrometers). Pores with such sizes can be called "micrometer-level pores", and composite compounds with such pores can be called "micrometer-level composite compounds" or "micrometer-level composite compounds". Depending on the specific assembly form of the structural units in the composite compound, the composite compound may also include both nanopores and micrometer-level pores. In this case, the composite compound can also be called a "mixed composite compound".

[0043] According to one embodiment of the present application, the basic units are assembled periodically along one direction, for example, along one, two or three directions to form a composite compound of the present application having one or more geometric shapes selected from the following: nanorods or microrods, nanowires, single-layer or multi-layer sheets, cubes, quasi-cubes, cuboids, parallelepipeds, asymmetric hexahedrons, regular octahedrons, asymmetric octahedrons, spheres, near-spheres, ellipsoids, near-ellipsoids, ovals, near-ovals, irregular particles, etc. In the present application, "near" a certain shape or "quasi" a certain shape means that the contour deviation of the shape at any point on its outer contour relative to the standard shape defined after the word "near" or "quasi" is less than or equal to 20%, for example, less than or equal to 15%, or less than or equal to 10%, or less than or equal to 8%, or less than or equal to 5%, or less than or equal to 2%, or less than or equal to 1%, and the so-called contour deviation is determined based on the distance between a specific point on the outer contour and the mass center of the composite compound.

[0044] According to one embodiment of the present application, the metal cation M is selected from one or more of Zn, Co, Cu, Fe, Cd, Mn, Ag, Rh, Ru, Be, Mg, Al, Sc, Cr, Ni, Y, Ti, Zr, Hf, Li, Na, K, In, Ca, Sr, Pb, lanthanide metals and actinide metals, for example, selected from one or more of Zn, Mn, Ni, Co, Fe and Cu, for example, Co or Zn. a is a value of 1-10, for example, an integer of 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10, or a value within the range obtained by combining any two of the above values; in some cases, due to the doping, substitution or presence of a certain degree of lattice defects of a specific metal part in the composite compound of the present application, a can be expressed as a non-integer, for example, about 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4.0, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9, 5.0, 5.1, 5.2, 5.3, 5.4, 5.5, 5.6, 5.7, 5.8, 5.9, 6.1 .9, 4.0, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9, 5.0, 5.1, 5.2, 5.3, 5.4, 5.5, 5.6, 5.7, 5.8, 5.9, 6.0, 6.1, 6.2, 6.3, 6.4, 6.5, 6.6, 6.7, 6.8, 6.9, 7.0, 7.1, 7.2, 7 .3, 7.4, 7.5, 7.6, 7.7, 7.8, 7.9, 8.0, 8.1, 8.2, 8.3, 8.4, 8.5, 8.6, 8.7, 8.8, 8.9, 9.0, 9.1, 9.2, 9.3, 9.4, 9.5, 9.6, 9.7, 9.8, 9.9 or 10.0, or a value within the range obtained by combining any two of the above values.

[0045] In the basic unit of the composite compound shown in the above formula I, C is one or more atoms, atomic groups, small molecules or anions selected from the following: O, =O, O 2- , S 2- , Cl - Br - ,I - , CO, -OH, OH -, H2O, which is connected to the metal cation M through ionic bonds, covalent bonds or coordination bonds to form a cluster structure of metal cation-anion / metal cation-small atom / metal cation-small molecule, and then the cluster structure is used as a component of the basic unit together with the ligand as described above, and the composite compound of the present application is formed by periodic self-assembly. According to one embodiment of the present application, the C is an oxygen atom or an oxygen anion, and the combination of the metal cation and C constitutes a cluster structure, such as a cluster structure in which the central metal cation is surrounded by oxygen anions, such as a "metal-oxygen tetrahedron cluster" or a "metal-oxygen octahedron cluster". Depending on the type of anions surrounding the metal cation, the cluster structure, "metal-oxygen tetrahedron cluster" or "metal-oxygen octahedron cluster" can be either a regular tetrahedron or a regular octahedron, or a partially or completely deformed tetrahedron or octahedron. According to another embodiment of the present application, at least one oxygen ion or oxygen atom surrounding the metal cation (for example, located at the top of the cluster corner) in the above-mentioned cluster structure is selected from S 2- , Cl - Br - ,I - 、CO、CO2、-OH、OH -, H2O anion or small molecule substitution, so that the cluster structure is partially or completely deformed. b is a value of 0-20, for example, an integer of 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19 or 20, or a value within the range obtained by combining any two of the above values; in some cases, due to the doping, substitution or presence of a certain degree of lattice defects in a specific part of the composite compound of the present application, b can be expressed as a non-integer, for example, about 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4.0, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9, 5.0, 5.1, 5.2, 5.3, 5.4, 5.5, 5.6, 5.7, 5.8, 5.9, 6.0, 6.1, 6.2, 6.3, 6.4, 6.5, 6.6, 6.7, 6.8, 6.9, 7.0, 7.1, 7.2, 7.3, 7.4, 7.5, 7.6, 7.7, 7.8, 7.9, 8.0, 8.1, 8.2, 8.3, 8. 4, 8.5, 8.6, 8.7, 8.8, 8.9, 9.0, 9.1, 9.2, 9.3, 9.4, 9.5, 9.6, 9.7, 9.8, 9.9, 10.0, 10.1, 10.2, 10.3, 10.4, 10.5, 10.6, 10.7, 10.8, 10.9, 11.0, 11.1, 11.2, 11.3, 11.4, 11.5, 11.6, 11.7, 11.8, 11.9, 12.0, 12.1, 12.2, 12.3, 12.4, 12.5, 12.6, 12.7, 12.8, 12.9, 13.0, 13.1, 13.2, 13.3, 13.4, 13.5, 13.6、13.7、13.8、13.9、14.0、14.1、14.2、14.3、14.4、14.5、14.6、14.7、14.8、14.9、5.0、15.1、15.2、15.3、15.4、15.5、15.6、15.7、15.8、15.9、16.0、16.1、16.2、16.3、16.4、16.5、16.6、16.7、16.8、16.9、17.0、17.1、17.2、17.3、17.4、17.5、17.6、17.7、17.8、17.9、18.0、18.1、18.2、18.3、18.4, 18.5, 18.6, 18.7, 18.8, 18.9, 19.0, 19.1, 19.2, 19.3, 19.4, 19.5, 19.6, 19.7, 19.8, 19.9 or 20.0, or a value within the range obtained by combining any two of the above values. y is a value of 1-50, for example, an integer of 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, 50, or a value within the range obtained by combining any two of the above values. It can be seen that the product of a and y represents the number of M metal cations in a single basic unit shown in Formula I. When Formula I contains two or more different metal cations, the product of a and y represents the number of all metal cations in a single basic unit shown in Formula I; similarly, the product of b and y represents the number of anions, atoms or atomic groups represented by C in a single basic unit shown in Formula I. When the basic unit shown in Formula I contains two or more different Cs, the product of b and y represents the number of all Cs in a single basic unit shown in Formula I. According to some embodiments of the present application, the value of b is zero. In some embodiments of the present application, when C does not exist, for the sake of simplicity, the value of M in a specific compound may be directly written as the product of a and y. .

[0046] According to another embodiment of the present application, the ligand L is selected from one or more of the following: optionally substituted imidazole (acid radical / ester), optionally substituted polypyrazole (acid radical / ester). In the present application, the term "imidazole (acid radical / ester)" includes any one of imidazole, imidazole acid radical and imidazole ester, and the term "pyrazole (acid radical / ester)" includes any one of pyrazole, pyrazole acid radical and pyrazole ester. In the present application, the term "optionally substituted" means that at least one hydrogen atom directly bonded to a carbon atom, a nitrogen atom, an oxygen atom or a sulfur atom by a covalent bond (e.g., a hydrogen atom directly bonded to a carbon atom by a covalent bond) in the above-mentioned ligand is replaced by a substituent selected from the following: cyano, nitro, nitroso, amino, imino, aldehyde, carboxyl, halogen (e.g., fluorine, chlorine, bromine, iodine), C1-C8 alkyl (e.g., methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, sec-pentyl, n-hexyl, isohexyl, n-heptyl, isoheptyl, n-octyl, isooctyl), hydroxy C1-C8 alkyl (e.g., hydroxymethyl, hydroxyethyl or hydroxypropyl), C1-C8 alkoxy (e.g., methoxy, ethoxy, propoxy), C2-C8 alkenyl (e.g., vinyl, propenyl, allyl), C2-C8 alkynyl (e.g., ethynyl), C3-C8 16Cycloalkyl (e.g., cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, adamantyl), C6-C 20 Aryl (e.g. phenyl, benzyl, biphenyl, naphthyl, anthracenyl), C6-C 20 Heteroaryl.

[0047] According to another embodiment of the present application, the optionally substituted imidazole (acid root / ester) can be selected from one or more of the following: imidazole (acid root / ester), 2-methylimidazole (acid root / ester), 2-nitroimidazole (acid root / ester), 2-cyanoimidazole (acid root / ester), 2-chloroimidazole (acid root / ester), 2-aminoimidazole (acid root / ester), 2-formaldehydeimidazole (acid root / ester), 2-hydroxymethylimidazole (acid root / ester), 2-bromoimidazole (acid root / ester), 4-methylimidazole (acid root / ester), 4-nitroimidazole (acid root / ester), 4-cyanoimidazole (acid root / ester), 4-chloroimidazole (acid root / ester), 4-aminoimidazole (acid root / ester), 4 -Formaldehyde imidazole (acid radical / ester), 4-hydroxymethyl imidazole (acid radical / ester), 4-bromoimidazole (acid radical / ester), 5-methylimidazole (acid radical / ester), 5-nitroimidazole (acid radical / ester), 5-cyanoimidazole (acid radical / ester), 5-chloroimidazole (acid radical / ester), 5-aminoimidazole (acid radical / ester), 5-formaldehyde imidazole (acid radical / ester), 5-hydroxymethylimidazole (acid radical / ester), 4,5-dichloroimidazole (acid radical / ester), 4,5-dinitroimidazole (acid radical / ester), 5-chlorobenzimidazole (acid radical / ester), 5-nitrobenzimidazole (acid radical / ester), 5-bromoimidazole (acid radical / ester), 4-hydroxymethyl-5-methylimidazole (acid radical / ester).

[0048] According to another embodiment of the present application, the ligand can also be selected from one or more of the following: 1,4-phenylenebis(pyrazole) (acid radical / ester), 1,4-phenylenebis(tetrazolyl) (acid radical / ester), 1,3,5-phenyltri(tetrazolyl) (acid radical / ester).

[0049] x represents the number of ligands contained in the basic unit shown in Formula I, and is a value of 1-50, for example, an integer of 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, 50, or a value within the range obtained by combining any two of the above values, or a decimal between any two of the above values, for example, the value of x can be within the range obtained by combining any two of the following values: .1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3. 2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4.0, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9, 5.0, 5.1, 5.2, 5.3, 5.4, 5.5, 5.6, 5.7, 5.8, 5.9, 6.0, 6.1, 6.2, 6.3 , 6.4, 6.5, 6.6, 6.7, 6.8, 6.9, 7.0, 7.1, 7.2, 7.3, 7.4, 7.5, 7.6, 7.7, 7.8, 7.9, 8.0, 8.1, 8.2, 8.3, 8.4, 8.5, 8.6, 8.7, 8.8, 8.9, 9.0, 9.1, 9.2, 9.3, 9. 4, 9.5, 9.6, 9.7, 9.8, 9.9, 10.0, 10.1, 10.2, 10.3, 10.4, 10.5, 10.6, 10.7, 10.8, 10.9, 11.0, 11.1, 11.2, 11.3, 11.4, 11.5, 11.6, 11.7, 11.8, 11.9, 12. 0, 12.1, 12.2, 12.3, 12.4, 12.5, 12.6, 12.7, 12.8, 12.9, 13.0, 13.1, 13.2, 13.3, 13.4, 13.5, 13.6, 13.7, 13.8, 13.9, 14.0, 14.1, 14.2, 14.3, 14.4, 14. 5, 14.6, 14.7, 14.8, 14.9, 5.0, 15.1, 15.2, 15.3, 15.4, 15.5, 15.6, 15.7, 15.8, 15.9, 16.0, 16.1, 16.2, 16.3, 16.4, 16.5, 16.6, 16.7, 16.8, 16.9, 17.0, 17.1, 17.2, 17.3, 17.4, 17.5, 17.6, 17.7, 17.8, 17.9, 18.0, 18.1, 18.2, 18.3, 18.4, 18.5, 18.6, 18.7, 18.8, 18.9, 19.0, 19.1, 19.2, 19.3, 19.4, 19.5, 19.6, 19.7, 19.8, 19.9, 20.0, 20.1, 20.2, 20.3, 20.4, 20.5, 20.6, 20.7, 20.8 , 20.9, 21.1, 21.2, 21.5, 21.8, 22.0, 22.1, 22.2, 22.5, 22.8, 23.0, 23.2, 23.5, 23.8, 24.0, 24.2, 24.5, 24.8, 25.0, 26.2, 26.5, 26.8, 27.0, 27.2, 27.5, 27.8, 28.0, 28.2, 28.5, 28.8, 29.0, 29.2, 29.5, 29.8, 30.0, 30.2, 30.5, 30.8, 3 1.0, 31.2, 31.5, 31.8, 32.0, 32.2, 32.5, 32.8, 33.0, 33.2, 33.5, 33.8, 34.0, 34.2, 34.5, 34.8, 35.0, 35.2, 35.5, 35.8, 36.0, 36.2, 36.5, 36.8, 37.0, 37.2, 37.5, 37.8, 38.0, 38.2, 38.5, 38.8, 39.0, 39.2, 39.5, 39.8, 40.0, 40.2, 40. 5, 40.8, 41.0, 41.2, 41.5, 41.8, 42.0, 42.2, 42.5, 42.8, 43.0, 43.2, 43.5, 43.8, 44.0, 44.2, 44.5, 44.8, 45.0, 45.2, 45.5, 45.8, 46.0, 46.2, 46.5, 46.8, 47.0, 47.2, 47.5, 47.8, 48.0, 48.2, 48.5, 48.8, 49.0, 49.2, 49.5, 49.8, 50.0. When the basic unit represented by formula I contains two or more different ligands L, x represents the total number of all ligands L in a single basic unit represented by formula I. .

[0050] In the basic unit shown in the above formula I, A is an atom or cation of one or more metal elements selected from the following: Li, Na, K, Rb, Cs, Be, Sr, Zn, Al, Mg and Ca, or one or more molecules selected from the following: H2, O2, H2O, CO2, NH3, CH4, methyl formate, ethyl acetate, propylene carbonate. In the present application, there is no significant bonding interaction between the atom, ion or small molecule shown in A and the other components M, L and C of the composite compound of the present application, such as no covalent bond, coordination bond and / or ionic bond, for example, there is only a very weak dispersion force, hydrogen bond or very weak charge interaction between A and M, L and C. That is to say, A can only be accommodated in the pore structure of the composite compound of the present application, and there is no real bonding interaction with other components of the composite compound. z represents the number of atoms, ions or small molecules accommodated in the pore structure of the composite compound of the present application, and is an integer or decimal from 0 to 100, for example, an integer of 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, 50, 99, 100, or a value within the range obtained by combining any two of the above values, or a decimal between any two of the above values.

[0051] In the present application, the ratio of x to y (x:y) can vary in the range of 0.5-6, for example, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1 , 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4.0, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9, 5.0, 5.1, 5.2, 5.3, 5.4, 5.5, 5.6, 5.7, 5.8, 5.9, 6.0, or a value within the range obtained by combining any two of the above values. In the present application, when b is not zero, the ratio of a to b (a:b) can vary in the range of 0.1-8, for example, 0.1, 0.2, 0.25, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7 , 3.8, 3.9, 4.0, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9, 5.0, 5.1, 5.2, 5.3, 5.4, 5.5, 5.6, 5.7, 5.8, 5.9, 6.0, 6.1, 6.2, 6.3, 6.4, 6.5, 6.6, 6.7, 6.8, 6.9, 7.0, 7.1, 7.2, 7.3, 7.4, 7.5, 7.6, 7.7, 7.8, 7.9, 8.0, or a value within the range obtained by combining any two of the above values.According to one embodiment of the present application, the basic unit shown in Formula I is periodically assembled along at least one of the three spatial directions of X, Y and Z of the Cartesian coordinate system (for example, along the X direction, or along the Y direction, or along the Z direction, or along the X direction and the Y direction, or along the X direction and the Z direction, for example, along the X direction, the Y direction and the Z direction) The number of repetitions is an integer from 3 to 10,000, for example, an integer from 5 to 8,000, or an integer from 10 to 7,000, or an integer from 20 to 6,000, or an integer from 50 to 5,000. An integer, or an integer from 70 to 4,000, or an integer from 80 to 3,000, or an integer from 90 to 2,000, or an integer from 100 to 1,000, for example, the number of periodic assembly repetitions along any one of the X, Y and Z directions (for example, along the three directions of X, Y and Z) is 3, 5, 9, 10, 20, 30, 40, 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, 150, 160, 170, 200, 220, 250, 280, 300, 320, 350, 380, 400 , 450, 500, 550, 600, 650, 700, 750, 800, 850, 900, 950, 1000, 1100, 1200, 1300, 1400, 1500, 1600, 1700, 1800, 1900, 2000, 2100, 2200, 2300, 2400, 2500, 2600, 2700, 2800, 2900, 3000, 3100, 3200, 3300, 3400, 3500, 3600, 3700, 3800, 3900, 4000, 4100, 420 0, 4300, 4400, 4500, 4600, 4700, 4800, 4900, 5000, 5100, 5200, 5300, 5500, 5600, 5800, 6000, 6200, 6400, 6500, 6600, 6800, 7000, 7200, 7400, 7500, 7800, 8000, 8200, 8400, 8600, 8800, 9000, 9200, 9400, 9500, 9800, 10000, or a value within the range obtained by combining any two of the above values.

[0052] According to another embodiment of the present application, the basic unit shown in Formula I is periodically assembled along any one or more of the X', Y' and Z' spatial directions that deviate from the X, Y and Z directions of the Cartesian coordinate system. For example, the X', Y' and Z' directions deviate from at least one of the three directions of X, Y and Z of the Cartesian coordinate system by a specific angle, such as 0-70 degrees, such as 2-65 degrees, or 5-60 degrees, or the deviation angle is 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 64, 65, 66, 67, 68, 69, 70, or the deviation angle value is within the range of values ​​obtained by combining any two of the above values.According to one embodiment of the present application, the number of repetitions of the basic unit shown in Formula I periodically assembled along any one or more of the X', Y' and Z' directions (for example, along the X' direction, or along the Y' direction, or along the Z' direction, or along the X' direction and the Y' direction, or along the X' direction and the Z' direction, for example, along the X' direction, the Y' direction and the Z' direction) is an integer from 3 to 10,000, for example, an integer from 5 to 8,000, or an integer from 10 to 7,000, or an integer from 20 to 6,000, or 50 to 5, The number of repetitions of the periodic assembly in any direction of the X', Y' and Z' directions (for example, along the three directions of X', Y' and Z') is 3, 5, 9, 10, 20, 30, 40, 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, 150, 160, 170, 200, 220, 250, 280, 300, 320, 350, 360, 370, 380, 390, 400, 410, 420, 430, 440, 450, 460, 470, 480, 490, 500, 510, 520, 530, 540, 550, 560, 570, 580, 590, 600, 610, 620, 630, 640, 650, 660, 670, 680, 700, 710, 720, 730, 740, 750, 760, 770, 780, 790, 800, 810, 820, 830, 840, 850, 860, 870, 880, 890, 900 , 380, 400, 450, 500, 550, 600, 650, 700, 750, 800, 850, 900, 950, 1000, 1100, 1200, 1300, 1400, 1500, 1600, 1700, 1800, 1900, 2000, 2100, 2200, 2300, 2400, 2500, 2600, 2700, 2800, 2900, 3000, 3100, 3200, 3300, 3400, 3500, 3600, 3700, 3800, 3900, 4000, 4100 , 4200, 4300, 4400, 4500, 4600, 4700, 4800, 4900, 5000, 5100, 5200, 5300, 5500, 5600, 5800, 6000, 6200, 6400, 6500, 6600, 6800, 7000, 7200, 7400, 7500, 7800, 8000, 8200, 8400, 8600, 8800, 9000, 9200, 9400, 9500, 9800, 10000, or a value within the range obtained by combining any two of the above values.

[0053] According to one embodiment of the present application, for the purpose of simplification, the basic unit of general formula I is used to represent the composite compound of the present application. As described above, the composite compound is composed of the basic units shown in formula I that are periodically assembled along at least one spatial direction. According to one embodiment of the present application, the composite compound of the present application is formed by the basic units shown in formula I that are periodically assembled along three spatial directions, and its macroscopic structure is manifested as basically spherical particles, the particle size of which can be measured by various conventional technical means, and the size of the basic unit is determined by the types of all the components shown in formula I. The average value or maximum value of the above-mentioned periodic assembly repetition number of the composite compound of the present application can be determined by the ratio of the particle size of the particle to the one-dimensional size of the basic unit.

[0054] According to one embodiment of the present application, the composite compound of the present application contains neither C nor A; according to another embodiment of the present application, the composite compound of the present application contains both C and A; according to another embodiment of the present application, the composite compound of the present application contains C but not A; according to another embodiment of the present application, the composite compound of the present application contains A but not C.

[0055] The present application also includes new embodiments obtained by combining any two or more embodiments of the present application.

[0056] According to one embodiment of the present application, the skeleton structure of the composite compound is mainly composed of basic units composed of metal cations represented by M and ligands represented by L (and optionally C and A) assembled in a periodic, orderly and uniform manner, and the obtained composite compound has a highly regular oriented structure. According to the types and relative proportions of the metal cations and ligands used, as well as the processing conditions and other raw materials used in the synthesis process, the assembly pattern and pore size of the skeleton structure of the composite compound can be adjusted. According to one embodiment of the present application, the metal cation M and the ligand L are connected by one or more of coordination bonds, covalent bonds and ionic bonds. According to another embodiment of the present application, the composite compound of the present application contains M and C at the same time, M first forms a cluster structure with C, and then the cluster structure is connected to the ligand L by one or more of coordination bonds, covalent bonds and ionic bonds.

[0057] According to a particular embodiment of the present application, the composite compound of the present application has the following structure: In the structure, the ligand shown in formula I is an optionally substituted imidazole, an aromatic polyimidazole compound or a heteroaromatic polyimidazole compound, for example, it can be one or more ligands selected from the following: imidazole (acid root / ester), 2-methylimidazole (acid root / ester), 2-nitroimidazole (acid root / ester), 2-cyanoimidazole (acid root / ester), 2-chloroimidazole (acid root / ester), 2-aminoimidazole (acid root / ester), 2-formaldehydeimidazole (acid root / ester), 2-hydroxymethylimidazole (acid root / ester), 2-bromoimidazole (acid root / ester), 4-methylimidazole (acid root / ester), 4-nitroimidazole (acid root / ester), 4-cyanoimidazole (acid root / ester), 4-chloroimidazole (acid root / ester), Imidazole (acid radical / ester), 4-aminoimidazole (acid radical / ester), 4-formaldehydeimidazole (acid radical / ester), 4-hydroxymethylimidazole (acid radical / ester), 4-bromoimidazole (acid radical / ester), 5-methylimidazole (acid radical / ester), 5-nitroimidazole (acid radical / ester), 5-cyanoimidazole (acid radical / ester), 5-chloroimidazole (acid radical / ester), 5-aminoimidazole (acid radical / ester), 5-formaldehydeimidazole (acid radical / ester), 5-hydroxymethylimidazole (acid radical / ester), 4,5-dichloroimidazole (acid radical / ester), 4,5-dinitroimidazole (acid radical / ester), 5-chlorobenzimidazole (acid radical / ester), 5-nitrobenzimidazole (acid radical / ester), 5-bromoimidazole (acid radical / ester), and 4-hydroxymethyl-5-methylimidazole (acid radical / ester). According to one embodiment of the present application, the metal cation M shown in Formula I is at least one cation selected from Zn, Co, Cu, Fe, Cd, Mn, Ag, Rh, Ru, Sc, Cr, Ni, Y, Ti, Zr, Hf, Sr, Pb and lanthanide metals, for example, it can be one or both of Zn (II) and Co (II). According to one embodiment of the present application, each M metal cation in the composite compound of the present application is connected to an imidazole L ligand (the lone pair of electrons of the nitrogen atom on the imidazole ring forms a coordination bond with the metal cation M), forming a metal-ligand tetrahedral structure, and then a plurality of tetrahedrons are interconnected with the help of imidazole ligands to form a structure rich in mesopores and / or micropores.

[0058] According to one embodiment of the present application, in the structure, each imidazole (ester) ligand and the two metal-ligand tetrahedrons directly connected thereto are connected in a fixed molar ratio of 1:2, and are connected at a bond angle of approximately 145° (may be slightly deformed due to the influence of intramolecular attraction, repulsion, and intramolecular stress, such as ±15 degrees, or ±10 degrees, or ±5 degrees, or ±2 degrees, or ±1 degree, or a deformation within ±0.5 degrees) to form a three-dimensional molecular structure, and the basic unit is periodically assembled along at least one of the three directions of X, Y, and Z of the Cartesian coordinate system to form a structure rich in mesopores and / or micropores.

[0059] According to one embodiment of the present application, the periodic assembly of the above-mentioned basic units constitutes a reciprocating zigzag structure in at least one direction, for example, a reciprocating zigzag structure in one, two or three directions, and a mesopore and / or micropore structure is formed in the zigzag structure. According to one embodiment of the present application, the periodic assembly of the above-mentioned basic units constitutes a reciprocating wavy structure in at least one direction, for example, a reciprocating wavy structure in one, two or three directions, and a mesopore and / or micropore structure is formed in the wavy structure. According to one embodiment of the present application, the periodic assembly of the above-mentioned basic units constitutes a spiral structure around the spatial direction as the central axis in at least one direction, for example, a spiral structure around the spatial direction as the central axis in one, two or three directions, and a mesopore and / or micropore structure is formed in the spiral structure. According to one embodiment of the present application, the periodic assembly of the above-mentioned basic units forms a closed spherical structure, and a mesopore and / or micropore structure is formed in the spherical structure.

[0060] According to one embodiment of the present application, the basic unit / basic unit is periodically assembled along one, two or three directions to form a composite compound of the present application having one or more geometric shapes selected from the following: nanorods or microrods, nanowires, single-layer or multi-layer sheets, cubes, quasi-cubes, cuboids, parallelepipeds, asymmetric hexahedrons, regular octahedrons, asymmetric octahedrons, spheres, near-spheres, ellipsoids, near-ellipsoids, ovoids, near-ovoids, irregular particles, etc. In the present application, "near" a certain shape or "quasi" a certain shape means that the contour deviation of the shape at any point on its outer contour relative to the standard shape defined after the word "near" or "quasi" is less than or equal to 20%, for example, less than or equal to 15%, or less than or equal to 10%, or less than or equal to 8%, or less than or equal to 5%, or less than or equal to 2%, or less than or equal to 1%, and the so-called contour deviation is determined based on the distance between a specific point on the outer contour and the mass center of the composite compound.

[0061] According to one embodiment of the present application, C in Formula I does not exist, that is, b = 0. According to one embodiment of the present application, A does not exist, that is, z can be zero.

[0062] According to one embodiment of the present application, the basic unit of the composite compound having the above structure is selected from one or more of the following: (mIm)2Co, (mIm)2Zn, (bIm)2Zn, (cnIm)2Zn, (cbIm) 39 [Zn 20(OH)], (cbIm)(nIm)Zn, (Ica)2Zn and (cbIm)2Zn, wherein cnIm represents 4-cyanoimidazole (acid / ester), cbIm represents 5-chlorobenzimidazole (acid / ester), nIm represents 2-nitroimidazole (acid / ester), Im represents imidazole (acid / ester), mIm represents 2-methylimidazole (acid / ester), Ica represents 2-formaldehydeimidazole (acid / ester), and bIm represents benzimidazole (acid / ester).

[0063] According to one embodiment of the present application, the "basic unit" serving as the minimum repeating unit in the composite compound is obtained by periodically assembling more than one minimum unit cell, for example, a 2×2×2 aggregate formed by periodically assembling 8 minimum unit cells is used as the basic structure of Formula I, or a 3×3×3 aggregate formed by periodically assembling 27 minimum unit cells is used as the basic structure of Formula I, or a 4×4×4 aggregate formed by periodically assembling 64 minimum unit cells is used as the basic structure of Formula I, or a 5×5×5 aggregate formed by periodically assembling 125 minimum unit cells is used as the basic structure of Formula I, or a 6×6×6 aggregate formed by periodically assembling 216 minimum unit cells is used as the basic structure of Formula I, or a 7×7×7 aggregate formed by periodically assembling 343 minimum unit cells is used as the basic structure of Formula I, or an 8×8×8 aggregate formed by periodically assembling 512 minimum unit cells is used as the basic structure of Formula I, or a larger aggregate is used as the basic structure of Formula I, in which case the ratios x, a, b, y and z in Formula I may have larger values.

[0064] According to the embodiment of the application, the diaphragm with improved performance is prepared by forming a coating comprising the composite compound of the application on at least one surface of the substrate layer. The substrate layer used in the application can be a polymer film with microporous structure, for example, it can be a polymer film selected from the following materials: polyolefin (such as ethylene-propylene copolymer), glass fiber, aramid, polyvinyl alcohol, cellulose, polyethylene oxide, polytetrafluoroethylene, polyallylamine, polyacrylonitrile, polyurethane, polymethyl methacrylate, polyimide, polyethylene terephthalate, polybutylene terephthalate, polyacetal, polycarbonate, polyetheretherketone, polysulfone, polyphenylene oxide, polystyrene, polyvinyl naphthylene and any two or more of the above materials Physical mixture or copolymer, wherein polyolefin can include polypropylene, polyethylene and its physical mixture or copolymer. The substrate layer of the application can have different micropore sizes as required, for example, 0.01-100 micron, or 0.1-10 micron, or 1-5 micron. The thickness of the substrate layer can be appropriately adjusted as needed, for example, the thickness can be 0.1-100 microns, such as 0.5-80 microns, or 1-70 microns, or 2-60 microns, or 4-50 microns, or 5-40 microns, or 6-30 microns, or 7-20 microns, or 8-15 microns, or 9-12 microns. As needed, before applying the coating containing the composite compound of the present application on the substrate layer, an adhesive layer or a primer layer can be optionally first applied to at least one surface of the substrate layer, so as to achieve the purpose of improving the bonding strength of the coating or improving the overall performance of the diaphragm. For example, non-limiting examples of adhesives that can be used include acrylonitrile-styrene-butadiene copolymers, acrylic acid-acrylate-acrylonitrile copolymers, acrylic acid-polyimide, carboxymethyl cellulose, cyanoethyl sucrose, cyanoethyl cellulose, cyanoethyl polyvinyl alcohol, cellulose acetate propionate, cellulose acetate butyrate, cellulose acetate, polyethylene oxide, ethylene-vinyl acetate copolymer, polyvinyl acetate, polyvinyl pyrrolidone, polyacrylonitrile, polymethyl methacrylate, vinylidene fluoride-trichloroethylene copolymer, vinylidene fluoride-hexafluoropropylene copolymer, and any mixture of the above-mentioned adhesives. According to another embodiment of the present application, the adhesive layer formed between the substrate layer and the coating can also include one or more inorganic particles, such as the inorganic particles can be selected from one or more of the following: boehmite, molecular sieves, zeolites, alumina, hydroxyalumina, silicon dioxide, aluminum nitride, silicon carbide, MgO, CaO, ZnO, ZrO2, TiO2, and any mixture of the above-mentioned inorganic particles.According to some embodiments of the present application, the molecular sieve is selected from one or more of the following: ZSM molecular sieves, such as ZSM-5, ZSM-11, ZSM-12, ZSM-34, ZSM-41, etc.; SAPO molecular sieves, such as SAPO-5, SAPO-11, SAPO-31, SAPO-34, SAPO-41, etc.; A-type molecular sieve; Y-type molecular sieve; X-type molecular sieve. According to one embodiment of the present application, the average particle size of these inorganic particles is 0.001-10 microns, such as 0.01-8 microns, or 0.02-7 microns, or 0.03-6 microns, or 0.05-5 microns, or 0.1-4 microns, or 0.5-3 microns, or 0.8-2 microns, or 0.5-1 micron. According to one embodiment of the present application, in the adhesive layer, the weight ratio of the adhesive to the inorganic particles can be 1:0 to 1:10, for example, 1:0.2 to 1:9, or 1:0.4 to 1:8, or 1:0.5 to 1:7, or 1:0.6 to 1:6, or 1:0.7 to 1:5, or 1:0.8 to 1:4, or 1:1 to 1:3, or 1:1.5 to 1:2. According to another embodiment of the present application, the coating layer containing the composite compound of the present application is directly applied on the substrate layer without applying an adhesive layer or a primer layer therebetween.

[0065] According to one embodiment of the present application, the composite compound of the present application is dispersed (dissolved or suspended) in an aqueous solvent, an organic solvent, or applied to the substrate layer without using a solvent. The specific application technique can be any of the following: dip coating, slot die coating, gravure coating, extrusion coating, blade coating, spin coating, curtain coating, etc. According to one embodiment of the present application, the organic solvent can be selected from one or more of the following: water, acetone, methanol, ethanol, acetic acid, dimethylformamide, dimethylacetamide, N-methyl-pyrrolidone, tetrahydrofuran, dichloromethane, chloroform, cyclohexane. According to one embodiment of the present application, when a solvent is used, the amount of the solvent can be 5-95% by weight, such as 10-90% by weight, or 20-80% by weight, or 30-70% by weight, or 40-60% by weight, or 45-50% by weight, compared to the total weight of the coating (solution or suspension) before application.

[0066] According to one embodiment of the present application, in addition to the composite compound of the present application, the coating formed on the substrate layer may also contain one or more adhesives, which may be selected from one or more of the following: polyacrylate, acrylonitrile-styrene-butadiene copolymer, acrylic acid-acrylate-acrylonitrile copolymer, acrylic acid-polyimide, carboxymethyl cellulose, cyanoethyl sucrose, cyanoethyl cellulose, cyanoethyl polyvinyl alcohol, cellulose acetate propionate, cellulose acetate butyrate, cellulose acetate, polyethylene oxide, ethylene-vinyl acetate copolymer, polyvinyl acetate, polyvinyl pyrrolidone, polyacrylonitrile, polymethyl methacrylate, vinylidene fluoride-trichloroethylene copolymer, vinylidene fluoride-hexafluoropropylene copolymer, and any mixture of the above adhesives. According to one embodiment of the present application, based on the total weight of the coating finally formed, the content of the adhesive may be 1-25% by weight, for example 3-20% by weight, or 5-15% by weight, or 6-10% by weight, or 7-9% by weight.

[0067] According to another embodiment of the present application, in addition to the composite compound of the present application, the coating formed on the substrate layer may also contain one or more inorganic particles, which may have a dielectric constant greater than 1, piezoelectricity and / or ionic conductivity, for example, the inorganic particles may be selected from one or more of the following: boehmite, molecular sieves, zeolites, alumina, hydroxyalumina, silicon dioxide, aluminum nitride, silicon carbide, MgO, CaO, ZnO, ZrO2, TiO2, and any mixture of the above inorganic particles. According to some embodiments of the present application, the molecular sieve is selected from one or more of the following: ZSM molecular sieves, such as ZSM-5, ZSM-11, ZSM-12, ZSM-34, ZSM-41, etc.; SAPO molecular sieves, such as SAPO-5, SAPO-11, SAPO-31, SAPO-34, SAPO-41, etc.; A-type molecular sieve; Y-type molecular sieve; X-type molecular sieve. According to one embodiment of the present application, based on the total weight of the final coating, the content of the inorganic particles can be 0-70% by weight, such as 10-65% by weight, or 20-60% by weight, or 30-50% by weight, or 35-45% by weight. According to one embodiment of the present application, the average particle size of these inorganic particles is 0.001-10 microns, such as 0.01-8 microns, or 0.02-7 microns, or 0.03-6 microns, or 0.05-5 microns, or 0.1-4 microns, or 0.5-3 microns, or 0.8-2 microns, or 0.5-1 micron.

[0068] According to another embodiment of the present application, the coating formed on the substrate layer may contain one or more other additives, such as stabilizers, wetting agents, rheology modifiers, pH adjusters, preservatives, etc., in addition to the composite compound of the present application.

[0069] According to one embodiment of the present application, the average particle size of the composite compound of the present application contained in the coating formed on the substrate layer is 0.001-10 microns, such as 0.01-8 microns, or 0.02-7 microns, or 0.03-6 microns, or 0.05-5 microns, or 0.1-4 microns, or 0.5-3 microns, or 0.8-2 microns, or 0.5-1 microns. According to another embodiment of the present application, based on the total weight of the coating finally formed, the content of the composite compound of the present application can be 0-99% by weight, such as 10-90% by weight, or 20-80% by weight, or 30-70% by weight, or 40-60% by weight, or 45-50% by weight.

[0070] According to one embodiment of the present application, a dispersion (solution or suspension or slurry) containing the composite compound of the present application is applied to at least one surface of a substrate layer to form a coating after drying. The thickness of the dry coating is 0.1-100 microns, for example, 0.5-80 microns, or 1-70 microns, or 2-60 microns, or 4-50 microns, or 5-40 microns, or 6-30 microns, or 7-20 microns, or 8-15 microns, or 9-12 microns.

[0071] In the present application, the technical effects that can be brought about by the diaphragm of the present application are mainly studied based on rechargeable sodium-ion batteries and rechargeable lithium-ion batteries. However, it should be pointed out here that the diaphragm of the present application can be used in many other electrical devices and bring corresponding technical improvements thereto. Examples of the other electrical devices may include potassium-ion batteries, lithium-sulfur batteries, supercapacitors, etc.

[0072] According to one embodiment, the electrical device of the present application is a battery cell or a battery. In the present application, a "battery cell" refers to a battery cell that can be charged and discharged independently. The battery cell structure includes a positive electrode, a negative electrode, a separator, an electrolyte (such as an electrolyte), and an outer packaging for encapsulating a positive electrode plate, a negative electrode plate, a separator, and an electrolyte (electrolyte). The present application has no particular restrictions on the type and shape of the battery cell, which can be a soft-pack battery cell, a cylindrical battery cell, a square battery cell, or other types of battery cells.

[0073] "Battery" refers to a single physical module that includes one or more battery cells to provide higher voltage and capacity. The battery may include battery modules and battery packs. The battery module is formed by electrically connecting a certain number of battery cells together and placing them in a frame in order to protect the battery cells from external impact, heat, vibration, etc. The battery pack is the final state of the battery system installed in an electrical device (such as an electric car, etc.). According to some embodiments of the present application, the battery pack may be made by assembling various control and protection systems such as a battery management system and thermal management components on one or more battery modules. According to some other embodiments of the present application, the various control and protection systems such as the above-mentioned battery management system and thermal management components may be omitted from the battery module, that is, in this embodiment, the battery pack may be directly formed by one or more battery cells. In such an embodiment, the battery system significantly reduces the number of components while its weight energy density and volume energy density are improved.

[0074] The positive electrode that can be used in the present application may include a common positive electrode active material in a battery, including, for example, alkali manganese oxide, alkali cobalt oxide, alkali nickel oxide, alkali nickel manganese oxide, alkali nickel cobalt manganese oxide, alkali nickel cobalt aluminum oxide, alkali iron oxide, alkali iron phosphate, and the positive electrode may also include other materials, such as dopants, conductive agents, adhesives, ion supplements, metal foils, etc. The negative electrode that can be used in the present application may include a common negative electrode material in a battery, such as graphite, metallic lithium, graphene, carbon nanotubes, soft carbon, hard carbon, titanium oxide, silicon, silicon oxide, silicon-carbon composite, lithium titanate, germanium, tin oxide, transition metal oxides (such as ferric oxide, ferric oxide, cobalt oxide, cobalt oxide, manganese oxide), organic matter with reversible redox properties, etc. According to one embodiment of the present application, the electrolyte includes a solvent and an electrolyte dissolved in the solvent. For example, the solvent for the electrolyte can include one or more of the following: ethylene carbonate, fluoroethylene carbonate, propylene carbonate, dimethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, butylene carbonate, diethyl carbonate, methyl butyl carbonate, ethyl propyl carbonate, dipropyl carbonate, cyclopentanone, dimethyl sulfoxide, methyl formate, methyl acetate, ethyl acetate, N-methyl pyrrolidone, tetrahydrofuran, dimethyl ether, nitromethane, 2-methoxyethyl acetate, 2-ethoxyethyl acetate, diethyl oxalate, γ-butyrolactone, γ-valerolactone, γ-caprolactone, dimethoxyethane, 2-methyltetrahydrofuran, dioxane. The electrolyte for the electrolyte can be a metal salt, such as a sodium salt, a lithium salt, a potassium salt, a magnesium salt, a zinc salt and an aluminum salt. According to one embodiment, the electrochemical device of the present application is a lithium ion battery, in which the electrolyte used is a sodium salt, for example, it may include one or more of the following: sodium hexafluorophosphate (V), sodium hexafluoroarsenate (V), sodium perchlorate, sodium tetrachloroaluminate, sodium chloride, sodium tetrafluoroborate, sodium trifluoromethanesulfonate, sodium tetrafluorophosphate, sodium dioxalate borate, sodium difluorooxalate borate, sodium di(trifluoromethylsulfonic acid)imide, or according to the circumstances, it may be a lithium salt or potassium salt corresponding to the above sodium salt, or a mixture of any two or more of the above sodium salt, lithium salt and potassium salt. According to one embodiment of the present application, based on the total weight of the electrolyte, the content of the solvent is 60-99% by weight, for example, 65-95% by weight, or 70-90% by weight, or 75-89% by weight, or 80-85% by weight. According to another embodiment of the present application, based on the total weight of the electrolyte, the content of the electrolyte is 1-40 wt%, such as 5-35 wt%, or 10-30 wt%, or 11-25 wt%, or 15-20 wt%.

[0075] According to one embodiment of the present application, the positive electrode, the separator and the negative electrode are stacked in order so that the separator is located between the positive electrode and the negative electrode to separate the two, and the above-mentioned stacked structure is wound into a roll to obtain a bare battery cell. The bare battery cell is packaged in an outer packaging material, and an electrolyte is injected therein to obtain a battery cell for use in electrical devices. According to one embodiment of the present application, the separator has a coating containing the composite compound of the present application on both sides of the substrate layer. According to another embodiment of the present application, the separator has a coating containing the composite compound of the present application only on one side of the substrate layer, in which case the coated surface faces the cathode side or the anode side.

[0076] According to one embodiment of the present application, the composite compound of the present application can be synthesized in the following manner: according to the general formula of the target product, the corresponding metal cation soluble salt or insoluble salt and the ligand are dispersed in a polar solvent (water, ammonia water, methanol, dimethylformamide, etc.) in the required proportion, and an oxidant, a reducing agent, a surfactant, etc. are optionally added as needed (it is also possible to add only one of the above additives, or not to add the above additives), and aged for a period of time in a sealed environment at room temperature to 280°C (for example, 80-200°C, or 80-120°C), and the target product is obtained by a self-assembly reaction.

[0077] According to some embodiments of the present application, an electrical device (such as a battery) including the diaphragm of the present application can be used in various electrical equipment (electrical equipment) using batteries, for example, the electrical equipment may include mobile phones, portable devices, laptops, battery vehicles, electric cars, ships, spacecraft, electric toys and electric tools, etc., wherein the spacecraft may include airplanes, rockets, space shuttles and spacecraft, etc., electric toys include fixed or mobile electric toys, for example, game consoles, electric car toys, electric ship toys and electric airplane toys, etc., electric tools include metal cutting electric tools, grinding electric tools, assembly electric tools and railway electric tools, such as electric drills, electric grinders, electric wrenches, electric screwdrivers, electric hammers, impact drills, concrete vibrators and electric planers.

[0078] The application of the battery of the present application is not limited to the electrical devices mentioned above, and its intended use may include batteries in automobiles. For example, Figure 2A and 2B A schematic diagram of a car according to an embodiment of the present application is shown. The car can be a fuel car, a gas car or a new energy car, and the new energy car can be a pure electric car, a hybrid car or an extended range car, etc. Figure 2A As shown, a battery 10 may be provided inside the automobile 1. Figure 2AThe battery 10 is shown to be arranged at the bottom of the vehicle, but it is also possible to arrange the battery 10 at the front or rear of the vehicle 1 as required. During the operation of the vehicle, the battery 10 can provide power to the vehicle 1 in an intermittent or continuous manner. For example, the battery 10 can be used to supply power to the vehicle 1 lights, LCD screen, ignition device and other devices. In the case of a hybrid vehicle or an electric vehicle, the battery 10 can also be used to supply driving power to the vehicle 1. Figure 2B As shown, the car 1 may also include a controller 30 and a motor 40. The controller 30 is used to control the battery 10 to supply power to the motor 40, for example, for starting, navigating, and driving the car 1. In another embodiment of the present application, the battery 10 may not only be used as an operating power source for the car 1, but also as a driving power source for the car 1, replacing or partially replacing fuel or natural gas to provide driving power for the car 1. According to one embodiment of the present application, the battery 10 used in the car may also include multiple Figures 3A-3C A battery pack of battery cells 20 is shown.

[0079] Figures 3A-3C A battery 10 according to an embodiment of the present application is shown. In this embodiment, it can also be referred to as a battery cell 20, which includes a box 21, an electrode assembly 22 and an electrolyte, wherein the electrode assembly 22 is contained in the box 21 of the battery cell 20, and the electrode assembly 22 includes a positive electrode sheet, a negative electrode sheet and a separator. The separator can be a separator prepared in an embodiment of the present application. The electrode assembly 22 can be a winding structure or a laminated structure, for example, it can be a structure actually adopted in an embodiment of the present application. The box 21 includes a shell 211 and a cover plate 212. The shell 211 includes a housing 211a formed by a plurality of walls and an opening 211b. The cover plate 212 is arranged at the opening 211b to close the housing chamber 211a. In addition to the electrode assembly 22, the housing chamber 211a also contains an electrolyte. The positive electrode sheet and the negative electrode sheet in the electrode assembly 22 are generally provided with tabs, and the tabs generally include positive tabs and negative tabs. According to some embodiments of the present application, the number of positive electrode tabs is multiple and stacked together, and the number of negative electrode tabs is multiple and stacked together. The tabs are connected to the positive electrode terminal 214a and the negative electrode terminal 214b outside the battery cell 20 through the connecting member 23. For a square battery cell, Figure 3A and Figure 3C As shown, the positive electrode terminal 214 a and the negative electrode terminal 214 b may generally be disposed on the cap plate 212 portion.

[0080] In the following, the influence of the diaphragm manufactured according to the implementation mode of the present application on the performance of the electrochemical device is characterized based on specific examples, but it should be pointed out in particular that the scope of protection of the present application is defined by the claims and is not limited to the above specific implementation modes.

[0081] Example

[0082] Unless otherwise specified, all raw materials used in this application were of analytical grade and all water was deionized water.

[0083] Example 1: Synthesis of the composite compound of the present application

[0084] In this example, the composite compound having the basic unit shown in Formula I was synthesized using the following steps.

[0085] (mIm)2Zn was prepared by the following steps: Zn(NO3)2 (29.75 g, 0.1 mol) was weighed and dissolved in dimethylformamide to obtain a solution with a concentration of 0.05 M. 2-Methylimidazole (16.42 g, 0.2 mol) was weighed and dissolved in dimethylformamide to obtain a solution with a concentration of 0.1 M, and then a dimethylformamide solution of zinc nitrate was added dropwise to the solution, and then 20 g of a 2 wt% solution of a surfactant CTAB in dimethylformamide was added to the mixture, and the mixture was sealed and aged at 60°C for 24 h to obtain a solid product.

[0086] After the reaction, the solid product was recovered by filtration, washed three times with dimethylformamide, and then dried at 110°C overnight. The solid product was characterized by X-ray diffraction, and it was found that the 2θ peak signal of the substance had a corresponding characteristic peak at the target angle position, confirming the formation of the target structure. The elemental analysis was performed by inductively coupled plasma emission spectrometry (ICP), proving that its elemental composition was consistent with the expected elemental composition of the target product. The average particle size was measured by laser particle size analysis technology to be 0.8 μm. The micrograph of the solid product was taken by scanning electron microscope SEM, as shown in FIG. Figure 1 As shown, it can be observed that a periodic orderly assembled structure is formed. It is proved that the target product is formed, which has a periodic orderly assembled structure.

[0087] The materials shown in Table 1 below were prepared in the same manner as the above steps, wherein the raw material types and raw material ratios of the specific materials are summarized in Table 1, and the products were characterized by the same technology, and the characterization results of the obtained products are also summarized in Table 1. The SEM micrographs of all these products have the same Figure 1 Very similar periodic assembly structure.

[0088] Raw materials for metal cations and ligands Aging temperature (°C) ICP analysis XRD strong peak position Average particle size <![CDATA[(mIm)2Co]]> <![CDATA[Co(NO3)2∶mIm=1∶2]]> 70 The proportion of elements conforms to the chemical formula ~7°~13° 1μm <![CDATA[(bIm)2Zn]]> <![CDATA[Zn(NO3)2∶bIm=1∶2]]> 100 The proportion of elements conforms to the chemical formula ~7.5°~16° 0.5μm <![CDATA[(mIm)2Zn]]> <![CDATA[Zn(NO3)2∶mIm=1∶2]]> 60 The proportion of elements conforms to the chemical formula ~7°~13° 1μm (nbIm)(nIm)Zn <![CDATA[Zn(NO3)2∶nbIm∶nIm=1∶1∶1]]> 80 The proportion of elements conforms to the chemical formula ~7°~13° 0.75μm <![CDATA[(cbIm) 39 (OH)Zn 20 ]]> <![CDATA[Zn(NO3)2∶cbIm=1∶2]]> 120 The proportion of elements conforms to the chemical formula ~7°~13° 0.8μm

[0089] Example 2: Preparation of diaphragm

[0090] A PP-PE copolymer microporous film with a thickness of 16 μm purchased from Zhuogao Electronic Technology Co., Ltd. was used as the substrate layer, with an average pore size of 80 nm. The composite compound prepared in Example 1 of the same mass was used, and it was mixed evenly with a binder of polymethyl acrylate (produced by Hubei Nona Co., Ltd.), a binder of acrylic acid-acrylate-acrylonitrile copolymer (produced by Hubei Nona Co., Ltd.), a stabilizer of sodium carboxymethyl cellulose (chemically pure), and a wetting agent of polyoxyethylene ether (produced by Hubei Nona Co., Ltd.) in a ratio of 85:6:3:3:3, and water was added while mixing to form a water-based coating with a solid content of 9%. The slurry was applied to both surfaces of the substrate layer by a blade coating method, and a wet coating with a thickness of about 10 μm was formed on both surfaces, and then transferred to an oven and dried at a temperature of 80°C for 60 minutes to obtain a separator with a dry coating thickness of 2 μm. The separator obtained in this embodiment is named below according to the type of the composite compound used. The separator, battery cell and battery obtained are named according to the type of the composite compound used.

[0091] In addition, this embodiment also prepares three diaphragms in which the coatings contain both the composite compound of the present application and the inorganic oxide. Specifically, these diaphragms are also coated with the steps described above, with the only difference being that the composite compound in a specific weight proportion is replaced by alumina (Shandong Shuochuang, with an average particle size of approximately 1.5 μm). In the following text, such diaphragms and battery cells are written as 80% (mIm) 2Zn + 20% Al2O3, 51% (mIm) 2Zn + 49% Al2O3, and 20% (mIm) 2Zn + 80% Al2O3, respectively.

[0092] Example 3: Preparation of battery cells

[0093] The active substance Na 0.9 Fe 0.5 Mn 0.5 O2, conductive agent acetylene black (Denka, Denka Black), and binder polyvinylidene fluoride (Arkema, HSV 900) were fully stirred and mixed in an N-methylpyrrolidone solvent system in a weight ratio of 94:3:3 to obtain a slurry with a solid content of 30%. A transfer coating method was used to form a wet coating with a thickness of 250 μm on one side of an Al foil with a thickness of 12 μm. The resulting slurry was then transferred into an oven and dried at a temperature of 150°C for 60 minutes. The positive electrode sheet was cold pressed using a roller press at a pressure of 60 tons to obtain a positive electrode sheet, wherein the dry coating thickness on one side of the Al foil was 130 μm.

[0094] The active material hard carbon, the conductive agent acetylene black, the binder styrene-butadiene rubber and the thickener sodium carboxymethyl cellulose are fully stirred and mixed in a deionized water solvent system in a weight ratio of 95:2:2:1 to obtain a slurry with a solid content of 15%. The slurry is applied on one side of an Al foil with a thickness of 12 μm using a scraper to form a wet coating with a thickness of 120 μm. The slurry is then transferred into an oven and dried at a temperature of 150°C for 60 minutes. The negative electrode sheet is cold pressed using a cold press at a pressure of 50 tons to obtain a dry coating thickness on the Al foil of 60 μm.

[0095] The positive electrode sheet, the separator prepared in Example 2, and the negative electrode sheet were rolled up in order to form a wound laminate structure with a size of 16 cm×10 cm×2.8 cm. The bare cell was placed in a steel shell, 150 g of electrolyte was injected into it and packaged to obtain a cell, wherein the electrolyte was a PC solution composed of 1 M NaPF6.

[0096] Comparative Examples 1-4: Preparation of Comparative Separators and Cells

[0097] In Comparative Example 1, the microporous film described in Example 2 was directly used as a separator. In Comparative Examples 2-4, the steps of Example 2 were first repeated to prepare a separator, except that the composite compound of the present application was replaced by the same weight of aluminum hydroxide (Shandong Shuochuang, average particle size of about 0.6 μm), SAPO-34 (Taizhou Juna, average particle size of about 1.2 μm) and aluminum oxide (Shandong Shuochuang, average particle size of about 1.5 μm). These separators were used to manufacture battery cells in the same manner as in Example 3.

[0098] Example 4: Electrolyte affinity of the separator and characterization of the cell performance

[0099] In this embodiment, the following parameters are characterized: the porosity, electrolyte wettability, and electrolyte retention rate of the diaphragms prepared in Example 2 and Comparative Examples 1-4; the cell injection rate, rate performance, and cycle performance of the cells prepared in Example 3 and Comparative Examples 1-4.

[0100] The measurement technique of the membrane porosity is as follows :

[0101] Take a diaphragm prepared in Example 2 or Comparative Examples 1-4 with a size of 10 cm×10 cm×20 μm (the diaphragm of Comparative Example 1 has no coating formed on its surface, so its thickness is 16 μm), calculate its volume according to the size of the above diaphragm, and weigh the dry mass m of the diaphragm p , from which the dry density ρ of the diaphragm is calculated p The membrane was then immersed in n-butanol for 10 hours, and the wet weight of the membrane was measured. The mass m of n-butanol absorbed by the membrane was determined based on the difference between the wet weight and the dry weight. a , the density of n-butanol ρa The parameters are known, and the porosity of the diaphragm is calculated using the following formula based on the above parameters. It can be seen that the overall porosity takes into account the total porosity of the substrate layer and the coating layer at the same time, but when other components in the substrate layer and the coating layer of each different diaphragm remain unchanged, the total porosity very intuitively reflects the effect of the composite compound of the present application on the porosity of the diaphragm.

[0102] P=(m a / ρ a ) / (m a / ρ a +m p / ρ p )×100%

[0103] The electrolyte wettability measurement technology of the diaphragm is as follows :

[0104] Drop 1 drop (about 0.05 mL) of proton-type hydrophilic electrolyte with electrolyte (1M NaPF6 in ethylene carbonate (EC): ethyl methyl carbonate (EMC) = 1 / 1 W / W solution) onto the horizontally placed diaphragm prepared in Example 2 or Comparative Examples 1-4. After 5 minutes, use the grid method to count the approximate area of ​​electrolyte infiltration. Specifically, the grid method is measured as follows: After 5 minutes, take a picture of the upper surface of the diaphragm from directly above, and then use an area of ​​0.1 cm in the picture. 2 The squares cover all areas showing traces of electrolyte infiltration. The squares in the image completely occupied by traces of electrolyte infiltration are recorded as "completely infiltrated", and the squares with an electrolyte infiltration area equal to or greater than half are also recorded as "completely infiltrated", while the squares with an electrolyte infiltration area less than half are recorded as "non-infiltrated". Finally, the electrolyte wettability of the diaphragm is equal to the number of completely infiltrated squares × 0.1, expressed in square centimeters.

[0105] The measurement technology of electrolyte retention rate of diaphragm is as follows :

[0106] Take a diaphragm prepared in Example 2 or Comparative Examples 1-4 with a size of 10 cm×10 cm×20 μm (no coating is formed on the surface of the diaphragm of Comparative Example 1, so its thickness is 16 μm), weigh the dry weight W0 of the diaphragm, then soak the diaphragm in the electrolyte for 10 hours and let it stand in a sealed container for 1 hour to saturate the electrolyte in the diaphragm, then weigh the wet weight W of the diaphragm, and calculate its electrolyte retention rate based on the following formula. It can be seen that the electrolyte retention rate not only characterizes the capacity of the diaphragm to hold the electrolyte, but also reflects the diaphragm's ability to retain the electrolyte.

[0107] Electrolyte retention rate = [(W-W0) / W0] × 100%

[0108] The cell filling rate measurement technology is as follows :

[0109] The electrolyte is injected into the battery cells of Example 3 and Comparative Examples 1-4 by vacuum injection, and the time required for the electrolyte to fully transfer from a discrete state to the inside of the diaphragm, and then to the inside of the positive and negative electrodes to completely soak the battery cells is recorded. This is based on the premise that the resulting battery cells have normal performance (no performance drop due to insufficient electrolyte within 100 cycles).

[0110] The measurement technology of rate performance is as follows :

[0111] The battery cell was placed in the test channel of the Arbin electrochemical workstation and charged at a constant current of 0.1C to a charge cut-off voltage of 4V, and then charged at a constant voltage for 30 minutes. After that, it was discharged at a constant current at a rate of 0.1C and 1C to a discharge cut-off voltage of 2.5V, and the discharge capacity was recorded as 0.1C capacity and 1C capacity, respectively. Rate performance = 1C capacity / 0.1C capacity × 100%.

[0112] The measurement technique for cycle performance is as follows :

[0113] The battery cell was placed in the test channel of the Arbin electrochemical workstation, and charged at a constant current of 1C to a charge cut-off voltage of 4V. After standing for 5 minutes, it was discharged at a constant current of 1C to a discharge cut-off voltage of 2.5V, and the discharge capacity was recorded. Then it was allowed to stand for another 5 minutes. This cycle was repeated 100 times, and the cycle performance = 100th cycle capacity / 1st cycle capacity × 100%.

[0114] The measurement results of the electrolyte affinity and battery core performance of the separator of the present application are summarized in Table 2 below:

[0115] Table 2 The electrolyte affinity and cycle performance measurement results of the separator and battery cell of the present embodiment

[0116]

[0117] It can be seen from Table 2 above that although the diaphragms of all the embodiments and comparative examples have very similar porosities, the diaphragms provided in the embodiments of the present application exhibit excellent electrolyte wetting performance and electrolyte retention rate due to the presence of the composite compound provided in the embodiments of the present application in the surface coating, and the battery cells prepared using these diaphragms have significantly shortened injection rates and significantly improved rate performance and cycle performance.

[0118] Example 5: Characterization of expansion resistance, mechanical properties, etc. of the separator and battery cell

[0119] In this embodiment, the following technical means were used to characterize various properties of the separators and cells of the inventive embodiments and comparative examples obtained in embodiments 2-3 and comparative examples 1-4.

[0120] The measurement technique for battery expansion rate is as follows :

[0121] The cells obtained in Example 3 and Comparative Examples 1-4 of the present application were assembled into soft-pack batteries for charge and discharge tests, and 1000 ppm of water was added to the electrolyte to accelerate gas production. The volume of the battery before charge and discharge was tested using the drainage method, recorded as V1, and the volume of the battery after 100 cycles of charge and discharge was recorded as V2. The expansion rate of the battery P = (V2-V1) / V1×100%.

[0122] The testing technology of battery cell energy density is as follows:

[0123] Using the battery cells obtained in the above Example 3 and Comparative Examples 1-4 of the present application, the battery cells were charged at a constant current rate of 0.1C to a charging cut-off voltage of 4.0V and maintained at a constant voltage for 30 minutes, and then discharged at a constant current rate of 0.1C to a discharge cut-off voltage of 2.5V. The energy released during constant current discharge was recorded, and the energy density of the battery cell was obtained by dividing it by the overall mass of the battery cell.

[0124] The test techniques for areal density are as follows:

[0125] Using the separators obtained in the above Example 2 and Comparative Examples 1-4 of the present application, a square coated separator having a size of 10 cm*10 cm was weighed to obtain its mass, which was then divided by its area to obtain the surface density.

[0126] The test techniques for air permeability are as follows:

[0127] The membranes obtained in Example 2 and Comparative Examples 1-4 of the present application were used, and the air permeability of the membranes was measured using a Gurley 4110N permeameter, that is, the Gurley index of the time required for 100 mL of air to pass through the membrane.

[0128] The testing technique for peel strength is as follows

[0129] Use the diaphragm obtained in the above Example 2 and Comparative Examples 1-4 of the present application (the only difference is that the diaphragm used here is coated on one side), take a clean and flat diaphragm sample, cut the sample into 15mm×20mm strips, and at the same time cut the polyethylene terephthalate (PET) sheet substrate into 15mm×20mm strips, tightly bond the uncoated side of the diaphragm to the polyethylene terephthalate (PET) sheet base plane, and tightly bond it to the coated surface with 3M tape, use a tensile testing machine to fix one end of the above-mentioned pressed sample, hold the 3M tape at the other end, start the tensile testing machine, and the test result is the peel force (peel strength).

[0130] Table 3 Measurement results of battery expansion rate, battery cell energy density, surface density, air permeability and peel strength of the separator and battery cell of the embodiment of the present application

[0131]

[0132] It can be seen from Table 3 above that, compared with the comparative examples, the diaphragms provided in the embodiments of the present application exhibit improved surface density, air permeability and peel strength due to the presence of the composite compound provided in the embodiments of the present application in the surface coating, and the cells and batteries prepared using these diaphragms exhibit excellent properties of inhibiting battery expansion and excellent cell energy density.

[0133] Example 6: Characterization of the heat resistance, limiting oxygen index, ionic conductivity and other properties of the separator and battery cell

[0134] In this embodiment, the following technical means were used to characterize various properties of the separators and cells of the inventive embodiments and comparative examples obtained in embodiments 2-3 and comparative examples 1-4.

[0135] The testing techniques for heat resistance are as follows:

[0136] Using the diaphragm obtained in the above Example 2 and Comparative Examples 1-4 of the present application, the uniform and flat diaphragm sample was cut into 12cm*12cm, and the transverse direction (TD) and the longitudinal direction (MD) were marked respectively. Then, straight lines were drawn in the transverse and longitudinal directions respectively with a marker pen, and the lengths were measured with a vernier caliper, and the data were recorded; the sample was placed in a constant temperature and humidity chamber with a preset temperature, and kept warm for a specified time. Then, the constant temperature and humidity chamber was opened to take out the diaphragm sample, and it was placed for 15-20 minutes. The length of the drawn straight line was measured with a vernier caliper, and the data was recorded. The thermal shrinkage data in the transverse direction (TD) and the longitudinal direction (MD) were calculated based on the dimensional data recorded before and after the heat treatment.

[0137] The measurement technique for hot box testing is as follows :

[0138] Batteries were made using the cells obtained from Example 3 and Comparative Examples 1-4 of the present application. The batteries were stored at 150°C for 1 hour and then checked to see if they would cause explosion or bursting. Samples that passed the hot box test were marked as ○, while samples that exploded or burst were marked as ×.

[0139] The testing technique for the Limiting Oxygen Index is as follows:

[0140] Using the membranes obtained in Example 2 and Comparative Examples 1-4 of the present application, the sample was cut into strips with a width of 20 mm and a length of 200 mm, and several layers of strips were stacked to a thickness as close to 0.1 mm as possible. The stacked strips were wound into a roll using a winding rod, and the oxygen index was measured using a limiting oxygen index tester based on GB / T2406-93. The measurement result was the minimum oxygen concentration (volume percentage) required for the sample to just maintain combustion. The higher the value, the better the flame retardancy of the obtained membrane.

[0141] The testing techniques for ionic conductivity are as follows:

[0142] Using the diaphragms obtained in Example 2 and Comparative Examples 1-4 of the present application, based on the method of confined symmetrical cells, constant voltage AC impedance spectroscopy tests were performed on diaphragms with different numbers of layers using a Bio-logic electrochemical workstation. The intercept where the impedance curve and the real part intersect on the Nyquist plot is taken as Rs, and compared with the known Rs parameter of the standard conductivity sample to obtain the ionic conductivity.

[0143] Table 4 Measurement results of heat resistance, flame retardancy and ionic conductivity of the separator of the present embodiment

[0144]

[0145] It can be seen from the experimental results in Table 4 above that, compared with the comparative example, the diaphragm provided in the embodiment of the present application exhibits improved heat resistance, flame retardancy and excellent ionic conductivity due to the presence of the composite compound provided in the embodiment of the present application in the surface coating.

Claims

1. A diaphragm, comprising: a polymer substrate layer, and A coating applied to at least one surface of the polymer substrate layer, the coating comprising an organic-inorganic hybrid composite compound, wherein the organic-inorganic hybrid composite compound is composed of basic units represented by formula I periodically assembled along at least one spatial direction: L x (M a C b ) y ·A z Formula I In Formula I, M is a cation of one or more metals selected from the group consisting of Zn, Co, Cu, Fe, Cd, Mn, Ag, Rh, Ru, Be, Mg, Al, Sc, Cr, Ni, Y, Ti, Zr, Hf, Li, Na, K, In, Ca, Sr, Pb, lanthanide metals, actinide metals, and a is a value of 0.1-10; C is one or more atoms, atomic groups, small molecules or anions selected from the following: O, =O, O 2- , S 2- , Cl - Br - ,I - , CO, -OH, OH - , H2O, b is a value from 0 to 20; y is a value from 1 to 50; When M is cations of two or more metals, the product of a and y represents the number of all metal cations in the basic unit represented by the single formula I; L is one or more ligands selected from the following: imidazole, porphyrin, pyridine, pyrazole, pyrimidine, piperidine, pyrrolidine, furan, thiophene, piperazine, pyridazine, indole, quinoline, carbazole, morpholine, and salts, acid radicals, esters, amides, anhydrides, dimers and trimers of the above ligands, and one or more hydrogen atoms in the above ligands are optionally substituted by one or more substituents selected from the following: cyano, nitro, amino, aldehyde, carboxyl, halogen, C1-C8 alkyl, hydroxy C1-C8 alkyl, C1-C8 alkoxy, C2-C8 alkenyl, C2-C8 alkynyl, C3-C8 16 Cycloalkyl, C6-C 20 Aryl, C6-C 20 heteroaryl, or any combination thereof, x is a value from 1 to 50; A is an atom or cation of one or more metal elements selected from the group consisting of Li, Na, K, Rb, Cs, Be, Sr, Zn, Al, Mg and Ca, or is one or more molecules selected from the group consisting of H2, O2, H2O, CO2, NH3, CH4, methyl formate, ethyl acetate, propylene carbonate, and z is a value from 0 to 100.

2. The diaphragm according to claim 1, wherein In the organic-inorganic hybrid composite compound, the number of the basic units represented by Formula I periodically assembled along at least one spatial direction is an integer from 3 to 10,000.

3. The diaphragm according to claim 1, wherein 0.5≤x:y≤6; and / or When b is not zero, 0.5≤a:b≤8.

4. The diaphragm according to any one of claims 1 to 3, wherein The metal cation M, the ligand L and optionally C together constitute a basic unit, and the basic unit has pores. When z is not zero, A is located in the pores of the basic unit. The basic unit is periodically assembled along at least one spatial direction to form the organic-inorganic hybrid composite compound with a multi-mesoporous or multi-microporous structure.

5. The diaphragm according to any one of claims 1 to 3, wherein M is a cation of one or more metals selected from the group consisting of Co and Zn; and L is one or more ligands selected from the following: 2-methylimidazole (acid group / ester), benzimidazole (acid group / ester), 4-cyanoimidazole (acid group / ester), 5-chlorobenzimidazole (acid group / ester), 2-formaldehydeimidazole (acid group / ester) and 2-nitroimidazole (acid group / ester).

6. The diaphragm according to any one of claims 1 to 3, wherein The basic unit is selected from one or more of the following: (mIm)2Co, (mIm)2Zn, (bIm)2Zn, (cnIm)2[Zn], (cbIm)2 39 [Zn 20 (OH)], (cbIm)(nIm)Zn, (Ica)2Zn and (cbIm)2Zn.

7. The diaphragm according to any one of claims 1 to 3, wherein The coating further comprises one or more components selected from the group consisting of a binder, an inorganic particle, a stabilizer, a wetting agent, a rheology modifier, a defoamer, a thickener, a pH adjuster, and a preservative; and / or The coating further comprises inorganic particles selected from at least one of the following: boehmite, molecular sieves, zeolites, alumina, aluminum oxyhydroxide, silica, aluminum nitride, silicon carbide, MgO, CaO, ZnO, ZrO2, TiO2, and mixtures thereof; and / or The weight ratio of the organic-inorganic hybrid composite compound to the inorganic particles is 1:5 to 5:

1.

8. A battery comprising the separator according to any one of claims 1 to 7.

9. An electrical device, comprising the diaphragm according to any one of claims 1 to 7.

10. An electrical device, comprising the battery according to claim 8 or the electrical device according to claim 9.

11. A method for manufacturing the diaphragm according to any one of claims 1 to 7, the method comprising: providing a polymer substrate layer, and A coating layer including the organic-inorganic hybrid composite compound is formed on at least one surface of the polymer base material layer.

12. A method for improving the performance of a diaphragm, the method comprising: A polymer substrate layer is provided, and a coating layer comprising an organic-inorganic hybrid composite compound is formed on at least one surface of the polymer substrate layer, wherein the organic-inorganic hybrid composite compound is composed of basic units represented by formula I periodically assembled along at least one spatial direction: L x (M a C b ) y ·A z Formula I In Formula I, M is a cation of one or more metals selected from the group consisting of Zn, Co, Cu, Fe, Cd, Mn, Ag, Rh, Ru, Be, Mg, Al, Sc, Cr, Ni, Y, Ti, Zr, Hf, Li, Na, K, In, Ca, Sr, Pb, lanthanide metals, actinide metals, and a is a value of 0.1-10; C is one or more atoms, atomic groups, small molecules or anions selected from the following: O, =O, O 2- , S 2- , Cl - Br - ,I - , CO, -OH, OH - , H2O, b is a value from 0 to 20; y is a value from 1 to 50; When M is cations of two or more metals, the product of a and y represents the number of all metal cations in the basic unit represented by the single formula I; L is one or more ligands selected from the following: imidazole, porphyrin, pyridine, pyrazole, pyrimidine, piperidine, pyrrolidine, furan, thiophene, piperazine, pyridazine, indole, quinoline, carbazole, morpholine, and salts, acid radicals, esters, amides, anhydrides, dimers and trimers of the above ligands, and one or more hydrogen atoms in the above ligands are optionally substituted by one or more substituents selected from the following: cyano, nitro, amino, aldehyde, carboxyl, halogen, C1-C8 alkyl, hydroxy C1-C8 alkyl, C1-C8 alkoxy, C2-C8 alkenyl, C2-C8 alkynyl, C3-C8 16 Cycloalkyl, C6-C 20 Aryl, C6-C 20 heteroaryl, or any combination thereof, x is a value from 1 to 50; A is an atom or cation of one or more metal elements selected from the group consisting of Li, Na, K, Rb, Cs, Be, Sr, Zn, Al, Mg and Ca, or is one or more molecules selected from the group consisting of H2, O2, H2O, CO2, NH3, CH4, methyl formate, ethyl acetate, propylene carbonate, and z is a value from 0 to 100; The improved membrane performance is selected from at least one of the following: (1) Affinity of the diaphragm for the electrolyte; (2) The permeability, gas capacity and expansion resistance of the diaphragm; (3) Surface density, energy density and mechanical strength of the diaphragm; (4) Heat resistance, flame retardancy and explosion resistance of the diaphragm; (5) Ionic conductivity of the membrane; (6) The rate performance and cycle performance of the battery cell made using the separator.

13. Use of an organic-inorganic hybrid composite compound for improving the performance of a diaphragm, wherein the organic-inorganic hybrid composite compound is composed of basic units represented by formula I periodically assembled along at least one spatial direction: L x (M a C b ) y ·A z Formula I In Formula I, M is a cation of one or more metals selected from the group consisting of Zn, Co, Cu, Fe, Cd, Mn, Ag, Rh, Ru, Be, Mg, Al, Sc, Cr, Ni, Y, Ti, Zr, Hf, Li, Na, K, In, Ca, Sr, Pb, lanthanide metals, actinide metals, and a is a value of 0.1-10; C is one or more atoms, atomic groups, small molecules or anions selected from the following: O, =O, O 2- , S 2- , Cl - Br - ,I - , CO, -OH, OH - , H2O, b is a value from 0 to 20; y is a value from 1 to 50; When M is cations of two or more metals, the product of a and y represents the number of all metal cations in the basic unit represented by the single formula I; L is one or more ligands selected from the following: imidazole, porphyrin, pyridine, pyrazole, pyrimidine, piperidine, pyrrolidine, furan, thiophene, piperazine, pyridazine, indole, quinoline, carbazole, morpholine, and salts, acid radicals, esters, amides, anhydrides, dimers and trimers of the above ligands, and one or more hydrogen atoms in the above ligands are optionally substituted by one or more substituents selected from the following: cyano, nitro, amino, aldehyde, carboxyl, halogen, C1-C8 alkyl, hydroxy C1-C8 alkyl, C1-C8 alkoxy, C2-C8 alkenyl, C2-C8 alkynyl, C3-C8 16 Cycloalkyl, C6-C 20 Aryl, C6-C 20 heteroaryl, or any combination thereof, x is a value from 1 to 50; A is an atom or cation of one or more metal elements selected from the group consisting of Li, Na, K, Rb, Cs, Be, Sr, Zn, Al, Mg and Ca, or is one or more molecules selected from the group consisting of H2, O2, H2O, CO2, NH3, CH4, methyl formate, ethyl acetate, propylene carbonate, and z is a value from 0 to 100; The improved membrane performance is selected from at least one of the following: (1) Affinity of the diaphragm for the electrolyte; (2) The permeability, gas capacity and expansion resistance of the diaphragm; (3) Surface density, energy density and mechanical strength of the diaphragm; (4) Heat resistance, flame retardancy and explosion resistance of the diaphragm; (5) Ionic conductivity of the membrane; (6) The rate performance and cycle performance of the battery cell made using the separator.