A three-dimensional porous silicon-carbon composite material and its preparation method and application

Three-dimensional porous silicon-carbon composite materials are generated through pyrolysis of bacterial cellulose, which solves the problems of low conductivity and volume expansion of lithium-ion battery anode materials, achieves efficient electrochemical performance improvement and safety improvement, and is suitable for high-energy-density lithium-ion applications. Battery negative electrode material.

CN115849381BActive Publication Date: 2024-10-01ZHEJIANG XINAN CHEM IND GRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211447503.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-18
Publication Date
2024-10-01
Estimated Expiration
2042-11-18

AI Technical Summary

Technical Problem

Existing lithium-ion battery anode materials have low conductivity and severe volume expansion during charging and discharging, which hinders the industrialization of silicon-based anodes. In addition, traditional nano-silicon preparation methods have safety issues, high energy consumption, and poor electrochemical performance. Good question.

Method used

Using bacterial cellulose as the carbon source, a three-dimensional porous silicon-carbon composite material is generated through a pyrolysis process. Small particle size nano-silica is generated in situ to form a uniformly distributed three-dimensional network structure. Alkali metal carbonates are used to form a porous structure to alleviate the volume. expands and improves electrical conductivity.

Benefits of technology

It effectively reduces the volume expansion during charge and discharge and improves the electrochemical performance of the battery. The first Coulombic efficiency is ≥85%, and the capacity retention rate after 100 cycles is ≥90%. It also improves the safety of the material and production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003950947010000101
    Figure BDA0003950947010000101
Patent Text Reader

Abstract

The present invention relates to a three-dimensional porous silicon-carbon composite material and a preparation method and application thereof. The preparation method of the three-dimensional porous silicon-carbon composite material comprises: (1) dispersing silicon oxide and alkali metal carbonate in a solvent to obtain a mixed solution containing silicon oxide and alkali metal carbonate; (2) immersing a bacterial cellulose membrane in the mixed solution containing silicon oxide and alkali metal carbonate, and drying after completion; (3) heating the product obtained by drying in step (2) under a non-oxidizing atmosphere, and then naturally cooling to room temperature; (4) dispersing the product obtained in step (3) in a solvent, separating to obtain a solid product; (5) washing the product obtained in step (4) and drying. The method of the present invention is environmentally friendly and safe. The obtained three-dimensional porous silicon-carbon composite material can effectively reduce the volume expansion during the charge and discharge process while improving the conductivity of the material, thereby greatly improving the electrochemical performance of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium ion battery materials, and specifically relates to a three-dimensional porous silicon-carbon composite material and a preparation method and application thereof. Background Art

[0002] Lithium-ion batteries are widely used in consumer electronics, power and energy storage due to their excellent performance. The negative electrode material of commercial lithium-ion batteries is mainly graphite. The preparation technology of this negative electrode material is quite mature, but the capacity of graphite negative electrode is close to the theoretical capacity (372mAh / g). As the market demand for battery energy density increases significantly, there is an urgent need to develop lithium-ion batteries with higher energy density.

[0003] Developing high-capacity negative electrode materials is an effective way to improve the energy density of lithium-ion batteries. Among them, silicon negative electrode materials are one of the most promising negative electrode materials. The theoretical specific capacity of pure silicon negative electrode can reach 4200mAh / g, but silicon-based negative electrode materials have low conductivity and face serious volume expansion (300%) during charging and discharging, which has become a major obstacle to the industrialization of silicon-based negative electrodes. In order to alleviate or overcome the adverse effects of low conductivity and volume expansion of silicon-based negative electrodes, the electrochemical performance of silicon negative electrodes can be improved through various methods such as nano-sizing of silicon particles, carbon coating, and constructing special composite material structures.

[0004] At present, the methods for preparing nano silicon include high-energy ball milling, silane thermal decomposition, etc. Patent CN105655569A discloses a method for preparing ultrafine nano silicon powder, which grinds the coarse silicon powder once, mixes the primary grinding material with auxiliary materials for secondary ball milling, and finally obtains nano silicon powder through steps such as drying. The nano silicon powder obtained by this method has irregular particles, the particle size distribution cannot be effectively controlled, the production efficiency is low, and the energy consumption is high. Patent CN103936009A discloses a method for producing nano-scale high-purity silicon powder by thermal decomposition of silane, wherein silane is a flammable and explosive gas, which is not conducive to transportation and storage, and has extremely high safety requirements for the process and equipment.

[0005] Although nano-sizing silicon particles can alleviate the volume expansion of silicon negative electrode during the cycle to a certain extent, nano-silicon has a strong surface effect, which will lead to secondary agglomeration and accelerate the attenuation of capacity; and nano-silicon has a large specific surface area, which has more contact with the electrolyte, which is not conducive to improving the electrochemical performance of the material. Therefore, nano-silicon is generally not used alone as a negative electrode, and usually needs to be compounded with other materials (such as carbon materials). Carbon coating of silicon-based materials can build a conductive network while alleviating the volume change of silicon negative electrode materials and improve the conductive performance. Therefore, carbon-coated silicon composite materials have received great attention in recent years. However, the plastic strain of the carbon material as a coating layer cannot completely buffer the volume expansion of the silicon material caused by the composite material during the de-lithiation process, which finally causes the coating layer to rupture, the battery's first coulombic efficiency to decrease, and the long-term cycle performance to deteriorate. Therefore, it is necessary to study the carbon material with good plastic deformation to coat silicon particles, in which the three-dimensional network structure can effectively buffer the huge volume change caused by the de-lithiation process of silicon, and the network structure can provide a channel for the transmission of lithium ions.

[0006] Patent CN103000865A discloses a method for preparing carbon fiber-silicon nanowire negative electrode materials, including the preparation of silicon nanowires and the preparation of carbon fiber-silicon nanowire composite materials, wherein the preparation of silicon nanowires requires the use of flammable and explosive silane gas, and the preparation of composite materials requires long-term ball milling. In addition, the method uses silicon wafers as carriers to prepare silicon nanowires, which is not conducive to industrial production, has high requirements for equipment safety, and has high energy consumption in the preparation process. Patent CN103337612A discloses a nanoporous silicon-carbon composite material and a preparation method thereof, wherein the nanoporous silicon-carbon composite material is prepared by corroding a multi-element alloy. The method realizes the controllable preparation of a highly active nanoporous silicon-carbon composite material by free corrosion in a strong electrolyte solution. However, since it is difficult for metals and carbon-based materials to be evenly dispersed in the composite matrix, the resulting pore structure is not evenly distributed, and the conductive properties of the material cannot be improved.

[0007] In view of this, the present invention is proposed. Summary of the invention

[0008] In view of the defects of the prior art, the present invention provides a method for preparing a three-dimensional porous silicon-carbon composite material. The method is environmentally friendly and safe in the process of preparing nano-silicon, and can generate silicon nanoparticles in situ. At the same time, bacterial cellulose is used as a carbon source, which can form a good three-dimensional network structure during the pyrolysis process, disperse small-size silicon particles, not only inhibit the agglomeration of silicon during the charge and discharge process, but also improve the electronic conductivity of the composite material. The added alkali metal carbonate can make the material form a porous structure, leaving more space for the volume expansion of silicon. The three-dimensional porous silicon-carbon composite material prepared by the method of the present invention can effectively reduce the volume expansion during the charge and discharge process while improving the conductivity of the material, thereby greatly improving the electrochemical performance of the battery.

[0009] In order to achieve the technical effect, the technical solution of the present invention is as follows:

[0010] A method for preparing a three-dimensional porous silicon-carbon composite material comprises the following steps:

[0011] (1) dispersing silicon oxide and alkali metal carbonate in a solvent to obtain a mixed solution containing silicon oxide and alkali metal carbonate;

[0012] (2) immersing the bacterial cellulose membrane in a mixed solution containing silicon oxide and alkali metal carbonate, and drying after the immersion is completed;

[0013] (3) heating the product obtained by drying in step (2) under a non-oxidizing atmosphere, and then cooling naturally to room temperature;

[0014] (4) dispersing the product obtained in step (3) in a solvent and separating to obtain a solid product;

[0015] (5) washing the product obtained in step (4) and drying it.

[0016] As an example, the molar ratio of silicon oxide to alkali metal carbonate is 1:0.5-1.

[0017] As an example, in the mixed solution of step (1), the total mass concentration of silicon dioxide and alkali metal carbonate is 1-30%.

[0018] As an example, the median particle size of silicon oxide is 1-10 μm.

[0019] As an example, the thickness of the bacterial cellulose membrane is 0.5-3 mm, and the immersion time is 0.5-3 h.

[0020] As an example, the mass of the bacterial cellulose is 1-10 times the mass of silicon dioxide in step (1).

[0021] As an example, the alkali metal carbonate is one or more of lithium carbonate, sodium carbonate or potassium carbonate, preferably sodium carbonate.

[0022] As an example, the heating treatment in step (3) is performed at a temperature of 600-1100° C. for a time of 2-10 h.

[0023] Optionally, the separation method in step (4) is one of suction filtration, centrifugation, filter pressing or filtration.

[0024] Optionally, the drying method is vacuum drying or drying in a protective atmosphere, supercritical drying, or freeze drying.

[0025] As an example, the dispersion method in step (1) is any one of stirring, ultrasound or ball milling.

[0026] Optionally, the non-oxidizing atmosphere includes any one of nitrogen, argon or helium.

[0027] The present invention provides a three-dimensional porous silicon-carbon composite material, which is obtained according to any one of the preparation methods described above.

[0028] The present invention provides a lithium ion battery, wherein the negative electrode material of the lithium ion battery comprises the three-dimensional porous silicon-carbon composite material.

[0029] The lithium-ion battery provided by the present invention uses the three-dimensional porous silicon-carbon composite material as the active material, and mixes the active material, the binder, and the conductive agent in a mass ratio of 8:1:1 to form a slurry, and then coats it on a copper foil, vacuum-dries it at 120°C for 12 hours, and then rolls it into a negative electrode sheet. A metal lithium sheet is used as a counter electrode, and the electrolyte is a mixed solvent of EC and DMC in which LiPF6 is dissolved, and 5% FEC is added, wherein LiPF6 is 1 mol / L and the volume ratio of EC:DMC is 1:1. The battery is assembled into a button cell in an argon atmosphere, and when the charge and discharge voltage range is 0.01-2.0V, the first efficiency obtained by testing is ≥85%, and the capacity retention rate after 100 cycles is ≥90%.

[0030] Compared with the prior art, the present invention has the following advantages:

[0031] (1) The preparation method of the present invention produces small-particle nano-silicon by heat treatment to cause silicon oxide to undergo a disproportionation reaction (2SiO=Si+SiO2). Compared with the traditional ball milling method or silane thermal decomposition method, the method is safer, more environmentally friendly, and has a low cost.

[0032] (2) The bacterial cellulose used in the preparation method of the present invention has a unique three-dimensional nano-network structure, and the three-dimensional network structure can be well preserved after pyrolysis, has better plastic deformation, and can better resist the volume expansion of silicon during the charging and discharging process;

[0033] Furthermore, by adsorbing silicon dioxide and alkali metal carbonates using bacterial cellulose membranes and then pyrolyzing them, nanosilicon can be evenly dispersed in the voids of the three-dimensional network carbon material, thereby effectively alleviating the volume expansion of the silicon-based material during the charging and discharging process. The obtained carbon fiber network is also beneficial to improving the electrical conductivity of the material. The in-situ method for generating nanosilicon of the present invention avoids the problem of nanosilicon agglomeration, thereby improving the electrochemical performance of the battery.

[0034] (3) Furthermore, the preparation method of the present invention uses inorganic sodium carbonate as a pore-forming agent. The sodium carbonate reacts with the silicon dioxide produced in the disproportionation process during the pyrolysis process (Na2CO3+SiO2=Na2O·SiO2+CO2↑). After the preparation is completed, the pore-forming agent can be removed by washing with water, without the need to use strong acidic substances such as hydrofluoric acid.

[0035] The removal of silica further increases the porosity in the final product, providing more buffer space for the silicon component to expand. DETAILED DESCRIPTION

[0036] The bacterial cellulose described in the present invention includes any one or a mixture of cellulose synthesized by a certain microorganism in the genus Acetobacter, Agrobacterium, Rhizobium or Sarcina, but is not limited to the bacterial cellulose listed above. Other bacterial cellulose commonly used in the art can also be used in the present invention.

[0037] In order to test the application performance of the three-dimensional porous silicon-carbon composite material prepared by the present invention in a lithium-ion battery, as an example, the three-dimensional porous silicon-carbon composite material of each embodiment is assembled into a lithium-ion battery according to the following method:

[0038] The three-dimensional porous silicon-carbon composite material was uniformly mixed with a binder CMC and SBR and a conductive agent SP in a mass ratio of 8:1:1 to prepare a slurry, which was then coated on a copper foil and vacuum dried at 120° C. for 12 hours before being rolled to form a negative electrode sheet.

[0039] The above-mentioned negative electrode sheets were used as test electrodes, the metal lithium sheet was used as the counter electrode, and the electrolyte was LiPF6 (1 mol / L) / EC:DMC (volume ratio 1:1), and button cells were assembled in a glove box filled with argon.

[0040] It should be noted that the above content is not intended to improperly limit the application scope of the three-dimensional porous silicon-carbon composite material of the present invention to the above-mentioned battery structure, but is only used as a demonstration of the test effect.

[0041] The electrolyte LiPF6 (1 mol / L) / EC:DMC (volume ratio 1:1) means: the electrolyte is LiPF6 / EC:DMC, wherein LiPF6 is 1 mol / L, the volume ratio of EC:DMC is 1:1, EC is ethylene carbonate, and DMC is dimethyl carbonate.

[0042] Example 1

[0043] 1) Weigh 4.5 g of silicon dioxide with a median particle size of 5 μm and 5.5 g of sodium carbonate, add them into 100 mL of deionized water under ultrasonic assistance (ultrasonic frequency is 40 KHZ), and continue ultrasonication for 30 minutes to obtain a silicon dioxide-sodium carbonate dispersion;

[0044] 2) 25 g of bacterial cellulose membrane was immersed in a silicon oxide and sodium carbonate dispersion for 1 hour. After adsorption, the residual liquid on the surface was rinsed with deionized water, and the membrane was frozen in a -20°C refrigerator for 24 hours, and then freeze-dried in a freeze drying oven for 12 hours;

[0045] 3) The product in step 2 was pyrolyzed at 800° C. for 6 h in a nitrogen atmosphere and then naturally cooled to room temperature.

[0046] 4) The pyrolysis product of step 3 was dispersed in 100 mL of deionized water, and then centrifuged to obtain a solid substance, which was pre-frozen in a -20°C refrigerator for 24 hours, and then freeze-dried in a cold dryer at -60°C for 12 hours to obtain a three-dimensional porous silicon-carbon composite material.

[0047] Example 2

[0048] 1) Weigh 5.7 g of silicon dioxide with a median particle size of 3 μm and 10.3 g of sodium carbonate, then add them into 80 mL of deionized water for ball milling (300 rpm / min, 0.5 h) to obtain a silicon dioxide-sodium carbonate dispersion;

[0049] 2) 30 g of bacterial cellulose membrane was immersed in a silicon oxide and sodium carbonate dispersion for 1.5 h. After the adsorption was completed, the residual liquid on the surface was rinsed with deionized water and freeze-dried.

[0050] 3) The product of step 2 was pyrolyzed at 800° C. for 6 h in a nitrogen atmosphere and naturally cooled to room temperature.

[0051] 4) The pyrolysis product of step 3 was dispersed in 100 mL of deionized water, and then filtered to obtain a solid substance. After pre-freezing in a -20°C refrigerator for 24 hours, it was freeze-dried in a cold dryer at -60°C for 12 hours to obtain a three-dimensional porous silicon-carbon composite material.

[0052] Example 3

[0053] 1) Weighing 4.8 g of silicon dioxide with a median particle size of 3 μm and 8.7 g of sodium carbonate, and then adding them into 90 mL of deionized water with the aid of stirring to uniformly disperse them to obtain a silicon dioxide-sodium carbonate dispersion;

[0054] 2) 26 g of bacterial cellulose membrane was immersed in a silicon oxide and sodium carbonate dispersion for 1 hour. After adsorption, the residual liquid on the surface was washed with water, and the membrane was pre-frozen in a -20°C refrigerator for 24 hours, and then freeze-dried in a cold dryer at -60°C for 12 hours;

[0055] 3) pyrolyzing the product of step 2 at 900° C. for 4 h in an argon atmosphere, and naturally cooling to room temperature;

[0056] 4) The pyrolysis product of step 3 was dispersed in 100 mL of deionized water, and then centrifuged to obtain a solid substance, which was vacuum dried at 50° C. to obtain a three-dimensional porous silicon-carbon composite material.

[0057] Example 4

[0058] 1) Weigh 10 g of silicon dioxide with a median particle size of 5 μm and 15 g of sodium carbonate, and then mix them in 100 mL of deionized water, and then ultrasonicate the solution at a frequency of 40 KHZ for 0.5 h to obtain a silicon dioxide-sodium carbonate dispersion;

[0059] 2) 50 g of bacterial cellulose membrane was immersed in a silicon oxide and sodium carbonate dispersion for 2 hours. After adsorption, the residual liquid on the surface was rinsed with deionized water, and the membrane was pre-frozen in a -20°C refrigerator for 24 hours, and then freeze-dried in a cold dryer at -60°C for 12 hours;

[0060] 3) pyrolyzing the product of step 2 at 900° C. for 4 h in a nitrogen atmosphere, and naturally cooling to room temperature;

[0061] 4) The pyrolysis product of step 3 was dispersed in 100 mL of deionized water, and then centrifuged to obtain a solid substance, which was vacuum dried at 50° C. to obtain a three-dimensional porous silicon-carbon composite material.

[0062] Example 5

[0063] 1) Weigh 5.5 g of silicon dioxide with a median particle size of 5 μm and 8 g of sodium carbonate, and then disperse them in 90 mL of deionized water, and then stir the solution (300 rpm / min, 2 h) to obtain a silicon dioxide-sodium carbonate dispersion;

[0064] 2) 29 g of bacterial cellulose membrane was immersed in a silicon oxide and sodium carbonate dispersion for 1 hour. After adsorption, the residual liquid on the surface was rinsed with deionized water, and the membrane was pre-frozen in a -20°C refrigerator for 24 hours, and then freeze-dried in a cold dryer at -60°C for 12 hours;

[0065] 3) pyrolyzing the product in step 2 at 1000° C. for 4 h under an argon atmosphere and cooling naturally to room temperature;

[0066] 4) The pyrolysis product of step 3 is dispersed in 100 mL of deionized water, and then filtered to obtain a solid substance, which is freeze-dried to obtain a three-dimensional porous silicon-carbon composite material.

[0067] Example 6

[0068] 1) Weigh 9 g of silicon dioxide with a median particle size of 3 μm and 11 g of sodium carbonate, and then disperse them in 100 mL of deionized water, and then ball mill the solution (250 rpm, 0.5 h) to obtain a silicon dioxide-sodium carbonate dispersion;

[0069] 2) 48 g of bacterial cellulose membrane was immersed in a silicon oxide and sodium carbonate dispersion for 2 h. After adsorption, the residual liquid on the surface was rinsed with deionized water, and the membrane was pre-frozen in a -20°C refrigerator for 24 h, and then freeze-dried in a cold dryer at -60°C for 12 h;

[0070] 3) pyrolyzing the product of step 2 at 900° C. for 4 h in an argon atmosphere, and naturally cooling to room temperature;

[0071] 4) The pyrolysis product of step 3 was dispersed in 100 mL of deionized water, and then centrifuged to obtain a solid substance, which was freeze-dried to obtain a three-dimensional porous silicon-carbon composite material.

[0072] Comparative Example 1

[0073] 1) 5.4 g of silicon dioxide with a median particle size of 5 μm is dispersed in 100 mL of deionized water to obtain a silicon dioxide dispersion;

[0074] 2) 30 g of bacterial cellulose membrane was immersed in silicon oxide dispersion. After adsorption, the residual liquid on the surface was rinsed with deionized water and freeze-dried (pre-frozen in a -20°C refrigerator for 24 hours, and then freeze-dried in a cold dryer at -60°C for 12 hours).

[0075] 3) The product in step 2 was pyrolyzed at 1000° C. for 3 h under an argon atmosphere and naturally cooled to room temperature.

[0076] 4) The pyrolysis product of step 3 is dispersed in deionized water, and then filtered to obtain a solid substance, which is freeze-dried to obtain a three-dimensional silicon-carbon composite negative electrode material.

[0077] Comparative Example 2

[0078] 1) 4.5 g of silicon dioxide with a median particle size of 3 μm is dispersed in 90 mL of deionized water to obtain a silicon dioxide dispersion;

[0079] 2) 25 g of bacterial cellulose membrane was immersed in silicon oxide dispersion. After adsorption, the residual liquid on the surface was rinsed with deionized water and freeze-dried (pre-frozen in a -20°C refrigerator for 24 hours, and then freeze-dried in a cold dryer at -60°C for 12 hours);

[0080] 3) The product of step 2 was pyrolyzed at 900° C. for 4 h in a nitrogen atmosphere and then naturally cooled to room temperature.

[0081] 4) The pyrolysis product of step 3 is dispersed in deionized water, and then centrifuged to obtain a solid substance, which is freeze-dried to obtain a three-dimensional silicon-carbon composite negative electrode material.

[0082] Test example

[0083] The three-dimensional porous silicon-carbon composite materials of Examples 1-6 of the present invention and the materials of Comparative Examples 1-2 were respectively used as active materials, and the active materials, binders CMC and SBR, and conductive agent SP were uniformly mixed in a mass ratio of 8:1:1 to form a slurry, which was then coated on a copper foil and vacuum dried at 120°C for 12 hours before being rolled to form a negative electrode sheet.

[0084] The above-mentioned negative electrode sheets were used as test electrodes, the metal lithium sheet was used as the counter electrode, and the electrolyte was LiPF6 (1 mol / L) / EC:DMC (volume ratio 1:1), and button cells were assembled in a glove box filled with argon.

[0085] The battery performance test was carried out on a Xinwei battery tester with a charge and discharge voltage range of 0.01-2.0V. The test data are shown in Table 1.

[0086] Table 1

[0087]

[0088] As shown in Table 1, the batteries made of the negative electrode materials of Examples 1-6 have higher specific capacity and initial efficiency than the batteries made of the negative electrode materials of Comparative Examples 1-2, and the electrochemical performance of the negative electrode materials is significantly improved, with the capacity retention rate after 100 cycles being above 90%.

Claims

1. A method for preparing a three-dimensional porous silicon-carbon composite material, characterized in that: The following steps are involved: (1) dispersing silicon oxide and alkali metal carbonate in a solvent to obtain a mixed solution containing silicon oxide and alkali metal carbonate; (2) immersing the bacterial cellulose membrane in a mixed solution containing silicon oxide and alkali metal carbonate, and drying after the immersion is completed; (3) heating the product obtained by drying in step (2) under a non-oxidizing atmosphere, and then cooling naturally to room temperature; (4) dispersing the product obtained in step (3) in a solvent and separating to obtain a solid product; (5) washing the product obtained in step (4) and drying it to obtain; Wherein, the molar ratio of silicon oxide to alkali metal carbonate is 1:0.5-1; In the mixed solution of step (1), the total mass concentration of silicon dioxide and alkali metal carbonate is 1-30%; the median particle size of silicon dioxide is 1-10 μm; The mass of the bacterial cellulose is 1-10 times the mass of silicon dioxide in step (1); the thickness of the bacterial cellulose film is 0.5-3 mm, and the immersion time is 0.5-3 h; The heating treatment temperature in step (3) is 600-1100° C. and the time is 2-10 h; The alkali metal carbonate is sodium carbonate.

2. The method for preparing the three-dimensional porous silicon-carbon composite material according to claim 1, characterized in that: The separation method in step (4) is one of suction filtration, centrifugation, filter pressing or filtration.

3. The method for preparing the three-dimensional porous silicon-carbon composite material according to claim 1, characterized in that: The drying method is vacuum drying, drying in a protective atmosphere, supercritical drying, or freeze drying.

4. The method for preparing the three-dimensional porous silicon-carbon composite material according to claim 1, characterized in that: The dispersion method in step (1) is any one of stirring, ultrasound or ball milling.

5. The method for preparing the three-dimensional porous silicon-carbon composite material according to claim 1, characterized in that: The non-oxidizing atmosphere includes any one of nitrogen, argon or helium.

6. A three-dimensional porous silicon-carbon composite material, characterized in that: Obtained according to the preparation method according to any one of claims 1 to 5.

7. A lithium ion battery, characterized in that: The negative electrode material of the lithium-ion battery comprises the three-dimensional porous silicon-carbon composite material according to claim 6.

8. The lithium-ion battery according to claim 7, characterized in that: The three-dimensional porous silicon-carbon composite material is used as the active material, the active material, the binder and the conductive agent are mixed uniformly in a mass ratio of 8:1:1 to prepare a slurry, and then coated on a copper foil, vacuum dried at 120°C for 12 hours and then rolled to form a negative electrode sheet, a metal lithium sheet is used as the counter electrode, the electrolyte is a mixed solvent of ethylene carbonate and dimethyl carbonate dissolved with LiPF6, and 5% of the total mass of the electrolyte is added with fluoroethylene carbonate, wherein LiPF6 is 1 mol / L and the volume ratio of ethylene carbonate: dimethyl carbonate is 1:1, and button batteries are assembled in an argon atmosphere, and when the charge and discharge voltage range is 0.01-2.0V, the first efficiency obtained by testing is ≥85%, and at the same time, the capacity retention rate after 100 cycles is ≥90%.