Electrolyte and battery
By using a combination of azaborane complex additives and negative electrode film-forming additives in the electrolyte, a stable interface film is formed, which solves the problem of oxidative decomposition reaction and poor compatibility of the battery under high pressure, and significantly improves the high voltage resistance of the battery. features and safety features.
Patent Information
- Application Number
- CN202111117804.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-23
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-09-23
AI Technical Summary
Existing batteries are prone to oxidative decomposition reactions under high pressure, resulting in increased battery impedance, bulging, and metal dissolution of the positive active material, shortening battery life and increasing safety risks. Moreover, conventional electrolytes have poor compatibility with graphite negative electrodes, making it difficult to form a stable interface. membrane.
Add azaborane complex additives to the electrolyte, combined with negative electrode film-forming additives, to form a stable solid electrolyte interface and cathode film formation, reduce the lowest unoccupied molecular orbital energy of the azaborane complex additives, and give priority to the positive electrode The surface forms a stable cathode-electrolyte interface, reducing side reactions and preventing the structural collapse of the cathode active material through the chelating structure.
It significantly improves the high-voltage resistance characteristics, cycle performance and safety performance of the battery, extends the battery life, reduces the dissolution of the positive active material, and improves the battery performance under high temperature and high pressure.
Smart Images

Figure CN115863740B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of battery electrolytes, and in particular to an electrolyte and a battery. Background Art
[0002] At present, high potential positive electrode materials are widely used in lithium-ion batteries due to their high voltage resistance, high capacity, and high energy density. The more common ones are ternary positive electrode materials. The charging cut-off voltage of ternary positive electrode active materials is generally 4.5V (vs. Li / Li + ) or above, but conventional electrolytes are prone to oxidative decomposition reactions at a voltage of 4.5V, which leads to a sharp increase in battery impedance, battery swelling, and accelerated metal dissolution of positive electrode active materials, seriously shortening the battery life and increasing safety hazards.
[0003] Although replacing the electrolyte organic solvent with a stronger antioxidant can improve the battery's high-voltage resistance, it has poor compatibility with the graphite negative electrode and will affect the physicochemical properties of the electrolyte system, thereby affecting the battery performance; introducing negative electrode film-forming additives into the conventional electrolyte system can also improve the battery's high-voltage resistance to a certain extent, but it is difficult to form a stable CEI film (cathode-electrolyte interface) on the surface of the positive electrode active material, and the improvement of the battery cycle performance (especially high-voltage cycle performance) is limited. Summary of the invention
[0004] In view of this, the present application provides an electrolyte, which, on the basis of the negative electrode film-forming additive, also adds a specific nitrogen-borane complex additive. The electrolyte can make the battery have good high-voltage resistance, excellent high-temperature and high-voltage cycle performance and high safety performance, and the electrolyte has good compatibility with various battery systems.
[0005] Specifically, the first aspect of the present application provides an electrolyte, which includes a lithium salt, an organic solvent, a negative electrode film-forming additive, and an azaborane complex additive as shown in (I):
[0006]
[0007] In formula (I), R1, R2, R3, and R4 are each independently selected from one or more of a hydrogen atom, an isocyanate group, an isothiocyanate group, a nitrile group, an aliphatic group, an aromatic group, an aliphatic group containing a substituent, and an aromatic group, wherein the substituent includes one or more of a halogen atom, an amino group, a hydroxyl group, an ester group, an alkoxy group, an isocyanate group, an isothiocyanate group, an acyl group, and a nitrile group.
[0008] The electrolyte provided in the first aspect of the present application, on the basis of the negative electrode film-forming additive, is further added with an azaborane complex additive. The synergistic electron donating effect of phenyl and azaborane in this type of complex additive can reduce the LUMO (lowest unoccupied molecular orbital) of the azaborane complex additive. According to the frontier orbital theory, the azaborane complex additive has a higher reduction potential. Therefore, it can take precedence over the organic solvent (such as ethylene carbonate EC) and the negative electrode film-forming additive in the electrolyte to undergo electrochemical reduction polymerization at the negative electrode of the battery, quickly forming a dense and stable SEI film (solid electrolyte interface), and cooperating with the SEI film formed on the negative electrode surface by the subsequent negative electrode film-forming additive, thereby stabilizing the negative electrode / electrolyte interface.
[0009] The synergistic electron-donating effect of the phenyl group and azaborane inherent in the structure of the present invention can further increase the electron cloud density of the complex additive, and make the complex additive contain more free electrons, which is more likely to be oxidized before the organic solvent, thereby preferentially forming a stable CEI film on the positive electrode surface, reducing the side reaction between the positive electrode active material and the electrolyte, and extending the battery life. In addition, the azaborane complex additive can effectively chelate a large amount of Ni formed by the positive electrode of the battery during the charge and discharge process. 4+ The chelate formed has a stable structure and can attach to the oxidation active sites on the positive electrode surface, forming a steric hindrance between the electrolyte and the electrode surface, thereby preventing the positive electrode from dissolving Ni 4+ , reducing the structural collapse of the positive electrode active material, improving its structural stability, and thus improving the safety performance and cycle performance of the battery (especially the cycle performance under high temperature and high pressure). In addition, the complex additive and the chelate formed have good compatibility with the carbonate system electrolyte and will not affect the physicochemical properties of the parent electrolyte.
[0010] In the embodiment of the present application, R1, R2, R3, and R4 can be independently selected from one or more of hydrogen atoms, isocyanate groups (-NCO), isothiocyanate groups (-NCS), nitrile groups (-CN), aliphatic groups, and aromatic groups, wherein the substituents include one or more of halogen atoms, amino groups, hydroxyl groups (-OH), ester groups (-COOR), acyl groups (-COR), alkoxy groups (-OR), isocyanate groups, isothiocyanate groups, and nitrile groups. Among them, the aliphatic groups include alkyl groups with 1-10 carbon atoms, alkenyl groups or alkynyl groups with 2-10 carbon atoms, and cycloalkyl groups with 3-10 carbon atoms; the aryl groups have 6-30 carbon atoms. The halogen atoms may include fluorine atoms (F), chlorine atoms (Cl), bromine atoms (Br), and iodine atoms (I). The amino groups may include primary amino groups (-NH2), secondary amino groups (or alkylamino groups, -NHR), and tertiary amino groups (or dialkylamino groups, -NRR'). It should be noted that the carbon chain of the above-mentioned substituents containing multiple carbon atoms (ie, ester group, secondary amino group, tertiary amino group, alkoxy group, acyl group) should not be too long to ensure that the viscosity of the azaborane complex additive is within an appropriate range.
[0011] In some specific embodiments of the present application, the structural formula of the azaborane complex additive can be any one of the following formulas (J)-(P):
[0012]
[0013]
[0014] Among them, the additive represented by formula (J) specifically refers to 1,3-dimethyl-2-phenyl-2,3-dihydro-1H-benzo[d][1,3,2]diazaborine. The additive represented by formula (K) specifically refers to phenyl-2,3-dihydro-1H-benzo[d][1,3,2]diazaborine. The additive represented by formula (L) specifically refers to isocyanate-1-methyl-3-propyl-2,3-dihydro-1H-benzo[d][1,3,2]diazaborine. The additive represented by formula (M) specifically refers to 1-ethyl-3-methyl-1H-benzo[d][1,3,2]diazaborine-2(3H)-carbonitrile. The additive represented by formula (N) specifically refers to 2-(2,6-dimethylphenyl)-1-ethyl-3-methyl-2,3-dihydro-1H-benzo[d][1,3,2]diazaborine. The additive represented by formula (O) specifically refers to 1-phenyl-2-(2,6-dimethylphenyl)-2,3-dihydro-1H-benzo[d][1,3,2]diazaborin. The additive represented by formula (P) specifically refers to 1-ethyl-2-(2-methylprop-1-en-1-yl)-2,3-dihydro-1H-benzo[d][1,3,2]diazaborin.
[0015] In some embodiments of the present application, R1 is phenyl, m-dimethylphenyl, isocyanate or nitrile, R2 is hydrogen, methyl, ethyl, propyl or phenyl, R3 is hydrogen or methyl, and R4 is hydrogen. In the above structure, the synergistic electron-donating effect of each substituent group, phenyl and azaborane can further increase the number of free electrons in the structure, making it easier to be oxidized, quickly forming a stable CEI film on the positive electrode surface, reducing the side reaction between the positive electrode active material and the electrolyte, and extending the battery life.
[0016] In the embodiment of the present application, the mass percentage of the azaborane complex additive is 0.1%-10% based on the mass of the electrolyte. In the presence of the negative electrode film-forming additive, an appropriate amount of the azaborane complex additive can preferentially form an interface film on the positive and negative electrode surfaces of the battery, and thereafter, the negative electrode film-forming additive will also form another layer of SEI film on the negative electrode surface, and the two cooperate with each other on the negative electrode surface to further optimize the interface composition between the battery negative electrode and the electrolyte, thereby stabilizing the electrode / electrolyte interface.
[0017] In the embodiment of the present application, the negative electrode film-forming additive includes one or more of fluoroethylene carbonate (FEC), vinyl ethylene carbonate (VC), vinyl sulfite (ES), methylene disulfonate (MMDS), vinyl carbonate (VEC), styrene carbonate, styrene carbonate, 1,3-propylene sulfonate (PST), and dithiothreitol (DTD), preferably FEC. FEC can form a thin but stable low-impedance SEI film on the negative electrode surface, and has a good coordination effect with the SEI film formed by the azaborane complex additive at the negative electrode.
[0018] In the embodiment of the present application, based on the mass of the electrolyte, the mass fraction of the negative electrode film-forming additive is 0.1%-10%, preferably 3%.
[0019] In the embodiment of the present application, the azaborane complex additive is 3%-300% of the mass of the negative electrode film-forming additive. When the content of the azaborane complex additive is too high, it is easy to cause the CEI or SEI film on the surface of the battery electrode to be too thick, resulting in an increase in battery impedance, and excessive azaborane complex additives will remain in the electrolyte, impairing the performance of the battery. If the content of the azaborane complex additive is too low, the improvement effect on the electrolyte is poor.
[0020] In the embodiment of the present application, the electrolyte further comprises propylene sulfite (PS). PS is used in combination with the azaborane complex additive provided in the present application to further improve the high voltage resistance, high temperature and high voltage cycle performance and safety performance of the battery.
[0021] In the embodiment of the present application, the organic solvent includes a cyclic carbonate and a linear carbonate in a mass ratio of 1-2.5; wherein the cyclic carbonate includes ethylene carbonate (EC), and the linear carbonate includes one or more of diethyl carbonate (DEC), dimethyl carbonate (DMC), and methyl ethyl carbonate (EMC). The dielectric constant of the cyclic carbonate is high, and the viscosity of the linear carbonate is low. The combination of the two is conducive to improving the ionic conductivity of the electrolyte. In addition, the cyclic carbonate can also participate in the formation of the SEI film, thereby effectively preventing the occurrence of negative electrode side reactions. Exemplarily, the organic solvent is a mixture of ethylene carbonate and diethyl carbonate, and the mass ratio of the two is 3:7.
[0022] In the embodiment of the present application, the lithium salt includes lithium hexafluorophosphate (LiPF6), and the molar concentration of the lithium hexafluorophosphate is 0.1mol / L-1.2mol / L, preferably 1mol / L, based on the electrolyte. Lithium hexafluorophosphate has the best overall performance as an organic solvent for the electrolyte. More preferably, the lithium salt also includes lithium bis(fluorosulfonyl)imide (LiFSI) or lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), and the above two lithium salts are used as additives. The fluorine content of such lithium salts is low and hydrofluoric acid is not easily produced. A small amount of the above lithium salt is added to the electrolyte, which is beneficial to improving the high temperature resistance of the electrolyte. At the same time, lithium bis(fluorosulfonyl)imide can also form a film at the negative electrode of the battery to enhance the stability of the SEI film.
[0023] The electrolyte provided in the first aspect of the present application contains an azoborane complexing additive and a negative electrode film-forming additive. Under the synergistic effect of the two, a stable interface film can be preferentially formed on the surface of the positive and negative electrode materials of the battery at the same time, and a large amount of Ni generated during battery operation can be chelated. 4+ , and it has good compatibility with various battery systems, thus ensuring that the battery has good high-voltage resistance, excellent high-temperature and high-voltage cycle performance and high safety performance.
[0024] The second aspect of the present application provides a battery, wherein the electrolyte provided in the first aspect of the present application is built in the battery. The battery containing the electrolyte has good high-voltage resistance, excellent high-temperature and high-voltage cycle performance, and good safety.
[0025] Specifically, the battery includes a battery shell and a battery cell and an electrolyte contained in the battery shell, wherein the battery cell includes a positive electrode sheet, a negative electrode sheet and a separator located between the positive electrode sheet and the negative electrode sheet, and the electrolyte is as described in the first aspect of the present application.
[0026] The preparation method of the battery comprises: stacking a positive electrode sheet, a separator and a negative electrode sheet in sequence to form a battery core, accommodating the battery core in a battery shell, injecting the above electrolyte, and then sealing the battery shell to obtain the battery.
[0027] Among them, the negative electrode sheet, the positive electrode sheet, and the separator are all conventional choices in the battery field. For example, the positive electrode sheet includes a positive electrode current collector and a positive electrode material layer disposed on the positive electrode current collector, wherein the positive electrode material layer includes a positive electrode active material, a positive electrode binder, and an optional conductive agent. The positive electrode active material includes a ternary nickel-manganese-cobalt material, such as Li 0.33 Ni 0.33 Co 0.33 MnO2(NCM111), Li 0.4 Ni 0.2 Co 0.4 MnO2(NCM424), Li 0.5 Ni 0.2 Co 0.3 MnO2(NCM523), Li 0.6 Ni 0.2 Co 0.2 MnO2(NCM622), Li 0.8 Ni 0.1 Co 0.1 MnO2(NCM811), Li 0.85 Ni 0.075 Co 0.075 MnO2, nickel-cobalt-aluminum ternary materials, lithium iron phosphate, lithium cobalt oxide, lithium-rich manganese-based materials, etc. The negative electrode sheet includes a negative electrode current collector and a negative electrode material layer disposed on the negative electrode current collector, wherein the negative electrode material layer may include a negative electrode active material, a negative electrode binder, and an optional conductive agent. For example, the negative electrode active material includes graphite, natural graphite, mesophase carbon microbeads (MCMB), silicon-carbon negative electrode materials, etc.
[0028] Advantages of the embodiments of the present application will be partially explained in the following description, and some will be obvious from the description, or can be learned through the implementation of the embodiments of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 1 is the cyclic voltammetry curve of the battery of Example 2 and Comparative Example 1 of the present application. DETAILED DESCRIPTION
[0030] The embodiments of the present application are further described below with reference to a plurality of embodiments.
[0031] Example 1
[0032] A method for preparing a lithium ion battery, comprising:
[0033] a) Prepare an electrolyte, the preparation method of which is as follows: In a glove box, mix 60g of organic solvent ethylene carbonate (EC) and 140g of diethyl carbonate (DEC) to obtain a mixed solvent. Add 30g of lithium hexafluorophosphate (LiPF6) to the mixed solvent, and the concentration of LiPF6 in the mixed solvent is 1mol / L. Then add 7.1g of negative electrode film-forming additive fluoroethylene carbonate (FEC) and a certain amount of azoborane film-forming additive 1,3-dimethyl-2-phenyl-2,3-dihydro-1H-benzo[d][1,3,2]diazaborane, stir until all solid substances are completely dissolved, and obtain the desired electrolyte, wherein the content of each azoborane complexing additive is shown in Table 1.
[0034] b) preparing a positive electrode sheet, the preparation method of which is as follows: 100 parts of the ternary nickel-manganese-cobalt material Li 0.5 Ni0.2Co 0.3 MnO2 (NCM523) was mixed with 2 parts of carbon nanotubes, 1 part of conductive agent Super-p, and 2 parts of polyvinylidene fluoride (PVDF) into a uniform paste, which was evenly coated on the positive electrode current collector aluminum foil and vacuum dried at 80°C for 24 hours to obtain a positive electrode sheet.
[0035] c) preparing a negative electrode sheet, the preparation method of which is as follows: 100 parts of graphite material, 1 part of conductive agent Super-p, 1.5 parts of thickener sodium carboxymethyl cellulose (CMC) and 2.5 parts of styrene-butadiene rubber (SBR) are mixed into a uniform paste, evenly coated on the negative electrode current collector copper foil, and vacuum dried at 80° C. for 24 hours to obtain a negative electrode sheet.
[0036] d) The assembly and formation of the battery, the steps are as follows: in an argon glove box with a water content of less than 5ppm, the above-mentioned positive electrode sheet, separator and negative electrode sheet are stacked in order, wound into a bare battery cell, the bare battery cell is loaded into a battery shell and welded, and then 1.6g of the above-mentioned electrolyte is injected into the battery shell, and the battery shell is sealed to make a SL582736 lithium-ion battery. The above-mentioned battery is first charged to 1.5V with a current of 40mA (0.05C) and maintained at 1.5V for 10h to fully wet the battery electrode sheet. After the constant voltage is completed, the battery is initially charged with a smaller current of 8mA (C / 100) for 10h to form a stable and dense SEI film, and then charged to 4.35V with a current of 40mA (0.05C), and then discharged to 3.0V. The battery prepared in Example 1 is recorded as S1.
[0037] According to the battery manufacturing method provided in Example 1, the electrolytes and batteries of Examples 2-5 were respectively manufactured according to the ratios in Table 1, and the batteries of Examples 2-5 were respectively recorded as S1-S5.
[0038] Example 6
[0039] The electrolyte was prepared by referring to the method of Example 1. The difference between Example 6 and Example 2 is that 1% of propylene sulfite (PS) was also added to the electrolyte of Example 6. The battery preparation and formation process were the same as in Example 1, and a soft-pack battery S6 was prepared.
[0040] According to the battery manufacturing method provided in Example 1, the electrolytes and batteries of Examples 7-10 were manufactured respectively according to the ratios in Table 1, and the batteries of Examples 7-10 were recorded as S7-S10.
[0041] Table 1 Composition of additives in the battery electrolyte of each embodiment
[0042]
[0043]
[0044] In order to highlight the beneficial effects of the embodiments of the present application, the following comparative examples 1-2 are provided.
[0045] Comparative Example 1
[0046] An electrolyte was prepared in the same manner as in Example 1, except that the electrolyte of Example 1 did not contain negative electrode film-forming additive FEC and azaborane complexing additive. The battery preparation and formation process were the same as in Example 1, and a soft-pack battery DS1 was prepared.
[0047] Comparative Example 2
[0048] The electrolyte was prepared in the same manner as in Example 1, except that the electrolyte of Example 2 did not contain a nitrogen-borane complexing additive. The battery preparation and formation process were the same as in Example 1, and a soft-pack battery DS2 was prepared.
[0049] Performance Testing
[0050] The lithium ion batteries prepared according to the above examples 1-10 and comparative examples 1-2 were respectively subjected to the following tests:
[0051] Battery expansion rate test: Charge batteries S1-10, DS1 and DS2 at 0.5C (400mA) with a cut-off voltage of 4.5V, and then charge at a constant voltage of 4.5V with a cut-off current of 40mA to obtain fully charged batteries. Store the fully charged batteries in a 60°C constant temperature oven for 5 days, 10 batteries for each condition, and take the average value of the results. Use a vernier caliper to measure the thickness of the battery before and after storage, subtract the thickness before storage from the thickness after storage, and divide the thickness difference by the thickness before storage to obtain a percentage that is recorded as the battery expansion rate.
[0052] Nickel element dissolution test: After disassembling the battery that has completed the battery expansion rate test, repeatedly rinse the positive and negative electrode separators and aluminum plastic film with 5mL of dichloromethane, and then send the washing liquid to the inductively coupled plasma spectrometer (ICP) for testing. The test instrument is the Thermo Fisher inductively coupled ion spectrometer, and the test conditions are familiar to general testers. 10 batteries are tested under each condition, and the results are averaged to record the amount of nickel element dissolution in the positive electrode.
[0053] Battery high voltage cycle test: Remove the airbags of S1-S10 and DS1, DS2 batteries and seal them in vacuum, then place them in a 25℃ constant temperature box, and perform charge and discharge cycles 200 times at a current of 1C (800mA) between 2.75V and 4.5V, and divide the discharge capacity of each battery at the 300th cycle by the initial discharge capacity of the first cycle to obtain the percentage as the capacity retention rate. Among them, 10 samples of each battery were taken, and the results were averaged.
[0054] The performance test results of each battery are shown in Table 2 below.
[0055] Table 2 Performance test results of each battery
[0056] Battery ID Battery expansion rate (%) Nickel dissolution from positive electrode (ppm) Capacity retention rate (%) S1 59.2 6.8 42.3 S2 20.8 2.2 65.3 S3 21.2 1.7 68.2 S4 22.4 2.0 67.5 S5 56.1 5.8 41.7 S6 14.7 1.0 85.2 S7 21.3 1.8 69.3 S8 20.9 1.4 67.9 S9 21.8 1.9 70.1 S10 21.1 1.6 69.8 DS1 88.9 12.9 31.1 DS2 80.3 9.1 38.9
[0057] From the results in Table 2, it can be seen that the batteries S1-S10 prepared by Examples 1-10 of the present application, compared with the batteries DS1 and DS2 prepared by the comparative examples, have a good high-voltage capacity retention rate, less nickel dissolution in the battery positive electrode, and a low expansion rate. In addition, S1 has too low an amount of azaborane complex additive added (less than 01.%, reaching the lower limit defined in the present application), and S5 has too high an amount of azaborane complex additive added (more than 10%, reaching the upper limit defined in the present application), so their various performances have declined, but they are still better than comparative examples DS1 and DS2. Compared with other examples, Example S6 also adds propylene sulfite (PS), and the various performance improvements of the battery are more obvious.
[0058] In addition, the reduction potential test was performed on the electrolytes in Example 1 and Comparative Example 2. The test results are as follows: Figure 1 As shown. Figure 1 It can be seen that the 1,3-dimethyl-2-phenyl-2,3-dihydro-1H-benzo[d][1,3,2]diazaborane in Example 1 exhibits a reduction peak at about 1.2 V, while the electrolyte of Comparative Example 2 does not show a reduction peak at this potential. This indicates that the azaborane complexing additive provided in the examples of the present application can be reduced to form a SEI film at the negative electrode in preference to the carbonate solvent.
[0059] It can be seen that the nitrogen-borane complex additive provided in the present application does not affect the physicochemical properties of the parent electrolyte within a suitable addition range, can significantly reduce the expansion rate of the ternary battery during high-temperature storage at full charge, improve the safety performance of the ternary battery at high temperature, and at the same time reduce the dissolution of metallic nickel during high-temperature storage of the battery, thereby improving the capacity retention rate of the ternary battery during the cycle at a high voltage of 4.5V.
[0060] The above is an exemplary embodiment of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made thereto without departing from the principles of the present application. These improvements and modifications are also considered to be within the scope of protection of the present application.
Claims
1. An electrolyte, characterized in that: The electrolyte includes a lithium salt, an organic solvent, a negative electrode film-forming additive, and an azaborane complexing additive as shown in formula (I): In formula (I), R1, R2, R3, and R4 are each independently selected from one or more of a hydrogen atom, an isocyanate group, an isothiocyanate group, a nitrile group, an aliphatic group, an aromatic group, an aliphatic group containing a substituent, and an aromatic group; wherein the substituent includes one or more of a halogen atom, an amino group, a hydroxyl group, an alkoxy group, an ester group, an isocyanate group, an isothiocyanate group, an acyl group, and a nitrile group; The negative electrode film-forming additive includes one or more of fluoroethylene carbonate, vinyl ethylene carbonate, vinyl sulfite, methylene methanedisulfonate, vinyl carbonate, styrene carbonate, styrene vinyl carbonate, 1,3-propylene sultone, and vinyl sulfate.
2. The electrolyte according to claim 1, characterized in that The aliphatic group includes an alkyl group having 1 to 10 carbon atoms, an alkenyl group or an alkynyl group having 2 to 10 carbon atoms, and a cycloalkyl group having 3 to 10 carbon atoms; the aryl group has 6 to 30 carbon atoms.
3. The electrolyte according to claim 1, characterized in that The R1 is a phenyl group, a m-dimethylphenyl group, an isocyanate group or a nitrile group, the R2 is a hydrogen atom, a methyl group, an ethyl group, a propyl group or a phenyl group, the R3 is a hydrogen atom or a methyl group, and the R4 is a hydrogen atom.
4. The electrolyte according to claim 1, characterized in that The mass percentage of the azaborane complex additive in the electrolyte is 0.1%-10%.
5. The electrolyte according to claim 1, characterized in that The mass percentage of the negative electrode film-forming additive in the electrolyte is 0.1%-10%.
6. The electrolyte according to claim 1, characterized in that The mass of the azaborane complex additive is 3%-300% of the mass of the negative electrode film-forming additive.
7. The electrolyte according to claim 1, characterized in that The organic solvent comprises a cyclic carbonate and a linear carbonate in a mass ratio of 1-2.5; wherein the cyclic carbonate comprises ethylene carbonate, and the linear carbonate comprises one or more of diethyl carbonate, dimethyl carbonate, and methyl ethyl carbonate.
8. The electrolyte according to claim 1, characterized in that The electrolyte also includes propylene sulfite.
9. The electrolyte according to claim 1, characterized in that The lithium salt includes lithium hexafluorophosphate, and the molar concentration of the lithium hexafluorophosphate in the electrolyte is 0.1 mol / L-1.2 mol / L.
10. A battery, wherein the electrolyte according to any one of claims 1 to 9 is built in the battery.