Electrolyte and secondary battery containing the same
By using zwitterionic compounds with specific structures and electrolytes of lithium difluorodioxalate dioxalate in lithium ion batteries, the problem of poor kinetics and high-temperature storage performance of nickel-manganate lithium phosphate in lithium ion batteries is solved, and the problem of poor kinetics and high-temperature storage performance in lithium ion batteries is achieved. Excellent dynamic performance and high temperature storage performance of the battery.
Patent Information
- Application Number
- CN202411104238.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-13
AI Technical Summary
The kinetic properties and high-temperature storage performance of nickel-manganese oxide positive electrode materials in lithium-ion batteries are poor, and existing electrolyte solvents such as fluorogenic compounds have a negative impact on the battery cell system.
An electrolyte including a compound and lithium difluorodioxalate is used, which is a zwitterionic compound of a specific structure. By combining it with lithium difluorodioxalate, the dynamic performance and high-temperature storage performance of the battery are improved.
This electrolyte gives lithium-ion batteries excellent kinetic performance and high-temperature storage performance, improving the safety and stability of the battery.
Smart Images

Figure SMS_9 
Figure SMS_11 
Figure SMS_12
Abstract
Description
Technical Field
[0001] The present application relates to the field of power storage, and in particular to an electrolyte and a secondary battery containing the electrolyte. Background Art
[0002] With the increasing depletion of fossil energy and the increasing pressure of environmental pollution, the automotive industry is in urgent need of a new type of energy to drive it. Lithium-ion batteries stand out due to their high energy density, no memory effect, and high operating voltage, making them the preferred power source for new energy vehicles. However, with the expansion of market demand for electronic products and the development of power and energy storage equipment, people's requirements for lithium-ion batteries are constantly increasing, and the development of lithium-ion batteries with high energy density has become a top priority. The energy density of lithium-ion batteries is determined by capacity and platform voltage, but high capacity and high platform voltage can lead to chemical, structural and thermodynamic instability of active materials, posing a major challenge to safety.
[0003] Lithium nickel manganese oxide (LNMO) has attracted widespread attention as the next generation of high energy density lithium-ion battery positive electrode material. It has low processing cost, high energy density, and high platform voltage, which can meet the needs of high energy density and long battery life. The high voltage of LNMO has led to the existing technical solutions using fluorinated compounds as electrolyte solvents to solve the problem of narrow electrochemical redox window of electrolytes. However, fluorinated compounds have a large viscosity, and their introduction will have a negative impact on the dynamics of the LNMO battery system, and it will also affect the storage performance of the LNMO battery system at high temperatures. Therefore, it is necessary to develop an electrolyte that can improve the dynamics and storage performance of LNMO batteries at high temperatures. Summary of the invention
[0004] This application is mainly to solve the problem of poor kinetic performance and high temperature storage performance of lithium nickel manganese oxide positive electrode materials when used in lithium ion batteries in the prior art, and provides an electrolyte and a secondary battery containing the same. When the electrolyte provided by this application is used in a secondary battery, the secondary battery has excellent kinetic performance and high temperature storage performance.
[0005] To solve the above technical problems, this application provides the following solutions:
[0006] In a first aspect, the present application provides an electrolyte comprising a compound and lithium difluorobisoxalate phosphate;
[0007] The compound includes a compound represented by the following formula I:
[0008] Formula I;
[0009] Among them, A is selected from an alkyl group having 1-3 carbon atoms or an alkenyl group having 2-3 carbon atoms; R1 is any one selected from an alkyl group having 1-3 carbon atoms, an alkenyl group having 2-5 carbon atoms, an ester group having 1-3 carbon atoms, a carbonyl-containing substituent having 1-3 carbon atoms and a hydrogen atom.
[0010] In a second aspect, the present application provides a secondary battery comprising the electrolyte as described above.
[0011] On the basis of conforming to the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present application.
[0012] The reagents and raw materials used in this application are commercially available.
[0013] The positive effects of this application are:
[0014] The present application provides an electrolyte containing a zwitterionic compound and lithium difluorobisoxalate phosphate, wherein the combination of the zwitterionic compound and lithium difluorobisoxalate phosphate has a good synergistic effect, and the zwitterionic compound can promote the decomposition of lithium difluorobisoxalate phosphate, so that the secondary battery prepared by using the electrolyte has excellent kinetic performance and high-temperature storage performance. At the same time, the secondary battery prepared by using the electrolyte also has excellent safety performance. DETAILED DESCRIPTION
[0015] In the electrolyte described in the present application, a compound and lithium difluorobisoxalate phosphate are included;
[0016] The compound includes a compound represented by the following formula I:
[0017] Formula I;
[0018] Among them, A is selected from an alkyl group having 1-3 carbon atoms or an alkenyl group having 2-3 carbon atoms; R1 is any one selected from an alkyl group having 1-3 carbon atoms, an alkenyl group having 2-5 carbon atoms, an ester group having 1-3 carbon atoms, a carbonyl-containing substituent having 1-3 carbon atoms and a hydrogen atom.
[0019] Electrolyte
[0020] The electrolyte of the present invention is suitable for secondary batteries, and generally comprises an electrolyte, a solvent and an additive. When the secondary battery is a lithium ion battery, the electrolyte is a lithium salt; when the secondary battery is a sodium ion battery, the electrolyte is a sodium salt.
[0021] In some embodiments, the mass content of the lithium difluorobis(oxalate)phosphate in the electrolyte is 0.1%-3%.
[0022] In some preferred embodiments, the mass content of the lithium difluorobis(oxalate)phosphate in the electrolyte is 0.5%-1%.
[0023] In some specific embodiments, the mass content of the lithium difluorobis(oxalate)phosphate in the electrolyte is 0.05%, 0.2%, 0.3%, 0.5%, 1% or 3.5%.
[0024] In some embodiments, the mass content of the compound represented by Formula I in the electrolyte is 0.1%-3%.
[0025] In some preferred embodiments, the mass content of the compound represented by formula I in the electrolyte is 0.5-1%.
[0026] In other preferred embodiments, the mass content of the compound represented by formula I in the electrolyte is 0.2%-1%.
[0027] In some specific embodiments, the mass content of the compound represented by Formula I in the electrolyte is 0.05%, 0.3%, 0.5%, 1% or 3.5%.
[0028] In some embodiments, the compound represented by Formula I is:
[0029] Formula I-1;
[0030] Here, R1 is any one selected from an alkyl group having 1 to 3 carbon atoms, an alkenyl group having 2 to 5 carbon atoms, an ester group having 1 to 3 carbon atoms, a carbonyl-containing substituent having 1 to 3 carbon atoms, and a hydrogen atom.
[0031] In some embodiments, the compound represented by Formula I is selected from at least one of the following compounds:
[0032] , , , .
[0033] In a specific embodiment, the compound represented by formula I is compound 1, the mass content of lithium difluorobis(oxalyl)phosphate in the electrolyte is 0.1%, and the mass content of the compound in the electrolyte is 0.1%.
[0034] In a specific embodiment, the compound represented by formula I is compound 1, the mass content of lithium difluorobisoxalate phosphate in the electrolyte is 0.5%, and the mass content of the compound in the electrolyte is 0.1%.
[0035] In a specific embodiment, the compound represented by formula I is compound 1, the mass content of lithium difluorobisoxalate phosphate in the electrolyte is 0.3%, and the mass content of the compound in the electrolyte is 0.1%.
[0036] In a specific embodiment, the compound represented by formula I is compound 1, the mass content of lithium difluorobisoxalate phosphate in the electrolyte is 0.3%, and the mass content of the compound in the electrolyte is 0.5%.
[0037] In a specific embodiment, the compound represented by formula I is compound 1, the mass content of lithium difluorobisoxalate phosphate in the electrolyte is 0.2%, and the mass content of the compound in the electrolyte is 0.3%.
[0038] In a specific embodiment, the compound represented by formula I is compound 1, the mass content of lithium difluorobisoxalate phosphate in the electrolyte is 1%, and the mass content of the compound in the electrolyte is 0.3%.
[0039] In a specific embodiment, the compound represented by formula I is compound 1, the mass content of lithium difluorobisoxalate phosphate in the electrolyte is 3%, and the mass content of the compound in the electrolyte is 0.3%.
[0040] In a specific embodiment, the compound represented by formula I is compound 1, the mass content of lithium difluorobisoxalate phosphate in the electrolyte is 0.5%, and the mass content of the compound in the electrolyte is 1%.
[0041] In a specific embodiment, the compound represented by formula I is compound 1, the mass content of lithium difluorobisoxalate phosphate in the electrolyte is 0.5%, and the mass content of the compound in the electrolyte is 3%.
[0042] In a specific embodiment, the compound represented by formula I is compound 2, the mass content of lithium difluorobisoxalate phosphate in the electrolyte is 1%, and the mass content of the compound in the electrolyte is 0.3%.
[0043] In a specific embodiment, the compound represented by formula I is compound 3, the mass content of lithium difluorobisoxalate phosphate in the electrolyte is 1%, and the mass content of the compound in the electrolyte is 0.3%.
[0044] In a specific embodiment, the compound represented by formula I is compound 4, the mass content of lithium difluorobisoxalate phosphate in the electrolyte is 1%, and the mass content of the compound in the electrolyte is 0.3%.
[0045] In a specific embodiment, the compound represented by formula I is compound 1, the mass content of lithium difluorobisoxalate phosphate in the electrolyte is 0.05%, and the mass content of the compound in the electrolyte is 0.3%.
[0046] In a specific embodiment, the compound represented by formula I is compound 1, the mass content of lithium difluorobisoxalate phosphate in the electrolyte is 3.5%, and the mass content of the compound in the electrolyte is 0.3%.
[0047] In a specific embodiment, the compound represented by formula I is compound 1, the mass content of lithium difluorobisoxalate phosphate in the electrolyte is 1%, and the mass content of the compound in the electrolyte is 0.05%.
[0048] In a specific embodiment, the compound represented by formula I is compound 1, the mass content of lithium difluorobisoxalate phosphate in the electrolyte is 1%, and the mass content of the compound in the electrolyte is 3.5%.
[0049] In some embodiments, the electrolyte further includes a first additive including one or more of vinyl sulfate, 1,3-propane sultone, vinylene carbonate, and propenyl-1,2-sultone.
[0050] In some specific embodiments, the mass content of the first additive in the electrolyte is 3%-7%.
[0051] In some embodiments, the electrolyte further comprises a second additive, wherein the second additive comprises a compound as shown in Formula II,
[0052] Formula II.
[0053] In some specific embodiments, the mass content of the second additive in the electrolyte is 0.3%-2%.
[0054] In certain embodiments, the electrolyte further comprises an organic solvent conventionally used in the art, and the organic solvent may be any non-aqueous solvent used for non-aqueous electrolytes to date. Examples include, but are not limited to, linear or cyclic carbonates, such as ethylene carbonate, propylene carbonate, diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, dipropyl carbonate, fluoroethylene carbonate; ethers, such as 1,2-dimethoxyethane, 1,2-diethoxyethane, γ-butyrolactone, tetrahydrofuran, 2-methyltetrahydrofuran, 1,3-dioxolane, 4-methyl-1,3-dioxolane, diethyl ether; sulfones, such as cyclopentane sulfone, methylcyclopentane sulfone; nitriles, such as acetonitrile, propionitrile; esters, such as acetate, propionate, butyrate, etc. These non-aqueous solvents may be used alone or in combination.
[0055] In some embodiments, the electrolyte further comprises fluoroethylene carbonate, and the mass content of the fluoroethylene carbonate is 10%-30%.
[0056] In some embodiments, the electrolyte further comprises a fluorinated chain carbonate, wherein the fluorinated chain carbonate comprises one or more of trifluoroethyl methyl carbonate and bistrifluoroethyl carbonate, and the mass content of the fluorinated chain carbonate is 20%-75%. In a specific embodiment, the organic solvent is fluoroethylene carbonate and trifluoroethyl methyl carbonate, and the mass ratio of the fluoroethylene carbonate to the trifluoroethyl methyl carbonate is 3:7.
[0057] In certain embodiments, the electrolyte can be prepared by the following preparation method: the electrolyte is prepared in a glove box, the nitrogen content in the glove box is 99.999%, the actual oxygen content in the glove box is 0.1ppm, and the moisture content is 0.1ppm; the organic solvent is mixed evenly, and lithium difluorobis(oxalyl)phosphate, the compound shown in Formula I, the first additive and the second additive are added and mixed evenly.
[0058] positive electrode
[0059] In certain embodiments, the positive electrode includes a positive electrode active material layer including a positive electrode active material.
[0060] Among them, the positive electrode active material can be a positive electrode active material conventionally used for lithium ion battery positive electrode in the art, and the positive electrode active material can include but is not limited to one or more of lithium iron phosphate, lithium iron manganese phosphate, lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide and lithium nickel manganese oxide, for example, lithium nickel manganese oxide.
[0061] In a specific embodiment, the chemical formula of the lithium nickel manganese oxide is LiNi 0.5 Mn 1.5O4.
[0062] In some embodiments, the positive electrode active material layer further includes a conductive agent.
[0063] Among them, the type of the conductive agent is not particularly limited, and can be selected from graphite materials such as natural graphite and artificial graphite, carbon black SP, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black and other carbon black materials, carbon fibers, metal fibers and other conductive fibers, metal powders such as carbon fluoride powder, aluminum powder, nickel powder and other metal powders, zinc oxide, potassium titanate and other conductive whiskers, and titanium dioxide and other conductive metal oxides or polyphenylene derivatives.
[0064] In some embodiments, the positive electrode active material layer further includes a binder.
[0065] Among them, the type of the binder is not particularly limited, and can be selected from polyvinylidene fluoride, polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose, starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer and its sulfonate, styrene-butadiene rubber, fluororubber and various copolymers.
[0066] In some embodiments, the positive electrode active material layer further includes a thickener, such as sodium carboxymethyl cellulose.
[0067] In some embodiments, the positive electrode includes a positive electrode current collector, and the positive electrode active material layer is disposed on at least one surface of the positive electrode current collector.
[0068] Among them, the positive electrode current collector is a substrate supporting the positive electrode active material layer, which is usually a metal foil with a thickness of 3μm-500μm. There is no special restriction on the material, as long as it has high conductivity and does not produce chemical reactions in the secondary battery system. For example, it can be a foil formed after surface treatment of nickel, titanium, aluminum, nickel, silver, stainless steel, carbon, etc. The positive electrode current collector usually has a smooth surface, but fine lines can also be formed on its surface to increase the adhesion between the positive electrode active material and the current collector. In addition to the foil, the positive electrode current collector can also be used in any one or more combinations of various forms such as film, mesh, porous, foam or non-woven fabric. Generally, the positive electrode current collector is aluminum foil.
[0069] In the present application, the positive electrode can be prepared by conventional methods in the art, generally including: fully stirring and mixing the components of the positive electrode material layer in a solvent to obtain a positive electrode slurry, coating the positive electrode slurry on a positive electrode collector, drying, cold pressing, and slitting.
[0070] negative electrode
[0071] In certain embodiments, the negative electrode includes a negative electrode active material layer, and the negative electrode active material layer includes a negative electrode active material.
[0072] Among them, as the negative electrode active material, a compound that can reversibly embed and deintercalate lithium can be used. Specific examples of negative electrode active materials include but are not limited to: carbon materials such as crystalline carbon (natural graphite and artificial graphite, etc.), amorphous carbon, carbon-coated graphite and resin-coated graphite, or oxide materials such as indium oxide, silicon oxide, tin oxide, lithium titanate, zinc oxide, lithium oxide, etc., and can also be lithium metal or a metal material that can form an alloy with lithium; wherein the metal material that can form an alloy with lithium is, for example, Cu, Sn, Si, Co, Mn, Fe, Sb and Ag. Binary or ternary alloys containing these metals and lithium can also be used as negative electrode active materials. These negative electrode active materials can be used alone or in combination of two or more. From the perspective of high energy density, carbon materials such as graphite can also be used in combination with Si, Si alloys, Si oxides and other Si-based materials.
[0073] In some embodiments, the negative electrode active material includes any one of soft carbon, hard carbon, artificial graphite, natural graphite, silicon, silicon oxides, silicon carbon compounds, or lithium titanate, or a combination of at least two thereof.
[0074] In some embodiments, the negative electrode active material layer further includes a conductive agent.
[0075] Among them, the type of the conductive agent is not particularly limited, and can be selected from graphite materials such as natural graphite and artificial graphite, carbon black SP, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black and other carbon black materials, carbon fibers, metal fibers and other conductive fibers, metal powders such as carbon fluoride powder, aluminum powder, nickel powder and other metal powders, zinc oxide, potassium titanate and other conductive whiskers, and titanium dioxide and other conductive metal oxides or polyphenylene derivatives.
[0076] In some embodiments, the negative electrode active material layer further includes a binder.
[0077] Among them, the type of the binder is not particularly limited, and can be selected from polyvinylidene fluoride, polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose, starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer and its sulfonate, styrene-butadiene rubber, fluororubber and various copolymers.
[0078] In some embodiments, the negative electrode active material layer further includes a thickener, such as sodium carbon methyl cellulose.
[0079] In some embodiments, the negative electrode includes a negative electrode current collector, and the negative electrode active material layer is disposed on at least one surface of the negative electrode current collector.
[0080] Among them, the negative electrode current collector is a substrate supporting the negative electrode active material, usually a metal foil with a thickness of 3μm-500μm. There is no special restriction on the material, as long as it has high conductivity and does not produce chemical reactions in the secondary battery system. For example, it can be a foil formed after surface treatment of nickel, titanium, aluminum, nickel, silver, stainless steel, carbon, etc. The negative electrode current collector usually has a smooth surface, but fine lines can also be formed on its surface to increase the adhesion between the positive electrode active material and the current collector. In addition to the foil, the negative electrode current collector can also be used in any one or more combinations of various forms such as film, mesh, porous, foam or non-woven fabric. Generally, the negative electrode current collector is copper foil.
[0081] In the present application, the negative electrode can be prepared by conventional methods in the art, generally including: fully stirring and mixing the components of the negative electrode material layer in a solvent to obtain a negative electrode slurry, coating the negative electrode slurry on a negative electrode current collector, drying, cold pressing, and cutting.
[0082] Diaphragm
[0083] The separator set between the positive electrode and the negative electrode uses an insulating film with high ion permeability and high mechanical strength. The typical thickness of the separator is 9μm-18μm; the pore size is 5μm-300μm; the air permeability is 180s / 100mL-380s / 100mL; the porosity is 30% to 50%. As a separator, a sheet or non-woven fabric made of the following substances is usually used: an olefin polymer such as polypropylene or polyethylene; or, further, the aforementioned sheet or non-woven fabric is used as a base film and coated with a coating (such as a nano-alumina coating).
[0084] In a specific embodiment, polyethylene with a thickness of 9 μm is used as a base film, and a nano-aluminum oxide coating with a thickness of 3 μm is coated on the base film to obtain a diaphragm.
[0085] Secondary battery
[0086] In some embodiments, the secondary battery is a lithium ion secondary battery.
[0087] In certain embodiments, the lithium-ion secondary battery is generally a square hard case battery, a soft pack battery, and a cylindrical battery.
[0088] In certain embodiments, the lithium-ion secondary battery can be prepared by conventional methods in the art. Taking a soft-pack battery as an example, the preparation method of the lithium-ion battery includes the following steps: stacking the positive electrode, the separator, and the negative electrode in order, so that the separator is located between the positive electrode and the negative electrode to play an isolating role, and stacking to obtain a bare cell; putting the bare cell into an aluminum-plastic film, drying and removing water, injecting the corresponding electrolyte and sealing, and then going through the processes of standing, hot and cold pressing, forming, clamping, and capacity division to obtain a finished soft-pack lithium-ion battery.
[0089] On the basis of being in accordance with the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present application. The present application is further described below by way of examples, but the present application is not limited to the scope of the embodiments described. The experimental methods for which specific conditions are not indicated in the following examples are selected according to conventional methods and conditions, or according to the product specifications. Unless otherwise specified, the reagents and raw materials used in the present application are commercially available.
[0090] Preparation Examples 1-4
[0091] The preparation methods of Preparation Examples 1-4 are as follows:
[0092] Pyrazine and cyclic phosphate were used as reaction raw materials, dissolved in dimethyl carbonate, sodium methoxide was added to the mixed solution at 0°C, reacted for 6 hours, inorganic sodium methoxide was removed by extraction, and the target product was obtained by recrystallization. The reaction conditions of Preparation Examples 1-4 and the structural formulas of the prepared compounds are listed in Table 1 below:
[0093] Table 1
[0094]
[0095] Example 1
[0096] This embodiment provides a lithium ion secondary battery, and the preparation method of the lithium ion secondary battery is as follows:
[0097] (1) Preparation of electrolyte
[0098] The electrolyte is prepared by the following preparation method: the electrolyte is prepared in a glove box, the nitrogen content in the glove box is 99.999%, the actual oxygen content in the glove box is 0.1ppm, and the moisture content is 0.1ppm. Taking the total mass of the electrolyte as 100%, the battery-grade organic solvent of fluoroethylene carbonate and trifluoroethyl methyl carbonate in a mass ratio of 3:7 is evenly mixed, and then fully dried LiPF6 is added, and then 0.1% of lithium difluorobisoxalate phosphate (LiODFP) is added, and 0.1% of the above-mentioned compound 1 is added to prepare the electrolyte of the lithium ion battery. Among them, the mass content of LiODFP and the compound is listed in the following Table 2.
[0099] (2) Preparation of positive electrode
[0100] The positive electrode active material LiNi 0.5 Mn 1.5 O4, conductive agent acetylene black, and binder polyvinylidene fluoride are fully stirred and mixed in an N-methylpyrrolidone solvent system in a mass ratio of 95:3:2 to obtain a positive electrode slurry. The positive electrode slurry is coated on an aluminum foil, dried, and cold-pressed to obtain a positive electrode.
[0101] (3) Preparation of negative electrode
[0102] The negative electrode active material graphite, the conductive agent acetylene black, the binder styrene butadiene rubber and the thickener sodium carbon methyl cellulose are fully stirred and mixed in a deionized water solvent system in a mass ratio of 96:2:1:1 to obtain a negative electrode slurry, and the negative electrode slurry is coated on a copper foil, dried and cold pressed to obtain a negative electrode.
[0103] (4) Preparation of diaphragm
[0104] A polyethylene with a thickness of 9 μm is used as a base film, and a nano-aluminum oxide coating with a thickness of 3 μm is coated on the base film to obtain a separator.
[0105] (5) Assembling batteries
[0106] The positive electrode, separator and negative electrode are stacked in order, so that the separator is placed between the positive electrode and the negative electrode to play an isolating role, and the sheets are stacked to obtain a bare cell. The bare cell is placed in an aluminum-plastic film, and then baked at 80°C to remove water, and then the electrolyte is injected and sealed. After that, it goes through the processes of standing, hot and cold pressing, formation, clamping, and capacity division to obtain a finished soft-package lithium-ion secondary battery.
[0107] Example 2-16
[0108] Example 2-16 provides a lithium ion secondary battery. The preparation method of the lithium ion secondary battery is the same as Example 1 except for the type of compound, the mass content of the compound and the mass content of LiODFP. The above parameters of Example 2-16 are listed in Table 2.
[0109] Among them, Examples 10-12 are respectively obtained by replacing Compound 1 in Example 1 with Compound 2, Compound 3 and Compound 4 mentioned above.
[0110] Examples 17-28
[0111] Examples 17-28 provide lithium ion secondary batteries. In the preparation method of the lithium ion secondary batteries, a first additive and / or a second additive is added after adding compound 1, and the other conditions are the same as those of Example 6, wherein the second additive is a compound shown in Formula II. The types and mass contents of the first additives and the mass contents of the second additives in Examples 17-28 are listed in Table 2.
[0112] The compound shown in formula II is:
[0113] Formula II.
[0114] Embodiment 29
[0115] Embodiment 29 provides a lithium ion secondary battery. In the preparation method of the lithium ion secondary battery, the electrolyte is prepared by the following steps:
[0116] Prepared in a glove box, the nitrogen content in the glove box is 99.999%, the actual oxygen content in the glove box is 0.1ppm, and the moisture content is 0.1ppm. Based on the total mass of the electrolyte as 100%, the battery-grade organic solvent of fluoroethylene carbonate and trifluoroethyl methyl carbonate in a mass ratio of 2:8 is evenly mixed, and then fully dried LiPF6 is added, and then 1% of lithium difluorobisoxalate phosphate (LiODFP) is added, and 0.3% of the above compound 1 is added to prepare the electrolyte of the lithium ion battery.
[0117] The other preparation steps are the same as those in Example 6.
[0118] Embodiment 30
[0119] Embodiment 30 provides a lithium ion secondary battery. In the preparation method of the lithium ion secondary battery, the electrolyte is prepared by the following steps:
[0120] Prepared in a glove box, the nitrogen content in the glove box is 99.999%, the actual oxygen content in the glove box is 0.1ppm, and the moisture content is 0.1ppm. Based on the total mass of the electrolyte as 100%, the battery-grade organic solvent of fluoroethylene carbonate (FEC): diethyl carbonate (DEC): dimethyl carbonate (DMC) with a mass ratio of 1:1:1 is mixed evenly, and then fully dried LiPF6 is added, and then 1% of lithium difluorobis(oxalate)phosphate (LiODFP) is added, and 0.3% of the above compound 1 is added to prepare the electrolyte of the lithium ion battery.
[0121] The other preparation steps are the same as those in Example 6.
[0122] Comparative Examples 1-6
[0123] Comparative Examples 1-6 provide lithium ion secondary batteries, and the preparation methods of the lithium ion secondary batteries are the same as those of Example 1 except for the different types of compounds, mass contents of the compounds and mass contents of LiODFP. The above parameters of Comparative Examples 1-6 are listed in Table 2.
[0124] Among them, in comparative example 6, the LiODFP in example 1 is replaced by LiBF4, and the other conditions are the same as those in example 1.
[0125] Table 2
[0126]
[0127] Effect Example 1
[0128] The following tests were performed on Examples 1-30 and Comparative Examples 1-6:
[0129] 1. Impedance DCR at -20℃:
[0130] Adjust the temperature of the constant temperature box to -20℃, let it stand for 2h, charge at 0.33C constant current to 4.25V, then charge at 4.25V constant voltage to 0.05C cutoff, let it stand for 30min, and then discharge at 0.33C constant current to 2.5V; cycle 0.33C charge and discharge twice, and record the last discharge capacity as C0; after standing for 30min, discharge at 0.33C to 50%C0, adjust the battery cell SOC to 50%, let it stand for 30min, record the static terminal voltage V1, discharge at C0 constant current for 30s, record the terminal voltage V2 and current I, and calculate DCR=(V1-V2) / I.
[0131] 2. Capacity recovery rate after 30 days of storage at 65°C:
[0132] At 25°C, charge the lithium-ion battery to 4.85V at a constant current of 0.33C, then charge at a constant voltage to a current of 0.05C, let it stand for 30 minutes, repeat 2-3 times, and record the last 0.33C discharge capacity C1. Then place the fully charged battery in a 65°C oven for 30 days, cool the battery cell, adjust the oven temperature to 25°C, let it stand for 10 minutes, discharge at a constant current of 0.33C to 2.5V, then charge and discharge at a rate of 0.33C, 2.5V-4.85V voltage range, cycle 2 times, and record the last discharge capacity C2. Calculate the capacity recovery rate of the lithium-ion battery relative to before storage according to the following formula:
[0133] Capacity recovery rate (%) = (C2 / C1) × 100%.
[0134] The above test results are listed in Table 3 below:
[0135] Table 3
[0136]
[0137] It can be seen from Table 1 and Table 2 that the lithium ion secondary battery provided by the embodiments of the present application, wherein the electrolyte contains a specific compound and contains lithium difluorobis(oxalate)phosphate, so that the prepared lithium ion secondary battery has excellent kinetic performance and high temperature storage performance, specifically: the impedance DCR at -20°C is below 887mOhm, and the capacity recovery rate after high temperature storage at 65°C for 30 days is above 88.5%; in some preferred embodiments, the impedance DCR at -20°C can reach below 800mOhm, and the capacity recovery rate after high temperature storage at 65°C for 30 days can reach above 93%.
[0138] According to Comparative Examples 1-6, when the electrolyte does not contain the compound and LiODFP in the present application, or contains only one of the components, the kinetic performance and high temperature storage performance of the prepared lithium ion secondary battery are poor. Among them, in Comparative Example 6, LiODFP is replaced with LiBF4, and its kinetic performance and high temperature storage performance are significantly reduced.
[0139] On the one hand, the excellent kinetic performance of the present application may be due to the fact that the compound of the present application is a zwitterion, and the nitrogen atom in the compound can provide a larger polarity, and can play an efficient dissociation role with a simpler molecular structure. At the same time, LiODFP has a low solubility in the electrolyte, and the introduction of a large polar substance can increase the solubility of LiODFP, and the decomposition of LiODFP will produce a series of inorganic salt substances, which is beneficial to the kinetic performance of the battery. On the other hand, the present application can also have excellent high-temperature storage performance, which may be due to the coordination of the pyrazine group and the phosphate ester in the compound, which can fix the transition metal ions on the positive electrode side and avoid the destruction of the protective film of the positive electrode interface layer, thereby achieving excellent high-temperature storage performance. Furthermore, the phosphate ester in the compound can capture the active oxygen that may be generated under the high voltage of the positive electrode, greatly improving the safety of the system.
[0140] According to the results of Examples 6 and 10-12, Example 6 and Example 11 respectively use Compound 1 and Compound 3, which can further reduce the impedance DCR at -20°C to below 780mOhm, and increase the capacity recovery rate after 30 days of high-temperature storage at 65°C to more than 92%.
[0141] According to the results of Examples 1-9, 13 and 14, the mass content of lithium difluorobis(oxalate)phosphate in the electrolyte of Example 1-9 is 0.1%-3%, which can further reduce the impedance DCR at -20°C to below 850mOhm, and increase the capacity recovery rate after high-temperature storage at 65°C for 30 days to more than 90%.
[0142] According to the results of Examples 1-9, 15 and 16, the mass content of the compound in the electrolyte of Example 1-9 is 0.1%-3%, which can further reduce the impedance DCR at -20°C to below 850mOhm, and increase the capacity recovery rate after high-temperature storage at 65°C for 30 days to more than 90%.
[0143] According to the results of Example 6, Example 18-20, and Example 22, the electrolytes of Example 18-20 and Example 22 also include a first additive, and the mass content of the first additive is 3%-7%, which can further reduce the impedance DCR at -20°C to below 765mOhm. According to the results of Example 6 and Example 24-26, the electrolytes of Example 24-26 also include a second additive, and the mass content of the second additive is 0.3%-2%, which can further reduce the impedance DCR at -20°C to below 760mOhm, and the capacity recovery rate of 65°C high temperature storage for 30 days is increased to more than 93%. The impedance DCR of Example 28 at -20°C is 652mOhm, and the capacity recovery rate of 65°C high temperature storage for 30 days is increased to 95%, indicating that the simultaneous addition of the first additive and the second additive can make the lithium-ion secondary battery made of its electrolyte have better kinetic performance and high temperature storage performance.
[0144] The specific embodiments described above further illustrate the purpose, technical solutions and beneficial effects of the present application. It should be understood that the above description is only a specific embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application should be included in the scope of protection of the present application.
Claims
1. An electrolyte, characterized in that: It includes compounds and lithium difluorobisoxalate phosphate; The compound includes a compound represented by the following formula I: Formula I; Among them, A is selected from an alkyl group having 1-3 carbon atoms or an alkenyl group having 2-3 carbon atoms; R1 is any one selected from an alkyl group having 1-3 carbon atoms, an alkenyl group having 2-5 carbon atoms, an ester group having 1-3 carbon atoms, a carbonyl-containing substituent having 1-3 carbon atoms and a hydrogen atom.
2. The electrolyte according to claim 1, characterized in that The mass content of the lithium difluorobis(oxalate)phosphate in the electrolyte is 0.1%-3%.
3. The electrolyte according to claim 1, characterized in that The mass content of the compound represented by formula I in the electrolyte is 0.1%-3%.
4. The electrolyte according to claim 2 or 3, characterized in that The electrolyte satisfies one or both of the following conditions (1)-(2): (1) The mass content of the lithium difluorobis(oxalate)phosphate in the electrolyte is 0.5%-1%; (2) The mass content of the compound represented by formula I in the electrolyte is 0.2%-1%.
5. The electrolyte according to claim 1, characterized in that The compound shown in formula I is: Formula I-1; Here, R1 is any one selected from an alkyl group having 1 to 3 carbon atoms, an alkenyl group having 2 to 5 carbon atoms, an ester group having 1 to 3 carbon atoms, a carbonyl-containing substituent having 1 to 3 carbon atoms, and a hydrogen atom.
6. The electrolyte according to claim 1, characterized in that The compound represented by formula I is selected from at least one of the following compounds: 、 、 、 。 7. The electrolyte according to claim 1, characterized in that The electrolyte satisfies one or both of the following conditions (1)-(2): (1) The electrolyte further includes a first additive, wherein the first additive includes one or more of vinyl sulfate, 1,3-propane sultone, vinylene carbonate and propenyl-1,2-sultone; (2) The electrolyte further comprises a second additive, wherein the second additive comprises a compound as shown in Formula II, Formula II.
8. The electrolyte according to claim 7, characterized in that The electrolyte satisfies one or both of the following conditions (1)-(2): (1) The mass content of the first additive in the electrolyte is 3%-7%; (2) The mass content of the second additive in the electrolyte is 0.3%-2%.
9. The electrolyte according to claim 1, characterized in that The electrolyte satisfies one or both of the following conditions (1)-(2): (1) The electrolyte further comprises fluoroethylene carbonate, wherein the mass content of the fluoroethylene carbonate is 10%-30%; (2) The electrolyte further comprises a fluorinated chain carbonate, wherein the fluorinated chain carbonate comprises one or more of trifluoroethyl methyl carbonate and bistrifluoroethyl carbonate, and the mass content of the fluorinated chain carbonate is 20%-75%.
10. A secondary battery, characterized in that: It comprises the electrolyte according to any one of claims 1 to 9.