A bismuth-based potassium ion battery negative electrode material with core-shell structure and preparation method thereof

By constructing a nano-Bi/BiOx core-shell structure and covering it with a conductive layer and a coating layer, the problem of the volume effect of potassium ion battery materials in the process of bismuth insertion and removal of potassium has been solved, and a high-capacity and long-life anode material has been achieved to meet the requirements Commercial application requirements.

CN115881924BActive Publication Date: 2024-10-18SHUNDE POLYTECHNIC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211738036.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-31
Publication Date
2024-10-18
Estimated Expiration
2042-12-31

AI Technical Summary

Technical Problem

Potassium-ion batteries have poor material cycle stability due to the volume effect during the process of bismuth insertion and removal of potassium, and cannot meet commercial application requirements.

Method used

Construct a nano-Bi/BiOx core-shell structure and use a multi-layer outer coating process, using a nano-carbon fiber conductive layer and a citric acid or pitch cracked carbon coating layer to reserve space to limit the volume expansion of bismuth and improve the material's conductivity and cycle stability. sex.

Benefits of technology

A high-capacity, long-life bismuth-based potassium-ion battery anode material has been achieved, which meets the needs of commercial applications and is simple to prepare and low-cost.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a bismuth-based potassium ion battery negative electrode material with a core-shell structure and a preparation method thereof. The negative electrode material has a Bi / BiOx core-shell structure particle as the innermost layer, a nano-carbon fiber conductive layer as the middle layer, and a citric acid or asphalt cracking carbon coating layer as the outermost layer. The negative electrode material has the characteristics of high capacity and long life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of battery negative electrode materials, and more specifically, to a bismuth-based potassium ion battery negative electrode material with a core-shell structure and a preparation method thereof. Background Art

[0002] Although lithium-ion batteries have become the most important energy storage system, the shortage of lithium resources has led to high prices for lithium-ion batteries. Potassium-ion batteries have attracted widespread attention due to their obvious resource reserves and the same working principle and similar electrochemical potential as lithium-ion batteries. However, compared with lithium ions, potassium ions have a larger radius, and commercial carbon negative electrode materials cannot be used in potassium-ion batteries. Bismuth (Bi) has a high capacity (3800mAh cm -3 ), almost graphite (756mAh cm-3 ) is 5 times greater than that of Bi. In addition, Bi has a unique large lattice stripe layer structure along the c-axis. It is conducive to the insertion of ions. However, there is a large volume effect in the process of bismuth insertion and removal of potassium, and the material shows poor cycle stability. Summary of the invention

[0003] The technical problem to be solved by the present invention is to construct nano Bi / BiO x The core-shell structure reserves space for the possible volume expansion of bismuth. At the same time, a multi-layer outer coating process is used to construct the conductive layer and the coating layer. This improves the conductivity of the material while ensuring that the main material is inhibited from expanding outward to meet the requirements of commercial applications.

[0004] The technical solution of the present invention to solve the technical problem is: a bismuth-based potassium ion battery negative electrode material with a core-shell structure, the innermost layer of the bismuth-based potassium ion battery negative electrode material is Bi / BiOx core-shell structure particles, the middle is coated with a nano-carbon fiber conductive layer, and the outermost layer is a citric acid or asphalt cracking carbon coating layer, which has the characteristics of high capacity and long life.

[0005] The value range of x in the Bi / BiOx core-shell structure is: x=0.1~2.

[0006] The present invention also provides a method for preparing a bismuth-based potassium ion battery negative electrode material having a core-shell structure, comprising the following steps:

[0007] (1) Take high-purity (purity above 99%) bismuth oxide powder as raw material, the maximum particle size of bismuth oxide is less than 100 nm, weigh bismuth oxide and graphite according to the molar ratio Bi2O3:C=2:3, and the graphite particle size does not exceed d 50 =20 microns;

[0008] (2) the material weighed in step (1) is subjected to high-energy ball milling for 2-5 hours in anhydrous ethanol environment, and the ball milling balls are zirconia balls with a radius not exceeding 5 mm;

[0009] (3) After vacuum drying for more than 24 hours, the mixture is heated from room temperature to 250-600° C. at a rate of 2-5° C. / min, while maintaining an argon inert atmosphere for 2-6 hours, and then naturally cooled to room temperature to obtain nano Bi / BiOx core-shell structure particles;

[0010] (4) weighing carbon nanotubes or carbon nanofibers or graphene at a mass ratio of 1% to 5% of the Bi / BiOx core-shell structure particles obtained in step (3), and weighing citric acid or asphalt at a mass ratio of 5% to 20% of the Bi / BiOx core-shell structure particles, and high-energy ball milling the mixture in an anhydrous ethanol environment for 2-5 hours, using a zirconia ball with a radius of no more than 5 mm;

[0011] (5) taking out and vacuum drying for more than 24 hours or spray drying, heating from room temperature to 400-600° C. at 2-5° C. / min, maintaining argon inert atmosphere protection during the period, and keeping the temperature for 2-6 hours, then heating from room temperature to 800-1100° C. at 2-5° C. / min, keeping the temperature for 2-6 hours, and naturally cooling to room temperature to obtain a bismuth-based potassium ion battery negative electrode material with a core-shell structure.

[0012] The beneficial effects of the present invention are:

[0013] The negative electrode material of the present invention has the advantages of high capacity, long life, simple preparation and low cost.

[0014] The present invention reduces Bi2O3 by thermal carbon to construct Bi / BiOx (x=0.1-2) with a core-shell structure, reserves expansion space for the volume expansion that may occur during the bismuth insertion and removal of potassium, and coats the outer layer with a citric acid or asphalt cracking carbon layer to construct a "cage" structure, thereby limiting the possible volume effect of the material within the "cage" structure and enabling the material to meet the requirements of commercial applications. DETAILED DESCRIPTION

[0015] Embodiments of the present invention are described in detail below. The described embodiments are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention.

[0016] Embodiment 1:

[0017] (1) Take high-purity (purity above 99%) bismuth oxide powder as raw material, the maximum particle size of bismuth oxide is less than 100 nm, weigh bismuth oxide and graphite according to the molar ratio Bi2O3:C=2:3, and the graphite particle size does not exceed d 50 =20 microns;

[0018] (2) the material weighed in step (1) is subjected to high-energy ball milling for 2 hours in anhydrous ethanol environment, and the ball milling balls are zirconia balls with a radius not exceeding 5 mm;

[0019] (3) After being taken out and vacuum dried for 24 hours, the mixture was heated from room temperature to 600°C at a rate of 2°C / min, while maintaining an argon inert atmosphere for protection. The temperature was kept for 6 hours, and the mixture was naturally cooled to room temperature to obtain nano Bi / BiOx core-shell structure particles.

[0020] (4) weighing carbon nanotubes at a mass ratio of 1% of the Bi / BiOx core-shell structure particles obtained in step (3), and weighing citric acid at a mass ratio of 5% of the Bi / BiOx core-shell structure particles, and high-energy ball milling the mixture in an anhydrous ethanol environment for 2 hours, using a zirconia ball with a radius of no more than 5 mm;

[0021] (5) Take out and spray dry, heat from room temperature to 400°C at 2°C / min, keep argon inert atmosphere for 2 hours, then heat from room temperature to 800°C at 2°C / min, keep for 2 hours, and cool to room temperature naturally to obtain a bismuth-based potassium ion battery negative electrode material with a core-shell structure. -1 The specific capacity at the current density is 450 mAh g -1 , 0.5A g-1 The reversible capacity after 300 cycles at the current density is 300 mAh g -1 .

[0022] Embodiment 2:

[0023] (1) Take high-purity (purity above 99%) bismuth oxide powder as raw material, the maximum particle size of bismuth oxide is less than 100 nm, weigh bismuth oxide and graphite according to the molar ratio Bi2O3:C=2:3, and the graphite particle size does not exceed d 50 =20 microns;

[0024] (2) the material weighed in step (1) is subjected to high-energy ball milling in an anhydrous ethanol environment for 5 hours, and the ball milling balls are zirconia balls with a radius not exceeding 5 mm;

[0025] (3) After being taken out and vacuum dried for 24 hours, the mixture was heated from room temperature to 250°C at a rate of 5°C / min, while maintaining an argon inert atmosphere for protection. The temperature was kept for 2 hours and then naturally cooled to room temperature to obtain nano Bi / BiOx core-shell structure particles.

[0026] (4) weighing carbon nanofibers at a mass ratio of 5% of the Bi / BiOx core-shell structure particles obtained in step (3), and weighing asphalt at a mass ratio of 20% of the Bi / BiOx core-shell structure particles, and high-energy ball milling the mixture in an anhydrous ethanol environment for 5 hours, using a zirconia ball with a radius of no more than 5 mm;

[0027] (5) Take out and vacuum dry for more than 24 hours, heat from room temperature to 600°C at 5°C / min, keep argon inert atmosphere for 6 hours, then heat from room temperature to 1100°C at 5°C / min, keep 6 hours, and cool to room temperature naturally to obtain a bismuth-based potassium ion battery negative electrode material with a core-shell structure. -1 The specific capacity at the current density is 550 mAh g -1 , 0.5A g-1 The reversible capacity after 300 cycles at the current density is 380 mAh g -1 .

[0028] Embodiment three:

[0029] (1) Take high-purity (purity above 99%) bismuth oxide powder as raw material, the maximum particle size of bismuth oxide is less than 100 nm, weigh bismuth oxide and graphite according to the molar ratio Bi2O3:C=2:3, and the graphite particle size does not exceed d 50 =20 microns;

[0030] (2) the material weighed in step (1) is subjected to high-energy ball milling for 4 hours in anhydrous ethanol environment, and the ball milling balls are zirconia balls with a radius not exceeding 5 mm;

[0031] (3) After being taken out and vacuum dried for 24 hours, the mixture was heated from room temperature to 400°C at a rate of 3°C / min, while maintaining an argon inert atmosphere for 4 hours. The mixture was then naturally cooled to room temperature to obtain nano Bi / BiOx core-shell structured particles.

[0032] (4) weighing graphene at a mass ratio of 4% of the Bi / BiOx core-shell structure particles obtained in step (3), weighing citric acid at a mass ratio of 15% of the Bi / BiOx core-shell structure particles, and subjecting the mixture to high-energy ball milling in an anhydrous ethanol environment for 4 hours, using a zirconia ball with a radius of no more than 5 mm;

[0033] (5) Take out and spray dry, heat from room temperature to 500°C at 3°C / min, keep argon inert atmosphere for 4 hours, then heat from room temperature to 900°C at 4°C / min, keep 4 hours, and cool to room temperature naturally to obtain bismuth-based potassium ion battery negative electrode material with core-shell structure. -1The specific capacity at the current density is 500mAhg -1 , 0.5A g -1 The reversible capacity after 300 cycles at the current density is 400 mAh g -1 .

[0034] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A method for preparing a bismuth-based potassium ion battery negative electrode material with a core-shell structure, characterized in that The following steps are involved: (1) taking high-purity bismuth oxide powder as a raw material, the maximum particle size of the bismuth oxide is less than 100 nm, weighing bismuth oxide and graphite according to the molar ratio of Bi2O3:C=2:3, and the particle size d50 of the graphite is not more than 20 microns; the purity of the high-purity bismuth oxide powder is more than 99%; (2) the material weighed in step (1) is subjected to high-energy ball milling for 2-5 hours in anhydrous ethanol environment, and the ball milling balls are zirconia balls with a radius not exceeding 5 mm; (3) After vacuum drying for more than 24 hours, the mixture is heated from room temperature to 250-600° C. at a rate of 2-5° C. / min, while maintaining an argon inert atmosphere for 2-6 hours, and then naturally cooled to room temperature to obtain nano Bi / BiOx core-shell structure particles; (4) weighing carbon nanotubes or carbon nanofibers or graphene at a mass ratio of 1% to 5% of the Bi / BiOx core-shell structure particles obtained in step (3), and weighing citric acid or asphalt at a mass ratio of 5% to 20% of the Bi / BiOx core-shell structure particles, and subjecting the mixture to high-energy ball milling in an anhydrous ethanol environment for 2 to 5 hours, using a zirconia ball with a radius of no more than 5 mm; (5) After vacuum drying for more than 24 hours or spray drying, the mixture is heated from room temperature to 400-600° C. at a rate of 2-5° C. / min, while maintaining an argon inert atmosphere for protection for 2-6 hours, and then heated from room temperature to 800-1100° C. at a rate of 2-5° C. / min for 2-6 hours, and then naturally cooled to room temperature to obtain a bismuth-based potassium ion battery negative electrode material with a core-shell structure.

Citation Information

Patent Citations

  • Preparation method of bismuth telluride / graphene / silicon composite core-shell structure

    CN109411596A

  • Bi-MOF-derived bismuth oxide-based negative electrode material and preparation and application thereof

    CN114551828A