Laminated body
By using aqueous dispersions containing different ethylene-unsaturated carboxylic acid copolymers to form an adhesive layer during the heat sealing process, the problems of insufficient low-temperature adhesion, water resistance and hot water resistance between the substrate and the adherend are solved. , achieving efficient heat sealing effect.
Patent Information
- Application Number
- CN202180044302.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-07-14
- Filing Date
- 2021-07-13
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-07-13
AI Technical Summary
During the heat sealing process between the base material and the adherend, the existing technology has insufficient low-temperature adhesion, water resistance and hot water resistance, making it difficult to meet certain application requirements.
Aqueous dispersions containing different ethylene-unsaturated carboxylic acid copolymers are used as the adhesive layer, and the adhesive layer is formed by drying to ensure that the content of unsaturated carboxylic acid structural units in the adhesive layer is between 5-18 mass%. To improve low temperature adhesion and water resistance.
It achieves excellent low-temperature adhesion, water resistance and hot water resistance, and is suitable for heat sealing materials in various industrial fields.
Smart Images

Figure BDA0004008214790000191 
Figure BDA0004008214790000192
Abstract
Description
Technical Field
[0001] The present invention relates to a laminate. Background Art
[0002] The method of bonding a substrate such as a plastic film, a vapor-deposited film, a metal foil, paper, a nonwoven fabric, and another adherend or bonding the substrates to each other (i.e., heat sealing) by heat and pressure has gradually been widely used in various industrial fields. In the heat sealing method, an adhesive layer that can be bonded by heat and pressure is usually provided on the substrate in advance, and the substrate and the other adherend, or the substrates to each other, are bonded via the adhesive layer.
[0003] For example, in Japanese Unexamined Patent Publication No. 57-137339, heat sealing is performed via an adhesive layer formed by coating an aqueous dispersion composition of a modified product of a copolymer of ethylene, α,β-unsaturated carboxylic acid, and α,β-unsaturated carboxylic acid metal salt.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Laid-Open No. 57-137339 Summary of the invention
[0007] Problems to be solved by the invention
[0008] Depending on the types and uses of substrates and adherends, there may be a demand for further improvement in low-temperature adhesiveness, water resistance, and hot water resistance.
[0009] An object of the present invention is to provide a laminate having an adhesive layer which is excellent in low-temperature adhesion, water resistance and hot water resistance.
[0010] Means for solving problems
[0011] The present invention includes the following inventions [1] to [6].
[0012] [1] A laminate comprising a substrate and an adhesive layer laminated on at least one surface of the substrate,
[0013] The adhesive layer is obtained by drying a coating of an aqueous dispersion containing water and the resin (X).
[0014] The resin (X) includes two or more ethylene-unsaturated carboxylic acid copolymers (a) having different contents of structural units derived from unsaturated carboxylic acids.
[0015] [2] A laminate as described in [1], wherein the total content of structural units derived from unsaturated carboxylic acids contained in the above-mentioned two or more ethylene-unsaturated carboxylic acid copolymers (a) is 5% by mass or more and less than 18% by mass relative to the total amount of structural units derived from monomers of the polymer contained in the above-mentioned resin (X).
[0016] [3] A laminate as described in [1] or [2], wherein the two or more ethylene-unsaturated carboxylic acid copolymers (a) include one or more ethylene-unsaturated carboxylic acid copolymers (a1) in which the content of structural units derived from unsaturated carboxylic acid is from 12 mass % to 30 mass %, and one or more ethylene-unsaturated carboxylic acid copolymers (a2) in which the content of structural units derived from unsaturated carboxylic acid is greater than 0 mass % and less than 12 mass %.
[0017] [4] The laminate according to [3], wherein the two or more ethylene-unsaturated carboxylic acid copolymers (a) satisfy at least one of the following conditions (i) and (ii).
[0018] (i) As the ethylene-unsaturated carboxylic acid copolymer (a1), two or more ethylene-unsaturated carboxylic acid copolymers having different contents of structural units derived from unsaturated carboxylic acids are included.
[0019] (ii) Two or more ethylene-unsaturated carboxylic acid copolymers having different contents of structural units derived from unsaturated carboxylic acids are included as the ethylene-unsaturated carboxylic acid copolymer (a2).
[0020] [5] The laminate according to [4], wherein the ethylene-unsaturated carboxylic acid copolymer (a1) comprises:
[0021] an ethylene-unsaturated carboxylic acid copolymer (a1-1) in which the content of the structural unit derived from the unsaturated carboxylic acid is 17% by mass or more and 30% by mass or less; and
[0022] An ethylene-unsaturated carboxylic acid copolymer (a1-2) having a content of a structural unit derived from an unsaturated carboxylic acid of 12% by mass or more and less than 17% by mass.
[0023] [6] A laminate comprising a substrate and an adhesive layer laminated on at least one surface of the substrate,
[0024] The adhesive layer contains two or more ethylene-unsaturated carboxylic acid copolymers (a) having different contents of structural units derived from unsaturated carboxylic acids.
[0025] Effects of the Invention
[0026] According to the present invention, a laminate having excellent low-temperature adhesiveness, water resistance, and hot water resistance can be obtained. DETAILED DESCRIPTION
[0027] In the present specification, a numerical range expressed using "to" means a range including the numerical values described before and after "to" as the lower limit and the upper limit.
[0028] In the numerical ranges described in stages in the present specification, the upper limit value or the lower limit value described in one numerical range may be replaced with the upper limit value or the lower limit value of another numerical range described in stages.
[0029] The laminated body of the present invention will be described in detail below.
[0030] The laminate of the present invention is characterized in that:
[0031] A substrate and an adhesive layer laminated on at least one surface of the substrate.
[0032] The adhesive layer contains two or more ethylene-unsaturated carboxylic acid copolymers (a) having different contents of structural units derived from unsaturated carboxylic acids.
[0033] One embodiment of the laminate of the present invention is a laminate comprising a substrate and an adhesive layer laminated on at least one surface of the substrate, wherein the adhesive layer is obtained by drying a coating material containing an aqueous dispersion of water and a resin (X), wherein the resin (X) contains two or more ethylene-unsaturated carboxylic acid copolymers (a) having different contents of structural units derived from unsaturated carboxylic acids.
[0034] <Aqueous Dispersion>
[0035] The aqueous dispersion used for producing the laminate of the present invention contains a resin (X) and water for dispersing the resin (X).
[0036] [Resin (X)]
[0037] The resin (X) contains two or more types of ethylene-unsaturated carboxylic acid copolymers (a) having different contents of the structural unit derived from the unsaturated carboxylic acid.
[0038] The total content (acid content) of the structural units derived from the unsaturated carboxylic acid contained in the ethylene-unsaturated carboxylic acid copolymer (a) is preferably 5% by mass or more, more preferably 8% by mass or more, and preferably less than 18% by mass, more preferably less than 16% by mass, relative to the total amount of the structural units derived from the monomers of the polymer contained in the resin (X). When the total content (acid content) of the structural units derived from the unsaturated carboxylic acid is within the above range, the obtained laminate can have excellent low-temperature adhesion, water resistance and hot water resistance.
[0039] The total content of the structural units derived from ethylene contained in the ethylene-unsaturated carboxylic acid copolymer (a) is preferably 82% by mass or more, more preferably 84% by mass or more, and preferably less than 95% by mass, more preferably 92% by mass or less, relative to the total amount of the structural units derived from the monomers of the polymer contained in the resin (X). If the total content of the structural units derived from ethylene is within the above range, the obtained laminate can have excellent low-temperature adhesion, water resistance and hot water resistance.
[0040] The weight average molecular weight of the resin (X) is, for example, 8,000 or more, preferably 10,000 or more, for example, 150,000 or less, preferably 100,000 or less. In the present invention, the weight average molecular weight is a value determined in terms of standard polystyrene measured by gel permeation chromatography (GPC).
[0041] The melting point of the resin (X) is, for example, 80° C. or higher, preferably 85° C. or higher, and for example, 97° C. or lower, preferably 92° C. or lower.
[0042] The melt flow rate (MFR ASTM D1238, 190°C, 2.16 kg load) of the resin (X) is preferably 0.1 g / 10 min or more, more preferably 0.5 g / 10 min or more, and is preferably 150 g / 10 min or less, more preferably 100 g / 10 min or less.
[0043] There is no particular limitation on the method for preparing the resin (X) comprising two or more ethylene-unsaturated carboxylic acid copolymers (a) having different contents of structural units derived from unsaturated carboxylic acids. For example, the resin (X) can be prepared by melt-kneading two or more ethylene-unsaturated carboxylic acid copolymers at a temperature above the melting point of the ethylene-unsaturated carboxylic acid copolymer (a) having the highest melting point among the two or more ethylene-unsaturated carboxylic acid copolymers (a), preferably at a temperature above 100° C., more preferably at a temperature above 110° C.
[0044] When two or more ethylene-unsaturated carboxylic acid copolymers (a) are used, the two or more ethylene-unsaturated carboxylic acid copolymers obtained by neutralizing a part or all of the carboxyl groups contained in these copolymers can be prepared, for example, by melt-kneading the inorganic alkali neutralized products of the two or more ethylene-unsaturated carboxylic acid copolymers as described above. In addition, as another method, two or more ethylene-unsaturated carboxylic acid copolymers can be melt-kneaded to produce a melt-kneaded product, and the obtained melt-kneaded product is put into an aqueous solution containing a neutralizer and water (which is maintained at a melting point of the ethylene-unsaturated carboxylic acid copolymer with the highest melting point among the two or more ethylene-unsaturated carboxylic acid copolymers, preferably at a melting point of 100° C. or more, and more preferably at a melting point of 110° C. or more), and mixed to produce two or more ethylene-unsaturated carboxylic acid copolymers obtained by neutralizing a part or all of the carboxyl groups.
[0045] As the neutralizing agent, for example, a basic compound can be used, specifically, inorganic basic compounds such as sodium hydroxide and potassium hydroxide; organic basic compounds represented by amines such as ammonia, triethylamine, triethanolamine, and dimethylethanolamine; and the like.
[0046] Among these basic compounds, inorganic basic compounds are preferred, and sodium hydroxide and potassium hydroxide are more preferred. These basic compounds may be used alone or in combination of two or more.
[0047] The amount of the basic compound added is, for example, 5 mol or more, preferably 20 mol or more, more preferably 25 mol or more, and for example 70 mol or less, preferably 60 mol or less, relative to 100 mol of all carboxyl groups contained in two or more ethylene-unsaturated carboxylic acids (a).
[0048] In addition, after adding the neutralizing agent for neutralization, it is preferably maintained at a predetermined temperature for a predetermined time. As the maintenance conditions, the maintenance temperature is, for example, 40° C. or more, preferably 50° C. or more, for example, 190° C. or less, preferably 180° C. or less. In addition, the maintenance time is, for example, 30 minutes or more, preferably 1 hour or more, for example, 12 hours or less, preferably 10 hours or less.
[0049] When the ethylene-unsaturated carboxylic acid copolymer is neutralized for use, the degree of neutralization is, for example, 20% or more, preferably 25% or more, and for example, 70% or less, preferably 60% or less, based on the total amount of the two or more ethylene-unsaturated carboxylic acid copolymers (a). The degree of neutralization herein refers to the molar percentage of carboxyl groups in the ethylene-unsaturated carboxylic acid copolymer (a) in the resin (X) neutralized by the basic compound as a neutralizing agent.
[0050] When the degree of neutralization is within the above range, an adhesive layer having excellent heat seal strength can be obtained from the aqueous dispersion. It should be noted that the degree of neutralization is calculated according to the Examples described below.
[0051] The resin (X) may optionally contain, in addition to water and two or more ethylene-unsaturated carboxylic acid copolymers (a), low-density polyethylene, ethylene-butene copolymers, ethylene-propylene copolymers, ethylene-1-butene-propylene copolymers, ethylene-propylene-ethylidene norbornene copolymers, ethylene-(meth)acrylate copolymers, ethylene-vinyl acetate copolymers, and ethylene-vinyl acetate-carbon monoxide copolymers.
[0052] [Two or more ethylene-unsaturated carboxylic acid copolymers (a)]
[0053] Each of the two or more ethylene-unsaturated carboxylic acid copolymers (a) is a copolymer containing a structural unit derived from ethylene and a structural unit derived from an unsaturated carboxylic acid.
[0054] The two or more ethylene-unsaturated carboxylic acid copolymers (a) preferably include: an ethylene-unsaturated carboxylic acid copolymer (a1) having a content of structural units derived from unsaturated carboxylic acid of 12% by mass to 30% by mass as a copolymer having a high carboxyl content; and an ethylene-unsaturated carboxylic acid copolymer (a2) having a content of structural units derived from unsaturated carboxylic acid of greater than 0% by mass and less than 12% by mass as a copolymer having a low carboxyl content.
[0055] The content of the structural unit derived from the unsaturated carboxylic acid in the ethylene-unsaturated carboxylic acid copolymer (a1) is preferably 15% by mass or more and preferably 25% by mass or less from the viewpoint of emulsion stability.
[0056] The weight average molecular weight of the ethylene-unsaturated carboxylic acid copolymer (a1) is, for example, 8,000 or more, preferably 10,000 or more, and for example, 150,000 or less, preferably 10,0000 or less, from the viewpoint of adhesive strength and emulsion stability.
[0057] From the viewpoint of heat sealability, the melting point of the ethylene-unsaturated carboxylic acid copolymer (a1) is, for example, 70°C or higher, preferably 80°C or higher, for example, 100°C or lower, preferably 95°C or lower.
[0058] From the aspects of adhesive strength and emulsion stability, the melt flow rate (MFR ASTM D1238, 190°C, 2.16 kg load) of the ethylene-unsaturated carboxylic acid copolymer (a1) is, for example, 0.1 g / 10 min or more, preferably 0.5 g / 10 min or more, for example, 150 g / 10 min or less, preferably 100 g / 10 min or less.
[0059] The content of the structural unit derived from the unsaturated carboxylic acid in the ethylene-unsaturated carboxylic acid copolymer (a2) is preferably 2% by mass or more and preferably 10% by mass or less from the viewpoint of emulsion stability.
[0060] The weight average molecular weight of the ethylene-unsaturated carboxylic acid copolymer (a2) is, for example, 8,000 or more, preferably 10,000 or more, and for example, 150,000 or less, preferably 100,000 or less, from the viewpoint of adhesive strength and emulsion stability.
[0061] From the viewpoint of heat sealability, the melting point of the ethylene-unsaturated carboxylic acid copolymer (a2) is, for example, 70°C or higher, preferably 80°C or higher, for example, 100°C or lower, preferably 95°C or lower.
[0062] From the aspects of adhesive strength and emulsion stability, the melt flow rate (MFR ASTM D1238, 190°C, 2.16 kg load) of the ethylene-unsaturated carboxylic acid copolymer (a2) is, for example, 0.1 g / 10 min or more, preferably 0.5 g / 10 min or more, for example, 150 g / 10 min or less, preferably 100 g / 10 min or less.
[0063] From the viewpoint of low-temperature adhesiveness, water resistance, and hot water resistance, the two or more ethylene-unsaturated carboxylic acid copolymers (a) preferably satisfy at least one of the following conditions (i) and (ii).
[0064] (i) As the ethylene-unsaturated carboxylic acid copolymer (a1), two or more ethylene-unsaturated carboxylic acid copolymers having different contents of structural units derived from unsaturated carboxylic acids are included.
[0065] (ii) Two or more ethylene-unsaturated carboxylic acid copolymers having different contents of structural units derived from unsaturated carboxylic acids are included as the ethylene-unsaturated carboxylic acid copolymer (a2).
[0066] Among the above-mentioned conditions (i), it is preferred that the ethylene-unsaturated carboxylic acid copolymer (a1) comprises: an ethylene-unsaturated carboxylic acid copolymer (a1-1) in which the content of structural units derived from unsaturated carboxylic acid is greater than 17 mass % and less than 30 mass %; and an ethylene-unsaturated carboxylic acid copolymer (a1-2) in which the content of structural units derived from unsaturated carboxylic acid is greater than 12 mass % and less than 17 mass %.
[0067] The content of the structural unit derived from the unsaturated carboxylic acid in the ethylene-unsaturated carboxylic acid copolymer (a1-1) is preferably 18% by mass or more and preferably 25% by mass or less from the viewpoint of emulsion stability.
[0068] The weight average molecular weight of the ethylene-unsaturated carboxylic acid copolymer (a1-1) is, for example, 8,000 or more, preferably 10,000, for example, 150,000 or less, preferably 100,000 or less, from the viewpoint of adhesive strength and emulsion stability.
[0069] From the viewpoint of heat sealability, the melting point of the ethylene-unsaturated carboxylic acid copolymer (a1-1) is, for example, 70°C or higher, preferably 80°C or higher, for example, 100°C or lower, preferably 95°C or lower.
[0070] From the aspects of adhesive strength and emulsion stability, the melt flow rate (MFR ASTM D1238, 190°C, 2.16 kg load) of the ethylene-unsaturated carboxylic acid copolymer (a1-1) is, for example, 0.1 g / 10 min or more, preferably 0.5 g / 10 min or more, for example, 150 g / 10 min or less, preferably 100 g / 10 min or less.
[0071] The content of the structural unit derived from the unsaturated carboxylic acid in the ethylene-unsaturated carboxylic acid copolymer (a1-2) is preferably 12% by mass or more and preferably 15% by mass or less from the viewpoint of emulsion stability.
[0072] The weight average molecular weight of the ethylene-unsaturated carboxylic acid copolymer (a1-2) is, for example, 8,000 or more, preferably 10,000, and for example, 150,000 or less, preferably 100,000 or less, from the viewpoint of adhesive strength and emulsion stability.
[0073] From the viewpoint of heat sealability, the melting point of the ethylene-unsaturated carboxylic acid copolymer (a1-2) is, for example, 70°C or higher, preferably 80°C or higher, for example, 100°C or lower, preferably 95°C or lower.
[0074] From the aspects of adhesive strength and emulsion stability, the melt flow rate (MFR ASTM D1238, 190°C, 2.16 kg load) of the ethylene-unsaturated carboxylic acid copolymer (a1-2) is, for example, 0.1 g / 10 min or more, preferably 0.5 g / 10 min or more, for example, 150 g / 10 min or less, preferably 100 g / 10 min or less.
[0075] In addition, as ethylene-unsaturated carboxylic acid copolymer (a), when using the above-mentioned ethylene-unsaturated carboxylic acid copolymer (a1-1), ethylene-unsaturated carboxylic acid copolymer (a1-2) and ethylene-unsaturated carboxylic acid copolymer (a2), the content of ethylene-unsaturated carboxylic acid copolymer (a2) is preferably 20% by mass or more, more preferably 25% by mass or more, preferably 85% by mass or less, and more preferably 80% by mass or less relative to the total amount of ethylene-unsaturated carboxylic acid copolymer (a) contained in resin (X). The content of ethylene-unsaturated carboxylic acid copolymer (a1-1) is preferably 20% by mass or more, more preferably 25% by mass or more, preferably 80% by mass or less, and more preferably 75% by mass or less. The content of ethylene-unsaturated carboxylic acid copolymer (a1-2) is preferably 10% by mass or more, more preferably 15% by mass or more, preferably 80% by mass or less, and more preferably 75% by mass or less relative to the total amount of ethylene-unsaturated carboxylic acid copolymer (a) contained in resin (X). However, the total content of the ethylene-unsaturated carboxylic acid copolymer (a1-1), the ethylene-unsaturated carboxylic acid copolymer (a1-2), and the ethylene-unsaturated carboxylic acid copolymer (a2) is 100% by mass.
[0076] Each of the two or more ethylene-unsaturated carboxylic acid copolymers (a) is obtained by polymerizing a monomer component containing ethylene and an unsaturated carboxylic acid according to the desired content of the structural unit derived from the unsaturated carboxylic acid.
[0077] Unsaturated carboxylic acid is a monomer having at least one ethylenically unsaturated bond and a carboxyl group. Examples of unsaturated carboxylic acids include monobasic acids having ethylenically unsaturated bonds, such as acrylic acid, methacrylic acid, and crotonic acid; dibasic acids having ethylenically unsaturated bonds, such as maleic acid, fumaric acid, and itaconic acid; and the like. Among the unsaturated carboxylic acids, monobasic acids having ethylenically unsaturated bonds are preferred from the viewpoint of water resistance, and acrylic acid and methacrylic acid are more preferred. These unsaturated carboxylic acids may be used alone or in combination of two or more.
[0078] The content ratio of ethylene in the monomer component can be appropriately set according to the content of the structural unit from ethylene of the obtained ethylene-unsaturated carboxylic acid copolymer. Similarly, the content ratio of the unsaturated carboxylic acid in the monomer component can be appropriately set according to the content of the structural unit from unsaturated carboxylic acid of the ethylene-unsaturated carboxylic acid copolymer.
[0079] The polymerization method of the monomer components is not particularly limited as long as the desired ethylene-unsaturated carboxylic acid copolymer can be obtained. As the polymerization method, for example, known polymerization methods can be cited. The ethylene-unsaturated carboxylic acid copolymer is obtained, for example, by contacting the monomer components with a polymerization initiator such as a peroxide under high temperature and high pressure conditions and polymerizing.
[0080] In addition, ethylene-unsaturated carboxylic acid copolymer can be obtained as a dispersion (aqueous dispersion) formed by its particles being dispersed in water. In such a case, it is possible to utilize the method described in, for example, Japanese Patent Publication No. 7-008933, Japanese Patent Publication No. 5-039975, Japanese Patent Publication No. 4-030970, Japanese Patent Publication No. 42-000275, Japanese Patent Publication No. 42-023085, Japanese Patent Publication No. 45-029909, Japanese Patent Publication No. 51-062890, Japanese Patent No. 4746337, etc., as a dispersion (aqueous dispersion). It should be noted that ethylene-unsaturated carboxylic acid copolymer has self-emulsification.
[0081] [Manufacturing of aqueous dispersion]
[0082] The aqueous dispersion can be obtained, for example, as described above, as a dispersion (aqueous dispersion) in which resin particles of the resin (X) containing two or more ethylene-unsaturated carboxylic acid copolymers (a) are dispersed in water. Specifically, it can be produced by dispersing the resin component containing two or more ethylene-unsaturated carboxylic acid copolymers in water preferably maintained at 100° C. or above, more preferably at 110° C. or above, or in an alkaline aqueous solution and stirring.
[0083] The aqueous dispersion obtained as described above can also contain additives except resin (X). As additives, for example, the above-mentioned emulsifier, curing agent, cross-linking agent, film-making aid, defoamer, anti-shrinkage agent, leveling agent, tackifier, hardness imparting agent, preservative, thickener, antifreeze agent, dispersant, inorganic pigment, organic pigment etc. can be enumerated. These additives can be used alone, or two or more can be used in combination. The addition of these additives and the period of addition etc. can be suitably set according to purpose and use.
[0084] [physical properties]
[0085] The melt flow rate (MFR ASTM D1238, 190°C, 2.16 kg load) of the resin (X) is preferably 0.1 g / 10 min or more, more preferably 0.5 g / 10 min or more, and is preferably 150 g / 10 min or less, more preferably 100 g / 10 min or less.
[0086] The weight average particle size (measurement method: light scattering measurement) of the resin particles of the resin (X) dispersed in the aqueous dispersion is preferably 0.01 μm or more, more preferably 0.02 μm or more, and is preferably 4.0 μm or less, more preferably 1.0 μm or less.
[0087] From the viewpoint of coating suitability, the viscosity of the aqueous dispersion at 25° C. (measured by Brookfield viscometer) is preferably 10 mPa·s or more, more preferably 50 mPa·s or more, and preferably 900 mPa·s or less, more preferably 500 mPa·s or less.
[0088] The nonvolatile content (solid content concentration) of the aqueous dispersion is preferably 20% by mass or more, more preferably 25% by mass or more, preferably 60% by mass or less, more preferably 55% by mass or less. The so-called nonvolatile content of the aqueous dispersion refers to the ratio of the components including the resin component remaining when the water of the aqueous dispersion is removed by heating or the like, relative to the aqueous dispersion.
[0089] The aqueous dispersion can be suitably used to form an adhesive layer (heat seal layer) of a laminate. The laminate having the adhesive layer is excellent in low-temperature adhesiveness, water resistance, and hot water resistance.
[0090] <Laminate>
[0091] The laminate of the present invention is a laminate having a substrate and an adhesive layer located on at least one surface of the aforementioned substrate and which can be made from the aforementioned aqueous dispersion. As described above, the adhesive layer comprises two or more ethylene-unsaturated carboxylic acid copolymers (a) having different contents of structural units from unsaturated carboxylic acids. The aforementioned adhesive layer may be present on one side of the substrate or on both sides of the substrate. In addition, the aforementioned adhesive layer may be present on the entire surface of the substrate or on a portion of the substrate.
[0092] [Base material]
[0093] Examples of the substrate include plastic films formed from plastic materials such as cellophane, polyethylene, ethylene-vinyl acetate copolymers, ionomers, polypropylene, polyamide (nylon), polyester, polyvinyl chloride, polyvinylidene chloride, polyvinyl alcohol, ethylene-vinyl alcohol copolymers, polycarbonate, polystyrene, polyacrylonitrile copolymers, and mixtures thereof; vapor-deposited films obtained by vapor-depositing metals such as aluminum, gold, silver, copper, nickel, zinc, titanium, cobalt, indium, and chromium, or inorganic oxides such as aluminum oxide and silicon oxide onto these plastic films; metal foils such as aluminum foil, paper, nonwoven fabrics, and the like.
[0094] There are no particular restrictions on the paper that can be used as the substrate of the above-mentioned laminate, and known paper with pulp as the main component can be used. Examples of the pulp that is the main component of the paper include chemical pulps such as LBKP (bleached kraft pulp of broadleaf trees) and NBKP (bleached kraft pulp of coniferous trees); mechanical pulps such as GP (groundwood), PGW (pressure groundwood), RMP (refiner mechanical pulp), TMP (thermomechanical pulp), CTMP (chemical thermomechanical pulp), CMP (chemical mechanical pulp), and CGP (chemical fine grinding pulp); wood pulps such as DIP (deinked pulp); non-wood pulps such as kenaf, bagasse, bamboo, and cotton; and the like. The density of these paper substrates is preferably 0.5 g / m 3 More preferably 0.7 g / m 3 above.
[0095] These may be used alone or in combination of two or more. For example, pulp containing 90 to 100% by mass of LBKP (bleached kraft pulp) may be used as the pulp.
[0096] Furthermore, the pulp may contain synthetic fibers within a range not impairing the effects of the present invention.
[0097] From the viewpoint of environmental protection, among the pulps, ECF (Elemental Chlorine Free) pulp, TCF (Total Chlorine Free) pulp, waste paper pulp, and pulp obtained from plantations are preferred.
[0098] The pulp beating degree is, for example, 200 to 700 ml CSF, preferably 450 to 620 ml CSF, in terms of Canadian Standard Freeness (JIS P 8121: 1995 "Test method for freeness of pulp").
[0099] As the paper used as the substrate, paper containing fillers may also be used. Examples of fillers include light calcium carbonate, heavy calcium carbonate, talc, clay, kaolin, calcined clay, titanium dioxide, and aluminum hydroxide. The filler content in the paper is, for example, 1 to 30 parts by mass relative to 100 parts by mass of the dry mass of the pulp. When light calcium carbonate is included as a filler, for example, 1 to 10 parts by mass of light calcium carbonate may be included relative to 100 parts by mass of the dry mass of the pulp.
[0100] In addition, the aforementioned paper may contain various known papermaking additives in addition to pulp. Examples of papermaking additives include internal paper strength enhancers such as sizing agents and wet paper strength enhancers; expanders, yield enhancers, filterability enhancers, coloring dyes, coloring pigments, fluorescent brighteners, fluorescent decolorizers, and pitch controllers. In addition, the paper used as the substrate may be a paper coated with a water-soluble polymer such as starch, polyvinyl alcohol, or polyacrylamide.
[0101] The papermaking method of the paper serving as the substrate is not particularly limited, and the paper can be manufactured by various papermaking machines such as a fourdrinier papermaking machine, a fourdrinier multilayer papermaking machine, a cylinder papermaking machine, a cylinder multilayer papermaking machine, a fourdrinier cylinder combination multilayer papermaking machine, and a sandwich papermaking machine. In addition, the paper used in the laminate of the present invention may be a single-layer papermaking machine, a multi-layer papermaking machine, or a multi-layer laminated product.
[0102] From the viewpoint that the adhesive layer included in the laminate has better heat sealability, among these substrates, metal foil such as aluminum foil, paper, nonwoven fabric, plastic film, and vapor-deposited film are preferred, and metal foil such as aluminum foil and paper are more preferred.
[0103] These substrates may be used alone or in combination of two or more.
[0104] The substrate may be subjected to pretreatment such as primer (titanate, polyethyleneimine, etc.) treatment, corona discharge treatment, chemical conversion treatment, etc., for the purpose of improving adhesion with the adhesive layer.
[0105] One or more layers different from the adhesive layer may be provided on the substrate. For example, when paper is used as the substrate, one or more coating layers may be provided. As the coating layer, for example, a pigment coating layer obtained from a coating liquid containing a pigment and an adhesive may be cited.
[0106] As the pigment contained in the pigment coating layer, known pigments used in the coating layer of conventional coated paper for printing can be used, and examples thereof include inorganic pigments such as calcium carbonate (heavy calcium carbonate, light calcium carbonate, etc.), kaolin (including clay), calcined clay, talc, magnesium carbonate, barium sulfate, calcium sulfate, titanium dioxide, zinc oxide, zinc sulfate, zinc carbonate, calcium silicate, aluminum silicate, magnesium silicate, diatomaceous earth, aluminum hydroxide, and magnesium hydroxide; and organic pigments (so-called plastic pigments) such as acrylic resins, styrene resins, vinyl chloride resins, nylon, and resins obtained by copolymerizing monomers constituting these resins.
[0107] As the pigment used in the pigment coating layer, for example, a combination of 20 to 40 parts by mass of kaolin and 60 to 80 parts by mass of heavy calcium carbonate can be used.
[0108] In addition, as the adhesive used in the pigment coating layer, a known adhesive used in the coating layer of a conventional coated printing paper can be used, and examples thereof include starches such as butadiene copolymer latex, crosslinker-modified starch, oxidized starch, enzyme-modified starch, esterified starch, etherified starch, cationic starch, and amphoteric starch; water-soluble polymers such as gelatin, casein, soy protein, and polyvinyl alcohol; and synthetic resins such as vinyl acetate, ethylene vinyl acetate, polyurethane resins, acrylic resins, polyester resins, and polyamide resins.
[0109] The mixing ratio of the pigment and the adhesive in the pigment coating layer is not particularly limited, but preferably the adhesive is 5 to 50 parts by mass relative to 100 parts by mass of the pigment. For example, a combination of 1 to 5 parts by mass of phosphated starch and 5 to 15 parts by mass of styrene butadiene latex adhesive relative to 100 parts by mass of the pigment can be used.
[0110] The pigment coating layer may contain various auxiliary agents as long as the effects of the present invention are not impaired, for example, viscosity modifiers, softeners, gloss imparting agents, water resistance agents, dispersants, flow modifiers, ultraviolet absorbers, stabilizers, antistatic agents, crosslinking agents, sizing agents, fluorescent whitening agents, colorants, pH adjusters, defoamers, plasticizers, and preservatives.
[0111] The coating amount of the coating liquid for forming such a pigment coating layer is, for example, 2 to 40 g / m2 in terms of non-volatile matter (solid matter) per side of the base paper. 2 .
[0112] [Adhesive layer]
[0113] The adhesive layer contained in the laminate of the present invention can be obtained, for example, by coating (applying) an aqueous dispersion containing the resin (X) on at least one surface of the aforementioned substrate, drying the layer formed by the coating, and removing at least a portion of volatile components such as water contained in the aforementioned aqueous dispersion.
[0114] There are no particular restrictions on the coating (application) method of the aqueous dispersion obtained in the present invention, and examples thereof include die coating, flow coating, spray coating, rod coating, gravure coating, gravure reverse coating, kiss reverse coating, micro gravure coating, roll coating, knife coating, rod coating, roll knife coating, air knife coating, comma roll coating, reverse roll coating, transfer roll coating, kiss roll coating, curtain coating, and printing.
[0115] The drying conditions for the layer formed from the applied material of the aqueous dispersion are not particularly limited as long as volatile components such as water from the aqueous dispersion can be removed. The drying temperature is, for example, 100 to 200° C. and the drying time is, for example, 10 seconds to 30 minutes.
[0116] The coating amount of the adhesive layer may be appropriately set according to the desired application, etc., and is preferably 1.5 g / m 2 More preferably 2.0 g / m 2 Above, preferably 13g / m 2 Below, preferably 10g / m 2 the following.
[0117] The ratio of the resin (X) in the adhesive layer may be appropriately set depending on the intended use, etc., and is preferably 50% by mass or more, and more preferably 80% by mass or more.
[0118] Regarding the water resistance of the adhesive layer, Cobb 300 (Cobb method: JIS P8140 contact time is 300 seconds) preferably 15 g / m 2 Below, more preferably 10g / m 2 the following.
[0119] The adhesive layer has excellent heat sealability at low temperatures. In addition, it is made from an aqueous dispersion having the above-mentioned resin particles. When the adhesive layer is made from the aqueous dispersion, the amount of organic solvent remaining in the adhesive layer is small, and the amount of residual organic solvent in the aforementioned adhesive layer can be set to preferably 100 ppm or less, more preferably 10 ppm or less.
[0120] [use]
[0121] The laminate obtained in the present invention can be suitably used as heat seal material in various industrial fields.By heat sealing, the base material contained in the laminate of the present invention and the adherend layer are pasted via the aforementioned adhesive layer.The aforementioned adherend layer can be contained in the laminate of the present invention, or can also be the layer contained in the article separated from the laminate of the present invention.
[0122] The adherend layer may include the same material as the base material included in the laminate. As the adherend layer, preferably metal foil such as aluminum foil, paper, nonwoven fabric, plastic film and vapor-deposited film, more preferably metal foil such as aluminum foil and paper. These adherend layers may be used alone or in combination of two or more.
[0123] The laminate of the present invention may also be a laminate comprising the aforementioned adherend layer in addition to the substrate and the adhesive layer. In this case, the substrate and the adherend layer may be pasted via the adhesive layer. When pasted, in the laminate of the present invention, the adherend layer is laminated on the surface opposite to the surface of the aforementioned adhesive layer that is in contact with the substrate.
[0124] There is no particular limitation on the method for heat-sealing the substrate and the adherend layer. For example, the substrate and the adherend layer included in the laminate may be superimposed via an adhesive layer and then heated and pressurized to perform heat sealing.
[0125] When the adherend layer further has an adhesive layer, the adhesive layer contained in the laminate of the present invention and the adhesive layer of the adherend layer may be superimposed on each other and then heated and pressed to perform heat sealing.
[0126] The heating temperature during heat sealing is, for example, 80° C. or more, preferably 100° C. or more, for example, 250° C. or less, preferably 200° C. or less. The pressure during heat sealing is, for example, 50 kPa or more, preferably 100 kPa or more, for example, 500 kPa or less, preferably 300 kPa or less.
[0127] The adhesive strength between the substrate and the adherend layer included in the laminate of the present invention can be evaluated by the peel strength between the substrate and the adherend layer. 2 The peel strength between the substrate and the adherend layer at 180 degrees peeling after 0.1 second of hot pressing under the conditions of , the tensile speed is 50 mm / min, and it is preferably 400 g / 15 mm or more, and more preferably 500 g / 15 mm or more.
[0128] A laminate obtained by laminating an adherend layer on at least one surface of an adhesive layer contained in the laminate as described above (in other words, a laminate obtained by laminating an adherend layer on at least one surface of an adhesive layer contained in the laminate) is included in the laminate of the present invention, regardless of its heat-sealed state (i.e., before and after heat sealing).
[0129] In addition, the laminate obtained in the present invention has excellent low-temperature adhesion, water resistance and hot water resistance. In addition, a water dispersion is used in the formation of the adhesive layer, and a dispersion in which resin particles are dispersed in an organic solvent such as ethyl acetate and toluene is not used, so the amount of residual organic solvent can be suppressed to a very small amount. Therefore, the laminate can be suitably used as a packaging material in various industrial fields. For example, it can be suitably used as a packaging material for food such as snacks, tea, and condiments; aromatics such as tobacco and fragrant wood; and various industrial products such as pharmaceuticals and paper.
[0130] Example
[0131] Hereinafter, the present invention will be described in more detail based on Examples, but the present invention is not limited to these Examples.
[0132] [Production Example 1]
[0133] A resin obtained by melt-kneading 50 parts by mass of an ethylene-methacrylic acid copolymer (resin B) having a methacrylic acid content of 15% by mass and 50 parts by mass of an ethylene-methacrylic acid copolymer (resin C) having a methacrylic acid content of 10% by mass, 4.4 parts by mass of sodium hydroxide, and 190 parts by mass of deionized water were placed in a reaction container, stirred, heated to 150° C. and maintained for 4 hours, and then cooled to room temperature to obtain a water dispersion 1 of resin particles 1 of resin 1. The average value of the content of the structural unit derived from methacrylic acid in resin 1 (acid content average value) was 12.5% by mass, and the weight average particle size of resin particles 1 was 0.5 μm. In addition, the viscosity of water dispersion 1 was 400 mPa·s, the non-volatile content (Nv) was 35%, and the melt flow rate (MFR) was 3.0 g / 10 minutes.
[0134] [Manufacturing Examples 2 and 3]
[0135] Aqueous dispersions 2 and 3 were obtained in the same manner as in Production Example 1 except that resins having the composition of Table 1 and resins having the composition of Table 2 were used instead of the resins including resin B and resin C in Production Example 1. Table 2 shows the physical property values.
[0136] [Production Example 4]
[0137] A mixture of 30 parts by mass of an ethylene-acrylic acid copolymer (resin A) having an acrylic acid content of 20.5% by mass and 70 parts by mass of an ethylene-methacrylic acid copolymer (resin E) having a methacrylic acid content of 4% by mass was fed from a feed hopper of a twin-screw extruder (manufactured by Ikegai Iron Works Co., Ltd., PCM-30, L / D=40) at a rate of 50 g / min, a 3.5% aqueous solution of potassium hydroxide was continuously fed at a rate of 28 g / min from a feed port provided in a vent portion of the extruder, and the mixture was continuously extruded at a heating temperature of 110° C. The extruded resin mixture was cooled to 90° C. in a static mixer with a jacket provided in the extruder port, and further introduced into warm water at 80° C., thereby obtaining an aqueous dispersion 4. The weight average particle size of the resin particles 4 was 0.9 μm. In addition, the viscosity of the aqueous dispersion 4 was 300 mPa·s, the nonvolatile content (Nv) was 37%, and the melt flow rate (MFR) was 1.0 g / 10 minutes.
[0138] [Manufacturing Examples 5 to 7] Manufacture of Aqueous Dispersions 5 to 7
[0139] Aqueous dispersions 5 to 7 were obtained in the same manner as in Production Example 1 except that the resins having the compositions in Table 1 and Table 2 were used instead of the resins containing the resins B and C in Production Example 1. Table 2 shows the physical property values.
[0140] [Table 1]
[0141] Resin A Resin B Resin C Resin D Resin E Ethylene 79.5 85 90 80 96 Methacrylic acid - 15 10 10 4 acrylic acid 20.5 - - - - Isobutyl acrylate - - - 10 - MFR(g / 10min@190℃) 300 60 500 35 7
[0142] [Table 2]
[0143] Aqueous dispersion 1 Aqueous dispersion 2 Aqueous dispersion 3 Aqueous dispersion 4 Aqueous dispersion 5 Aqueous dispersion 6 Aqueous dispersion 7 Resin A - 40 40 30 100 - - Resin B 50 20 30 - - 100 - Resin C 50 40 - - - - 100 Resin D 30 Resin E - - - 70 - - - Average acid content 12.5 15.2 15.7 9 20.5 15 10 Neutralizer (neutralization rate) NaOH (54%) KOH (30%) KOH (30%) KOH (30%) KOH (20%) NaOH (54%) NaOH (80%) Preparation method Autoclave Autoclave Autoclave Extrusion phase inversion Autoclave Autoclave Autoclave Resin input Melt Blending Melt Blending Melt Blending alone alone alone alone Nv(%) 35 42 42 37 42 27 33 Viscosity (mPa·s) 400 200 300 300 200 500 900 Particle size (μm) 0.5 0.5 0.5 0.9 0.3 0.02 3.8
[0144] Nv: non-volatile components
[0145] [Example 1]
[0146] The wax paper (weight 170g / m 2 ) as the substrate, an air knife coater was used to coat the resin in an amount of 6 g / m 2 The aqueous dispersion 1 was applied twice in a manner of , and dried at 130° C. for 20 seconds to obtain a paper coated product 1 as a laminate.
[0147] A soft aluminum foil (50 μm) was used as a substrate, and a bar coater was used to coat the resin in an amount of 3 g / m 2 The aqueous dispersion 1 was applied once in a manner of , and dried at 120° C. for 20 seconds to obtain an aluminum foil 1 as a laminate.
[0148] (Cobb value)
[0149] The Cobb value of the paper coated product 1 was measured by the Cobb method (JIS P8140) to determine the water absorption after 300 seconds (Cobb value). 300 ), and evaluated according to the criteria described in Table 3. The results are shown in Table 4.
[0150] (Cup hot water resistance)
[0151] Hot water at 95° C. or higher was poured into the paper cup molded using the above-mentioned paper coated product 1, and the cup was left for 1 hour. Water leakage from the sealed adhesive portion was observed and evaluated according to the criteria described in Table 3. The results are shown in Table 4.
[0152] (Low temperature adhesion)
[0153] At 110°C, 0.1 seconds, 1kg / cm 2 The resin-coated surfaces of the aluminum foil 1 were bonded together under the condition of , and the peel strength was measured under the condition of a tensile speed of 50 mm / min, and evaluated according to the criteria of Table 3. The results are shown in Table 4.
[0154] (Blocking resistance)
[0155] The aluminum foil 1 was cut into squares of 5 cm in length and width, and the coated surfaces were overlapped with each other. The aluminum foil was subjected to 45°C, 250 g / cm 2The blocking resistance was evaluated under the conditions of 100 ℃ and 24 hours. The results are shown in Table 4.
[0156] [Examples 2 to 4]
[0157] In Example 1, except that the above-mentioned water dispersions 2 to 4 were used instead of water dispersion 1, the same operation as in Example 1 was carried out to obtain paper coated products 2 to 4 and aluminum foils 2 to 4. Using the obtained paper coated products and aluminum foils, the various physical properties of Examples 2 to 4 were evaluated in the same manner as in Example 1. The results are shown in Table 4.
[0158] [Comparative Examples 1 to 3]
[0159] In Example 1, except that the above-mentioned water dispersions 5 to 7 were used instead of water dispersion 1, the same operation as in Example 1 was carried out to obtain paper coated products 5 to 7 and aluminum foils 5 to 7. Using the obtained paper coated products and aluminum foils, the physical properties of Comparative Examples 1 to 3 were evaluated in the same manner as in Example 1. The results are shown in Table 4.
[0160] [Table 3]
[0161]
[0162] [Table 4]
[0163]
[0164] [Measurement method]
[0165] (Average acid content)
[0166] After the resin was dealkalized, it was melted in tetrahydrofuran while hot and titrated with potassium hydroxide of a predetermined concentration under heating to measure the acid content, and the average acid content was calculated.
[0167] (Neutralization rate)
[0168] Measure the infrared absorption spectrum of the sample and find the 1700 cm-1 peak attributable to the carboxyl group. -1 The peak height a of the absorption is given by the formula (a). The peak height a corresponds to the number of carboxyl groups in the resin that are not ionically bonded.
[0169] The sample is brought into contact with hydrochloric acid to remove the metal ions in the resin (demetallization) and obtain an acid copolymer without ionic bonding (intramolecular crosslinking). The infrared absorption spectrum of the sample of the acid copolymer is measured to obtain the infrared absorption spectrum at 1700 cm -1 The peak height b of the absorption is corresponding to the total number of carboxyl groups in the resin.
[0170] From the obtained peak heights a and b, the neutralization ratio (%) was calculated by the following formula.
[0171] Neutralization rate (%) = 100 (1-a / b)
[0172] (Viscosity)
[0173] The viscosity was measured at 25°C using a B-type viscometer (manufactured by Toki Sangyo Co., Ltd.).
[0174] (Particle size)
[0175] The average particle size of the resin particles was measured using Nanotrac Wave II (Microtrac BEL).
[0176] (Melt flow rate)
[0177] The melt flow rate (MFR) was measured under the conditions of 190° C. and 2.16 kg load in accordance with ASTM D1238-65T.
Claims
1. A laminate comprising a substrate and an adhesive layer laminated on at least one surface of the substrate, The adhesive layer is obtained by drying a coating of an aqueous dispersion containing water and the resin (X). The resin (X) comprises two or more ethylene-unsaturated carboxylic acid copolymers (a) having different contents of structural units derived from unsaturated carboxylic acids. The two or more ethylene-unsaturated carboxylic acid copolymers (a) include one or more ethylene-unsaturated carboxylic acid copolymers (a1) in which the content of structural units derived from unsaturated carboxylic acid is 12% by mass or more and 30% by mass or less, and one or more ethylene-unsaturated carboxylic acid copolymers (a2) in which the content of structural units derived from unsaturated carboxylic acid is greater than 0% by mass and less than 12% by mass, The two or more ethylene-unsaturated carboxylic acid copolymers (a) satisfy at least one of the following conditions (i) and (ii), (i) as the ethylene-unsaturated carboxylic acid copolymer (a1), two or more ethylene-unsaturated carboxylic acid copolymers having different contents of structural units derived from unsaturated carboxylic acids are included; (ii) Two or more ethylene-unsaturated carboxylic acid copolymers having different contents of structural units derived from unsaturated carboxylic acids are included as the ethylene-unsaturated carboxylic acid copolymer (a2).
2. The laminate according to claim 1, wherein The total content of the structural units derived from unsaturated carboxylic acids contained in the two or more ethylene-unsaturated carboxylic acid copolymers (a) is 5% by mass or more and less than 18% by mass based on the total amount of structural units derived from monomers of the polymer contained in the resin (X).
3. The laminate according to claim 1 or 2, wherein: The ethylene-unsaturated carboxylic acid copolymer (a1) comprises: an ethylene-unsaturated carboxylic acid copolymer (a1-1) in which the content of the structural unit derived from the unsaturated carboxylic acid is 17% by mass or more and 30% by mass or less; and An ethylene-unsaturated carboxylic acid copolymer (a1-2) having a content of a structural unit derived from an unsaturated carboxylic acid of 12% by mass or more and less than 17% by mass.
Citation Information
Patent Citations
Aqueous dispersion, and laminate
CN106459524A
Aqueous dispersion, and laminate
CN107075197A
Aqueous adhesive for paper and laminate
JP2003213233A
Skin laminated film
JP2014151441A
Resin composition, heat-sealable film, and laminated film
WO2011152324A1