A method for producing high-viscosity long-carbon chain nylon by intermittent process

By controlling the pressure and temperature in the reactor and using a twin-screw extruder to perform a two-step viscosity-increasing reaction, the problems of low production efficiency and poor viscosity consistency of high-viscosity long carbon chain nylon in the existing technology are solved, and high-viscosity long-chain nylon is achieved. Stable and efficient production of carbon chain nylon.

CN115947937BActive Publication Date: 2024-10-01WUXI YINDA NYLON
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211687458.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-27
Publication Date
2024-10-01
Estimated Expiration
2042-12-27

AI Technical Summary

Technical Problem

It is difficult to produce high-viscosity long carbon chain nylon resin with existing technology, resulting in poor viscosity consistency in the reactor, reduced product quality, and low production efficiency.

Method used

The batch method is used to gradually increase the viscosity in the reaction kettle by inert gas replacement and pressure and temperature control, and a twin-screw extruder is used to perform a two-step viscosity increasing reaction to improve viscosity uniformity and production efficiency.

Benefits of technology

It achieves high-viscosity and stable production of long carbon chain nylon, avoids the problems of poor viscosity consistency and wide molecular weight distribution, and improves production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115947937B_ABST
    Figure CN115947937B_ABST
Patent Text Reader

Abstract

The present invention provides a method for producing high-viscosity long-chain nylon by an intermittent process, comprising the following steps: step S1, placing a dibasic acid, a diamine, deionized water, and an antioxidant in a reactor, and maintaining the pressure of the reactor by discharging the steam in the reactor during the reaction; step S2, transporting the long-chain nylon in the reactor to a first tackifier for polymerization, and staying for 30 to 90 minutes; step S3, transporting the long-chain nylon in the first tackifier to a second tackifier for continued polymerization, and obtaining high-viscosity long-chain nylon particles. The embodiment of the present invention first polymerizes in a reactor to obtain a long-chain nylon oligomer, avoiding the phenomenon of wide molecular weight distribution and sticking to the reactor wall due to high viscosity. The viscosity-increasing reaction adopts a two-step method, which improves the viscosity uniformity of the long-chain nylon in the intermittent production process, and greatly improves the production efficiency compared to the traditional solid phase viscosity-increasing method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of preparation and production of polymer materials, and in particular relates to a method for producing high-viscosity long-carbon chain nylon by an intermittent process. Background Art

[0002] Long-chain nylon usually refers to nylon with a methylene length of more than 10 carbon atoms in the chain segment, including nylon 11, nylon 12, nylon 1212, nylon 1012, nylon 1313, etc. From the chain structure of long-chain nylon resin, the methylene group in the macromolecular chain is relatively long and the amide group density is low. Therefore, in addition to most of the general properties of general nylon such as lubricity, wear resistance, compression resistance and easy processing, long-chain nylon also has high toughness and softness, low water absorption, good dimensional stability and other characteristics that conventional nylon 6 and nylon 66 do not have. Long-chain nylon is mostly used in the field of automotive pipelines, and long-chain nylon tubes are mostly formed by extrusion, so there are corresponding requirements for the viscosity of long-chain nylon resin.

[0003] The production of long carbon chain nylon resin is currently an intermittent process. Chinese patent CN112280032A discloses a method for preparing long carbon chain nylon, wherein a dibasic acid, a diamine, a solvent, an antioxidant and a catalyst are placed in a reactor, and a long carbon chain nylon resin is obtained through steps such as heating and pressure increase. The disadvantage of this method is that it is impossible to produce a long carbon chain nylon resin with high viscosity. Once the viscosity of the long carbon chain nylon in the reactor increases, the melt fluidity decreases significantly, and the discharge of the reactor becomes very difficult. Moreover, the high viscosity melt is easy to adhere to the inner wall of the reactor to form a retention layer, resulting in poor viscosity consistency and reduced product quality.

[0004] Chinese patent CN111100287A discloses a method for producing high-viscosity polyamide, which first uses a tubular reactor to obtain a polyamide melt with a relative viscosity of 2.6-3.6 by pre-polymerization under pressure and post-polymerization under reduced pressure. Then, it is transported by a melt gear pump and enters a horizontal high-viscosity self-cleaning reactor, where it flows from the feed end to the discharge end under the action of a rotor, while the polymerization reaction continues. This method requires continuous polymerization and is suitable for nylon 6, nylon 11, nylon 12, etc.

[0005] Chinese patent CN113881036A discloses a method for preparing long carbon chain nylon, using dibasic acid and diamine as raw materials to prepare nylon salt, and then using intermittent polymerization or solid phase post-condensation method to obtain long carbon chain nylon. The disadvantages of using solid phase post-condensation method are low reaction temperature, long reaction time, low production efficiency, and the reaction only reacts in the amorphous region of long carbon chain nylon, which easily leads to a widening of the molecular weight distribution of the product. Summary of the invention

[0006] The purpose of the present invention is to overcome the deficiencies in the prior art and provide a method for producing high-viscosity long-carbon-chain nylon by an intermittent process, wherein the long-carbon-chain nylon has stable viscosity and high production efficiency. To achieve the above technical purpose, the technical solution adopted in the embodiment of the present invention is:

[0007] The embodiment of the present invention provides a method for producing high-viscosity long-carbon chain nylon by an intermittent process, comprising the following steps:

[0008] Step S1, placing a dibasic acid, a diamine, a solvent, and an antioxidant in a reaction kettle, and continuously replacing the gas in the reaction kettle with an inert gas, and reserving the inert gas as a protective gas; increasing the pressure of the reaction kettle to 1.0-1.5 MPa, reacting for 1-4 hours, during which the pressure of the reaction kettle is maintained by discharging the steam in the reaction kettle, and then slowly releasing the gas to reduce the pressure of the reaction kettle to 0.05-0.1 MPa, while slowly raising the temperature to 240-260° C., and controlling the release time to be 1-4 hours; the relative viscosity of nylon in the reaction kettle is 1.20-1.50;

[0009] Step S2, continuously conveying the long carbon chain nylon in the reactor to the first viscosity increasing reactor for polymerization at a flow rate of 15 to 30 kg / hr, and staying in the first viscosity increasing reactor for 30 to 90 minutes, wherein the first viscosity increasing reactor is a vertical container and is provided with a ribbon screw agitator, wherein the ribbon screw agitator is used for mixing and conveying nylon, and the relative viscosity of the long carbon chain nylon at the outlet of the first viscosity increasing reactor is 2.0 to 2.30,

[0010] Step S3, continuously conveying the long carbon chain nylon in the first viscosity enhancer to the second viscosity enhancer at a flow rate of 15 to 30 kg / hr for continued polymerization, the second viscosity enhancer reactor is a twin-screw extruder, the twin-screw extruder includes three reaction zones and a compression conveying zone, the screw outer barrel of any reaction zone is provided with 1 to 3 exhaust ports, the relative viscosity of the long carbon chain nylon at the outlet of the second viscosity enhancer reactor is 2.60 to 2.90, the long carbon chain nylon at the outlet of the second viscosity enhancer is extruded, drawn, cooled, and pelletized to obtain high-viscosity long carbon chain nylon particles.

[0011] The solvent is selected from deionized water, ultrapure water and distilled water.

[0012] Further, in step S1, the dibasic acid is selected from dibasic acids of C10 to C20;

[0013] The diamine is selected from C10-C20 diamines.

[0014] Furthermore, in step S1, the molar ratio of the dibasic acid to the diamine is 1:1 to 1.06.

[0015] Furthermore, in step S1, the ratio of the weight of the solvent to the sum of the weights of the dibasic acid and the diamine is 1 to 2:1.

[0016] Furthermore, in step S1, the antioxidant is selected from one or more of copper compounds, phenol stabilizers, phosphite stabilizers, hindered amine stabilizers, triazine stabilizers, and ultraviolet light absorbers.

[0017] Furthermore, in step S1, the ratio of the weight of the antioxidant to the sum of the weight of the dibasic acid and the diamine is 0.1% to 1%:1.

[0018] Furthermore, in step S2, the reaction temperature of the first viscosity increasing reactor is 240-260° C. and the pressure is normal pressure.

[0019] Furthermore, in step S3, in the second viscosity increasing reactor, the reaction temperatures of the three reaction zones and the one compression conveying zone are set to 240-260° C.;

[0020] The three reaction zones include a first reaction zone, a second reaction zone and a third reaction zone. The absolute pressure of the first reaction zone is set to 80-100 KPa, the absolute pressure of the second reaction zone is set to 60-80 KPa, and the absolute pressure of the third reaction zone is set to 40-60 KPa.

[0021] Further, in step S3, the length of the first reaction zone accounts for 25-30% of the total screw length;

[0022] The length of the second reaction zone accounts for 25-30% of the total screw length;

[0023] The length of the third reaction zone accounts for 10-20% of the total screw length.

[0024] The technical solution provided by the embodiment of the present invention has the following beneficial effects:

[0025] The embodiment of the present invention provides a method for producing high-viscosity long-chain nylon by an intermittent method. First, a long-chain nylon oligomer with a relative viscosity of 1.2 to 1.5 is polymerized in an intermittent reactor, and the reaction pressure is controlled to maintain the appropriate viscosity and stable molecular weight of the long-chain nylon oligomer, thereby avoiding a wide molecular weight distribution due to high viscosity in the reactor, and even sticking to the reactor wall, which is beneficial to the next step of viscosity-increasing reaction. The viscosity-increasing reaction adopts a two-step method, and utilizes the strong self-cleaning ability of the twin-screw extruder to process high-viscosity long-chain nylon, thereby improving the viscosity uniformity of the long-chain nylon in the intermittent production process, and greatly improving the production efficiency compared to the traditional solid-phase viscosity-increasing method. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1This is a molecular weight distribution diagram of the long carbon chain nylon prepared by the method in Example 1 of the present invention.

[0027] Figure 2 This is the molecular weight distribution diagram of the long carbon chain nylon prepared by the method in Comparative Example 1 of the present invention.

[0028] Figure 3 This is the molecular weight distribution diagram of the long carbon chain nylon prepared by the method in Comparative Example 2 of the present invention. DETAILED DESCRIPTION

[0029] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0030] The present invention provides a method for producing high-viscosity long-carbon-chain nylon by an intermittent process, comprising the following steps:

[0031] Step S1, placing a dibasic acid, a diamine, a solvent, and an antioxidant in a reactor, and continuously replacing the gas in the reactor with an inert gas, and reserving the inert gas as a protective gas; increasing the pressure of the reactor to 1.0-1.5 MPa, reacting for 1-4 hours, during which the pressure of the reactor is maintained by discharging the steam in the reactor, and then slowly venting the gas to reduce the pressure of the reactor to 0.05-0.1 MPa, for example, 0.05 MPa, 0.06 MPa, 0.07 MPa, 0.08 MPa, 0.09 MPa, 0.1 MPa, etc., while slowly heating to 240-260° C., and controlling the venting time to be 1-4 hours; the relative viscosity of nylon in the reactor is 1.20-1.50;

[0032] It should be noted that when the pressure of the reactor drops to the set pressure, stop venting, maintain the pressure of the reactor at the set pressure, and maintain the temperature of the reactor at the set temperature. If the pressure of the reactor is lower than the set pressure, steam can be introduced to maintain the pressure of the reactor. At this time, since there is still a small amount of water in the reaction system, the viscosity of the system is not high, and the phenomenon of material hanging on the wall of the reactor will not occur. As long as the pressure of the reactor remains stable and the gas-liquid two-phase equilibrium state is maintained, the molecular weight of nylon in the reactor will also remain stable, which is conducive to the subsequent viscosity-increasing reaction.

[0033] Step S2, continuously conveying the long carbon chain nylon in the reactor to the first viscosity enhancer for polymerization at a flow rate of 15 to 30 kg / hr, for example, the flow rate can be 15 kg / hr, 18 kg / hr, 20 kg / hr, 22 kg / hr, 25 kg / hr, 28 kg / hr, 30 kg / hr, etc., and staying in the first viscosity enhancer reactor for 30 to 90 minutes, for example, 30 minutes, 40 minutes, 50 minutes, 60 minutes, 70 minutes, 80 minutes, 90 minutes, etc., the first viscosity enhancer reactor is a vertical container and is provided with a ribbon screw agitator, the ribbon screw agitator is used to mix and convey nylon, and the relative viscosity of the long carbon chain nylon at the outlet of the first viscosity enhancer reactor is 2.0 to 2.30;

[0034] Step S3, continuously conveying the long carbon chain nylon in the first viscosity enhancer to the second viscosity enhancer at a flow rate of 15 to 30 kg / hr for continued polymerization. For example, the flow rate can be 15 kg / hr, 18 kg / hr, 20 kg / hr, 22 kg / hr, 25 kg / hr, 28 kg / hr, 30 kg / hr, etc. The second viscosity enhancer reactor is a twin-screw extruder, which includes three reaction zones and a compression and conveying zone. The outer barrel of the screw in any reaction zone is provided with 1 to 3 exhaust ports. The relative viscosity of the long carbon chain nylon at the outlet of the second viscosity enhancer reactor is 2.60 to 2.90. The long carbon chain nylon at the outlet of the second viscosity enhancer is extruded, drawn, cooled, and pelletized to obtain high-viscosity long carbon chain nylon particles.

[0035] Furthermore, in step S1, the solvent is selected from deionized water, ultrapure water, and distilled water.

[0036] Further, in step S1, the dibasic acid is selected from dibasic acids of C10 to C20, such as dodecanedioic acid;

[0037] The diamine is selected from C10-C20 diamines, such as decanediamine.

[0038] Furthermore, in step S1, the molar ratio of the dibasic acid to the diamine is 1:1 to 1.06, for example, 1:1, 1:1.01, 1:1.02, 1:1.03, 1:1.04, 1:1.05, 1:1.06, etc. Since the diamine has a low boiling point, a small amount of diamine will volatilize during the exhaust process. In order to obtain a higher viscosity, when feeding, the diamine needs to be slightly excessive to compensate for the loss of diamine during the exhaust process.

[0039] Furthermore, in step S1, the molar ratio of the dibasic acid to the diamine is 1:1 to 1.02.

[0040] Furthermore, in step S1, the ratio of the weight of the solvent to the sum of the weights of the dibasic acid and the diamine is 1 to 2:1, for example, 1:1, 1.2:1, 1.5:1, 1.7:1, 2:1, etc.

[0041] Furthermore, in step S1, the antioxidant is selected from one or more of copper compounds, phenol stabilizers, phosphite stabilizers, hindered amine stabilizers, triazine stabilizers, and ultraviolet light absorbers.

[0042] Furthermore, in step S1, the ratio of the weight of the antioxidant to the sum of the weight of the dibasic acid and the diamine is 0.1% to 1%:1, for example, it can be 0.1%:1, 0.3%:1, 0.5%:1, 0.7%:1, 1.0%:1, etc.

[0043] Furthermore, in step S2, the reaction temperature of the first viscosity increasing reactor is 240-260° C. and the pressure is normal pressure.

[0044] Further, in step S3, in the second viscosity increasing reactor, the reaction temperature of the three reaction zones and the one compression conveying zone is set to 240-260°C, for example, 240°C, 245°C, 250°C, 255°C, 260°C, etc.;

[0045] The three reaction zones include a first reaction zone, a second reaction zone and a third reaction zone. The absolute pressure of the first reaction zone is set to 80-100 KPa, for example, 80 KPa, 85 KPa, 90 KPa, 95 KPa, 100 KPa, etc. The absolute pressure of the second reaction zone is 60-80 KPa, for example, 60 KPa, 65 KPa, 70 KPa, 75 KPa, 80 KPa, etc. The absolute pressure of the third reaction zone is 40-60 KPa, for example, 40 KPa, 45 KPa, 50 KPa, 55 KPa, 60 KPa, etc.

[0046] Further, in step S3, the length of the first reaction zone accounts for 25-30% of the total screw length;

[0047] The length of the second reaction zone accounts for 25-30% of the total screw length;

[0048] The length of the third reaction zone accounts for 10-20% of the total screw length.

[0049] In the following specific examples, the operations involved were carried out under conventional conditions or conditions recommended by the manufacturer without specifying the conditions. All raw materials without specifying the manufacturer and specifications are conventional products that can be obtained from the market.

[0050] Example 1

[0051] A method for producing high-viscosity long-carbon chain nylon by an intermittent process comprises the following steps:

[0052] Step S1, add 50kg of dodecanedioic acid, 37kg of decanediamine, 100kg of deionized water, and 50g of antioxidant 1098 into a 300L reactor, fill with nitrogen to make the reactor pressure reach 1MPa, discharge the nitrogen to reduce the reactor pressure to 0.1MPa, and do this three times; introduce high-temperature heat transfer oil into the reactor jacket, increase the pressure of the reactor, start stirring, when the reactor pressure reaches 1.5MPa, open the reactor exhaust valve to discharge steam so that the reactor pressure is maintained at 1.5MPa, after reacting for 2 hours, slowly open the exhaust valve to slowly reduce the reactor pressure, and slowly increase the reactor temperature until the reactor pressure reaches 0.08MPa, maintain the reactor pressure at 0.08MPa, and adjust the temperature of the heat transfer oil to maintain the reactor temperature at 240°C.

[0053] Step S2, opening the bottom valve of the reactor and the melt pump, and conveying the material to the first viscosity-increasing reactor at a flow rate of 25 kg / hr; the first viscosity-increasing reactor is a 50L vertical reactor with a ribbon screw stirrer, the reaction temperature is 240°C, and the pressure is normal pressure;

[0054] Step S3, when the liquid level of the first viscosity enhancer reaches a certain value, open the bottom valve of the first viscosity enhancer reactor and the melt pump to transport materials to the second viscosity enhancer reactor at a flow rate of 25kg / hr; the second viscosity enhancer reactor is a twin-screw extruder with a screw diameter of 36mm and a screw aspect ratio of 68. The screw speed is 300rpm to maintain a material flow rate of 25kg / hr. The heating zone 1-3 is the first reaction zone, the temperature is 240°C, the two exhaust ports are connected to the vacuum pump, and the absolute pressure is 90KPa; the heating zone 4-6 is the second reaction zone, the temperature is 245°C, the two exhaust ports are connected to the vacuum pump, and the absolute pressure is 75KPa; the heating zone 7-8 is the third reaction zone, the temperature is 250°C, one exhaust port is connected to the vacuum pump, the absolute pressure is 60KPa, and the heating zone 9-8 is the compression and conveying zone, the temperature is 250°C; the long carbon chain nylon obtained at the outlet of the second viscosity enhancer reactor is extruded, stretched, cooled, and pelletized to obtain high-viscosity long carbon chain nylon particles.

[0055] The present application tests the relative viscosity and melt index of the long carbon chain nylon provided in Example 1. Specifically, the test is performed according to the following method:

[0056] 1) Relative viscosity:

[0057] Weigh 1g of long carbon chain nylon accurately, add it to 100ml of 96% sulfuric acid, and stir to dissolve at 20-30℃. After complete dissolution, take the solution and place it in an Ubbelohde viscometer. After placing it in a constant temperature bath at 25℃ for 10 minutes, measure the falling speed and mark it as t. In addition, measure the falling speed of 96% sulfuric acid at the same time and mark it as t0. According to the formula: relative viscosity = t / t0, calculate the relative viscosity of long carbon chain nylon.

[0058] 2) Melt index:

[0059] When long carbon chain nylon flows through a capillary with a diameter of 1.18 mm at 235°C and a load of 2.16 kg, the outflow mass within 10 minutes is the melt index.

[0060] The long carbon chain nylon in Example 1 was sampled and analyzed at different time points. The analysis results are shown in Table 1:

[0061]

[0062] Comparative Example 1

[0063] The one-step process for producing high viscosity long carbon chain nylon includes the following steps:

[0064] 50kg of dodecanedioic acid, 37kg of decanediamine, 100kg of deionized water and 50g of antioxidant 1098 were added into a 300L reactor, and nitrogen was introduced to make the reactor pressure reach 1MPa, and the nitrogen was discharged to reduce the reactor pressure to 0.1MPa. This operation was repeated three times, and high-temperature heat transfer oil was introduced into the reactor jacket to increase the pressure of the reactor. The stirring was started. When the reactor pressure reached 1.5MPa, the exhaust valve of the reactor was opened to discharge steam to keep the reactor pressure at 1.5MPa. After reacting for 2 hours, the exhaust valve was slowly opened to reduce the reactor pressure slowly, and the reactor temperature was slowly increased. The pressure dropped to normal pressure and the temperature was maintained at 250°C. After reacting for 1 hour, the reaction was continued at an absolute pressure of 80KPa for 30 minutes, and the material was discharged. During the discharging process, the discharging was normal in the early stage, and there were a large number of bubbles in the strips in the later stage. The strips were easily broken and could not be pelletized normally. Finally, high-viscosity long-chain nylon particles were obtained. The relative viscosity of the high-viscosity long-chain nylon particles was 2.69.

[0065] When the one-step method was continued to be used to produce the second batch of high-viscosity long-chain nylon, the heating and exhaust time became longer, and the material strips were uneven during discharging. There were also a large number of bubbles in the later stage of discharging, and qualified high-viscosity long-chain nylon particles could not be obtained.

[0066] Comparative Example 2

[0067] The two-step process for producing high viscosity long carbon chain nylon includes the following steps:

[0068] Step S1, add 50kg of dodecanedioic acid, 37kg of decanediamine, 100kg of deionized water, and 50g of antioxidant 1098 into a 300L reactor, fill with nitrogen to make the reactor pressure reach 1MPa, discharge the nitrogen to reduce the reactor pressure to 0.1MPa, and do this three times, introduce high-temperature heat transfer oil into the reactor jacket, increase the pressure of the reactor, start stirring, and when the reactor pressure reaches 1.5MPa, open the exhaust valve of the reactor to discharge steam to keep the reactor pressure at 1.5MPa, react for 2 hours, slowly open the exhaust valve to slowly reduce the reactor pressure, slowly increase the reactor temperature, reduce the pressure to normal pressure, and maintain the temperature at 250°C. After reacting for 1 hour, discharge the material in the reactor, and obtain low-viscosity long-carbon chain nylon particles through extrusion, drawing, cooling, and pelletizing. The relative viscosity of the low-viscosity long-carbon chain nylon is 2.18;

[0069] Step S2, placing 50 kg of low-viscosity long-carbon-chain nylon particles into a 300 L vacuum drum, reacting at 150° C. and an absolute pressure of 20 KPa for 24 hours to obtain high-viscosity long-carbon-chain nylon, wherein the relative viscosity of the high-viscosity long-carbon-chain nylon is 2.60.

[0070] The present application evaluates the molecular weight of the long carbon chain nylon prepared in Example 1 and Comparative Examples 1-2, and uses gel permeation chromatography (GPC) to measure the molecular weight distribution of the long carbon chain nylon. Figure 1 The figure shows the molecular weight distribution of the long carbon chain nylon obtained by the intermittent method for producing high viscosity long carbon chain nylon in Example 1. Figure 2 The figure shows the molecular weight distribution of long carbon chain nylon obtained by the one-step method for producing high viscosity long carbon chain nylon in Comparative Example 1. Figure 3 The figure shows the molecular weight distribution of long carbon chain nylon obtained by the two-step method for producing high viscosity long carbon chain nylon in Comparative Example 2. The specific values ​​are shown in Table 2 below:

[0071]

[0072] From Table 1-2 and Figure 1-3 , we can see that:

[0073] 1) The high-viscosity long-carbon-chain nylon produced by the one-step method in Comparative Example 1 has a wide molecular weight distribution, a large amount of residual material in the reactor, unstable quality, and even causes subsequent normal production failure.

[0074] 2) The high-viscosity long-carbon-chain nylon produced by the two-step method in Comparative Example 2 has a relatively mature process, but the production efficiency is low, the molecular weight distribution of the long-carbon-chain nylon shows a double peak, and the viscosity consistency is poor.

[0075] 3) The high-viscosity long-carbon-chain nylon produced by the intermittent method in Example 1 of the present invention has a short production time and high efficiency. At the same time, the long-carbon-chain nylon has a narrow molecular weight distribution, stable viscosity and good quality.

[0076] Finally, it should be noted that the above specific implementation methods are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.

Claims

1. A method for producing high-viscosity long-carbon chain nylon by an intermittent process, characterized in that: The following steps are involved: Step S1, placing a dibasic acid, a diamine, a solvent, and an antioxidant in a reaction kettle, and continuously replacing the gas in the reaction kettle with an inert gas, and reserving the inert gas as a protective gas; increasing the pressure of the reaction kettle to 1.0-1.5 MPa, reacting for 1-4 hours, during which the pressure of the reaction kettle is maintained by discharging the steam in the reaction kettle, and then slowly releasing the gas to reduce the pressure of the reaction kettle to 0.05-0.1 MPa, while slowly raising the temperature to 240-260° C., and controlling the release time to be 1-4 hours; the relative viscosity of nylon in the reaction kettle is 1.20-1.50; Step S2, continuously conveying the long carbon chain nylon in the reactor to the first viscosity increasing reactor at a flow rate of 15 to 30 kg / hr for polymerization, and retaining it in the first viscosity increasing reactor for 30 to 90 minutes, wherein the first viscosity increasing reactor is a vertical container and is provided with a spiral screw agitator, wherein the spiral screw agitator is used for mixing and conveying the nylon, the reaction temperature of the first viscosity increasing reactor is 240 to 260° C., the pressure is normal pressure, and the relative viscosity of the long carbon chain nylon at the outlet of the first viscosity increasing reactor is 2.0 to 2.30; Step S3, continuously conveying the long carbon chain nylon in the first viscosity enhancer to the second viscosity enhancer at a flow rate of 15 to 30 kg / hr for continued polymerization, the second viscosity enhancer reactor is a twin-screw extruder, the twin-screw extruder includes three reaction zones and one compression conveying zone, in the second viscosity enhancer reactor, the reaction temperature of the three reaction zones and one compression conveying zone is set to 240 to 260° C.; the three reaction zones include a first reaction zone, a second reaction zone and a third reaction zone, the absolute pressure of the first reaction zone is set to 80 to 100 KPa, the absolute pressure of the second reaction zone is set to 60 to 80 KPa, and the absolute pressure of the third reaction zone is set to 40 to 60 KPa, 1 to 3 exhaust ports are provided on the outer barrel of the screw of any reaction zone, the relative viscosity of the long carbon chain nylon at the outlet of the second viscosity enhancer reactor is 2.60 to 2.90, and the long carbon chain nylon at the outlet of the second viscosity enhancer is extruded, drawn, cooled, and pelletized to obtain high-viscosity long carbon chain nylon particles; The relative viscosity is as follows: accurately weigh 1g of long carbon chain nylon, add it to 100ml of sulfuric acid with a mass concentration of 96%, and stir to dissolve at 20-30°C; after complete dissolution, take the solution and place it in an Ubbelohde viscometer, place it in a constant temperature bath at 25°C for 10 minutes, and then measure the decreasing speed, marked as t; in addition, simultaneously measure the decreasing speed of 96% sulfuric acid, marked as t0; according to the formula: relative viscosity = t / t0, calculate the relative viscosity of the long carbon chain nylon.

2. The method for producing high-viscosity long-carbon-chain nylon by an intermittent process as claimed in claim 1, characterized in that: The solvent is selected from deionized water, ultrapure water and distilled water.

3. The method for producing high-viscosity long-carbon-chain nylon by an intermittent process as claimed in claim 1, characterized in that: In step S1, the dibasic acid is selected from dibasic acids of C10 to C20; The diamine is selected from C10-C20 diamines.

4. The method for producing high-viscosity long-carbon-chain nylon by an intermittent process as claimed in claim 1, characterized in that: In step S1, the molar ratio of the dibasic acid to the diamine is 1:1 to 1.

06.

5. The method for producing high-viscosity long-carbon-chain nylon by an intermittent process as claimed in claim 1, characterized in that: In step S1, the ratio of the weight of the solvent to the sum of the weights of the dibasic acid and the diamine is 1 to 2:

1.

6. The method for producing high-viscosity long-carbon-chain nylon by an intermittent process as claimed in claim 1, characterized in that: In step S1, the antioxidant is selected from one or more of copper compounds, phenol stabilizers, phosphite stabilizers, hindered amine stabilizers, and triazine stabilizers.

7. The method for producing high-viscosity long-carbon-chain nylon by an intermittent process as claimed in claim 1, characterized in that: In step S1, the ratio of the weight of the antioxidant to the sum of the weight of the dibasic acid and the diamine is 0.1% to 1%:

1.

8. The method for producing high-viscosity long-carbon-chain nylon by an intermittent process as claimed in claim 1, characterized in that: In step S3, the length of the first reaction zone accounts for 25-30% of the total screw length; The length of the second reaction zone accounts for 25-30% of the total screw length; The length of the third reaction zone accounts for 10-20% of the total screw length.