A method for preparing graphene by recycling graphite negative electrode of waste lithium-ion batteries
Preparing high-quality graphene from waste lithium-ion batteries through the electrochemical cathode stripping method solves the problem of resource recovery and carbon resource shortage of waste graphite in lithium-ion batteries, and achieves low-cost, high-performance graphene production, which is suitable for a variety of applications. Application areas.
Patent Information
- Application Number
- CN202310012383.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-05
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-01-05
AI Technical Summary
Existing technology makes it difficult to effectively utilize and recycle waste graphite in lithium-ion batteries, leading to a shortage of carbon resources and environmental pollution, and the cost of raw materials for producing graphene is high.
The electrochemical cathode stripping method is used to purify graphite from used lithium-ion batteries, and high-quality, low-defect graphene is prepared through steps such as ultrasonic treatment, electrolytic stripping, and freeze-drying to maximize resource recycling.
It saves production costs and achieves the preparation of high-quality graphene with a conductivity of 10,000 to 20,000 S/cm and a layer number of 1 to 3. It is suitable for new energy batteries, industrial catalysts and biomedical materials.
Smart Images

Figure CN115959654B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of graphene preparation, and in particular to a method for preparing graphene by utilizing recycled graphite negative electrodes of waste lithium-ion batteries. Background Art
[0002] As a green and environmentally friendly secondary power source, lithium-ion batteries have developed rapidly in recent years due to their advantages such as high specific capacity, high operating voltage, low self-discharge, good cycle performance, long service life, and no memory effect. Lithium-ion batteries are composed of a positive electrode, a negative electrode, a diaphragm, an electrolyte, and a shell. Graphite is widely used in the negative electrode material of lithium-ion batteries because of its good conductivity, orderly layered crystal structure, high reversible lithium storage capacity, low charge and discharge potential, long and stable platform, etc. While the lithium-ion battery industry is developing rapidly, a large amount of waste graphite will be generated. These resources can be turned into treasure after purification. If these waste graphites are made into high-quality graphene, it will alleviate the shortage of carbon resources, avoid environmental pollution, and promote the sustainable development of the graphene industry. In addition, the raw material cost of waste graphite is much lower than the cost of high-purity graphite, and it is suitable for making raw materials for producing graphene. Therefore, the present invention adopts an electrochemical cathode stripping method to strip pre-purified waste graphite to prepare graphene, which can save production costs and can be re-applied to lithium-ion batteries, realizing the maximization of comprehensive resource utilization. In addition, compared with the electrochemical anodic stripping method (BD Ossonon, D. Belanger. Functionalization of graphene sheets by the diazonium chemistry during electrochemical exfoliation of graphite [J]. Carbon, 2017, 11: 83-93.), the cathode stripping method produces some hydrogen during the cathode electrolysis process, which can prevent the cathode graphite or the stripped graphene from being oxidized. The prepared graphene has very little oxygen content, so there is no need for reduction, and graphene with fewer defects and a low number of layers can be obtained in one step. The conductivity of the graphene prepared by the present invention is 10000-20000 S / cm, the number of layers is 1-3 layers, and the specific surface area is 800-1000m 2 / g. Summary of the invention
[0003] The present invention utilizes recycled waste graphite to prepare high-quality, low-defect graphene through an electrochemical cathode stripping method, thereby realizing resource recycling of waste graphite and alleviating the shortage of carbon resources.
[0004] The method for preparing graphene provided by the present invention comprises the following specific steps:
[0005] (1) Graphite purification: soak the waste lithium-ion battery in a saturated sodium chloride solution for 1 to 3 days to release the charge stored in the battery; disassemble the battery to remove the negative electrode copper foil with graphite attached, put it in an organic solvent, and perform ultrasonic treatment for 30 to 60 minutes to separate the negative electrode copper foil and the graphite negative electrode; collect the separated graphite negative electrode, repeatedly rinse the collected graphite negative electrode filter cake with distilled water for 4 to 6 times through a vacuum filter, then place the filter cake in a drying oven at 60°C to dry for 30 to 60 minutes, and then grind the filter cake into powder; after the powder is sieved, it is calcined in a tubular furnace with an inert protective gas to remove impurities, the calcination temperature is 400 to 600°C, and the time is 2 to 4 hours to obtain purified graphite powder;
[0006] (2) Tableting: The purified graphite powder is pressed into graphite sheets with a thickness of 0.5 to 3 mm using a powder tablet press;
[0007] (3) Electrolytic stripping treatment: The electrolyte is placed in an electrolytic cell, and then the pressed graphite sheet is bound with a nickel mesh and placed in the electrolytic cell as a cathode, and the platinum sheet is used as an anode. The graphite sheet as the cathode is first pre-electrolyzed at 18V for 30 to 60 minutes, and then electrolytically stripped at a voltage of 20 to 30V. The graphite sheet gradually expands and strips to produce graphene, which is suspended on the surface of the electrolyte.
[0008] (4) Vacuum filtration treatment: The electrolyte after electrolytic stripping is cleaned by a vacuum filtration device, and the cathode-stripped graphene is cleaned in sequence with N,N-dimethylformamide DMF, DMF and H2O with a volume ratio of 1:1, DMF and 5 wt.% HCl solution with a volume ratio of 1:1, and DMF and C2H5OH with a volume ratio of 1:1, and then repeatedly rinsed with distilled water for 4 to 6 times to obtain a graphene solution;
[0009] (5) Ultrasonic treatment: The graphene solution is subjected to ultrasonic treatment, and the process parameters of the ultrasonic treatment are power 70 to 120 W, ultrasonic frequency 45 to 60 Hz, and ultrasonic time 30 to 60 min;
[0010] (6) Freeze drying: The graphene solution after ultrasonic treatment is placed in an evaporating dish, and the outlet of the evaporating dish is sealed with filter paper for freeze drying. Pre-freeze for 8 to 10 hours, then dry for 24 to 30 hours, and finally grind the dried graphene into powder, and sieve the powder to prepare the final graphene product.
[0011] The graphite negative electrode recovered from the waste lithium-ion battery in step (1) is waste high-temperature pyrolytic graphite, artificial graphite or natural flake graphite.
[0012] The organic solvent in step (1) is NMP, anhydrous ethanol or DMF.
[0013] The protective gas used for calcination in step (1) is nitrogen, argon or helium.
[0014] The electrolyte in step (3) is mainly composed of an organic solvent, lithium perchlorate (LiClO4) and tetrabutylammonium hexafluorophosphate (TBAPF6).
[0015] The organic solvent in the electrolyte of step (3) is propylene carbonate PC, N,N-dimethylformamide DMF or dimethyl sulfoxide DMSO.
[0016] The concentration of lithium perchlorate LiClO4 in the electrolyte of step (3) is 0.1 mol / L, and the concentration of tetrabutylammonium hexafluorophosphate TBAPF6 is 0.1 mol / L.
[0017] The electrolytic stripping voltage of step (3) is 26 to 30V.
[0018] The vacuum degree of the freeze-drying in step (6) is 2-10 Pa.
[0019] The graphene prepared by the method for preparing graphene by recycling graphite negative electrodes of waste lithium-ion batteries is applied in the fields of new energy batteries, industrial catalysts and biomedical materials.
[0020] The present invention has the following beneficial effects: the graphene prepared from waste graphite generated in lithium batteries can realize the recycling of waste resources, saving part of the raw material capital cost, and producing high-value-added and high C:O mass ratio graphene products by cathode stripping method, and the performance of the corresponding products is as follows: the conductivity of graphene is 10000-20000S / cm, the number of layers is 1-3, and the specific surface area is 800-1000m 2 / g. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a SEM image of high-quality graphene obtained from recycled waste graphite in Example 2 of the present invention.
[0022] Figure 2 This is the XPS image of graphene in Example 2 of the present invention.
[0023] Figure 3 This is a Raman image of graphene according to Example 2 of the present invention. DETAILED DESCRIPTION
[0024] The features of the present invention are further described below by way of examples:
[0025] Embodiment 1:
[0026] The method for preparing graphene provided by the present invention comprises the following specific steps:
[0027] (1) Graphite purification: soak the waste lithium-ion battery in a saturated sodium chloride solution for 1 to 3 days to release the charge stored in the battery; disassemble the battery to remove the negative electrode copper foil with graphite attached, put it in an organic solvent, and perform ultrasonic treatment for 60 minutes to separate the negative electrode copper foil and the graphite negative electrode; collect the separated graphite negative electrode, repeatedly rinse the collected graphite negative electrode filter cake with distilled water for 6 times through a vacuum filter, then place the filter cake in a drying oven at 60°C to dry for 60 minutes, and then grind the filter cake into powder; after the powder is sieved, it is calcined and impurities are removed in a tubular furnace with an inert protective gas, the calcination temperature is 500°C, and the time is 3 hours to obtain purified graphite powder;
[0028] (2) tabletting: using a powder tabletting machine to press the purified graphite powder into graphite sheets with a thickness of 0.5 to 3 mm;
[0029] (3) Electrolytic stripping treatment: The electrolyte is placed in the electrolytic cell, and then the pressed graphite sheet is bound with a nickel mesh and placed in the electrolytic cell as the cathode, and the platinum sheet is used as the anode. The graphite sheet as the cathode is first pre-electrolyzed at a voltage of 18V for 30 minutes, and then electrolytically stripped at a voltage of 26V. The graphite sheet gradually expands and strips to produce graphene, which is suspended on the surface of the electrolyte. The hydrogen produced at the cathode in the cathode stripping method can prevent the oxidation of graphite or graphene and play a role in atmosphere protection.
[0030] (4) Vacuum filtration treatment: The electrolyte after electrolytic stripping is cleaned by a vacuum filtration device, and the cathode-stripped graphene is cleaned in sequence with N,N-dimethylformamide DMF, DMF and H2O with a volume ratio of 1:1, DMF and 5 wt.% HCl solution with a volume ratio of 1:1, and DMF and C2H5OH with a volume ratio of 1:1, and then repeatedly rinsed with distilled water for 6 times to obtain a graphene solution;
[0031] (5) Ultrasonic treatment: The graphene solution is subjected to ultrasonic treatment, and the process parameters of the ultrasonic treatment are power 70 W, ultrasonic frequency 45 Hz, and ultrasonic time 60 min;
[0032] (6) Freeze drying: The graphene solution after ultrasonic treatment is placed in an evaporating dish, and the outlet of the evaporating dish is sealed with filter paper, and then the evaporating dish is placed in the tray of the freeze dryer. The freezing button is turned on, and the pre-freezing is performed for 10 hours. Then, the vacuum gauge and the vacuum button are turned on for drying, and the drying time is 30 hours. Finally, the dried graphene is placed in a powder pulverizer for powdering, and the powder is sieved to prepare the final graphene product.
[0033] The graphite negative electrode recovered from the waste lithium-ion battery in step (1) is waste high-temperature pyrolytic graphite, artificial graphite or natural flake graphite.
[0034] The organic solvent in step (1) is NMP, anhydrous ethanol or DMF.
[0035] The protective gas used for calcination in step (1) is nitrogen, argon or helium.
[0036] The electrolyte in step (3) is mainly composed of an organic solvent, lithium perchlorate LiClO4 and tetrabutylammonium hexafluorophosphate TBAPF6.
[0037] The organic solvent in the electrolyte of step (3) is propylene carbonate PC, N,N-dimethylformamide DMF or dimethyl sulfoxide DMSO.
[0038] The concentration of lithium perchlorate LiClO4 in the electrolyte of step (3) is 0.1 mol / L, and the concentration of tetrabutylammonium hexafluorophosphate TBAPF6 is 0.1 mol / L.
[0039] The vacuum degree of the freeze-drying in step (6) is 2-10 Pa.
[0040] The graphene prepared by the method for preparing graphene by recycling graphite negative electrodes of waste lithium-ion batteries can be applied to the fields of new energy batteries, industrial catalysts, and biomedical materials.
[0041] The properties of the graphene obtained in Example 1 are as follows: the conductivity of the graphene is 15350 S / cm, the number of layers is 1 to 3, and the specific surface area is 803.2 m 2 / g.
[0042] Embodiment 2:
[0043] The method for preparing graphene provided by the present invention comprises the following specific steps:
[0044] (1) Graphite purification: Soak the waste lithium-ion battery in a saturated sodium chloride solution for 1 to 3 days to release the charge stored in the battery; disassemble the battery to remove the negative electrode copper foil with graphite attached, put it in an organic solvent, and perform ultrasonic treatment for 30 minutes to separate the negative electrode copper foil and the graphite negative electrode; collect the separated graphite negative electrode, repeatedly rinse the collected graphite negative electrode filter cake with distilled water for 4 times through a vacuum filter, then place the filter cake in a drying oven at 60°C and dry it for 60 minutes, and then grind the filter cake into powder; after the powder is sieved, it is calcined and impurities are removed in a tubular furnace with inert protective gas, the calcination temperature is 600°C, and the time is 2 hours to obtain purified graphite powder.
[0045] (2) tabletting: using a powder tabletting machine to press the purified graphite powder into graphite sheets with a thickness of 0.5 to 3 mm;
[0046] (3) Electrolytic stripping treatment: The electrolyte is placed in the electrolytic cell, and then the pressed graphite sheet is bound with a nickel mesh and placed in the electrolytic cell as the cathode, and the platinum sheet is used as the anode. The graphite sheet as the cathode is first pre-electrolyzed at a voltage of 18V for 40 minutes, and then electrolytically stripped at a voltage of 28V. The graphite sheet gradually expands and strips to produce graphene, which is suspended on the surface of the electrolyte.
[0047] (4) Vacuum filtration treatment: The electrolyte after electrolytic stripping is cleaned by a vacuum filtration device, and the cathode-stripped graphene is cleaned in sequence with N,N-dimethylformamide DMF, DMF and H2O with a volume ratio of 1:1, DMF and 5 wt.% HCl solution with a volume ratio of 1:1, and DMF and C2H5OH with a volume ratio of 1:1, and then repeatedly rinsed with distilled water for 5 times to obtain a graphene solution;
[0048] (5) Ultrasonic treatment: The graphene solution is subjected to ultrasonic treatment, and the process parameters of the ultrasonic treatment are power 120 W, ultrasonic frequency 60 Hz, and ultrasonic time 30 min;
[0049] (6) Freeze drying: The graphene solution after ultrasonic treatment is placed in an evaporating dish, and the outlet of the evaporating dish is sealed with filter paper, and then the evaporating dish is placed in the tray of the freeze dryer. The freezing button is turned on, and the pre-freezing is performed for 8 hours. Then, the vacuum gauge and the vacuum button are turned on for drying. The drying time is 28 hours. Finally, the dried graphene is placed in a powder pulverizer for powdering. The powder is sieved to prepare the final graphene product.
[0050] The graphite negative electrode recovered from the waste lithium-ion battery in step (1) is waste high-temperature pyrolytic graphite, artificial graphite or natural flake graphite.
[0051] The organic solvent in step (1) is NMP, anhydrous ethanol or DMF.
[0052] The protective gas used for calcination in step (1) is nitrogen, argon or helium.
[0053] The electrolyte in step (3) is mainly composed of an organic solvent, lithium perchlorate LiClO4 and tetrabutylammonium hexafluorophosphate TBAPF6.
[0054] The organic solvent in the electrolyte of step (3) is propylene carbonate PC, N,N-dimethylformamide DMF or dimethyl sulfoxide DMSO.
[0055] The concentration of lithium perchlorate LiClO4 in the electrolyte of step (3) is 0.1 mol / L, and the concentration of tetrabutylammonium hexafluorophosphate TBAPF6 is 0.1 mol / L.
[0056] The vacuum degree of the freeze-drying in step (6) is 2-10 Pa.
[0057] The graphene prepared by the method for preparing graphene by recycling graphite negative electrodes of waste lithium-ion batteries can be applied to the fields of new energy batteries, industrial catalysts, and biomedical materials.
[0058] The properties of the graphene obtained in Example 2 are as follows: the conductivity of the graphene is 19782 S / cm, the number of layers is 1 to 3, and the specific surface area is 903.15 m 2 / g. Figure 1 It shows that the lateral size of graphene is about 20μm, and the flakes are transparent, which means that the number of graphene layers is very thin, about 1 to 3 layers. Figure 2 It shows that the C:O mass ratio of graphene is 25.3:1, which means that the graphene contains very little oxygen and has high purity. Figure 3 The diffraction intensity ratio of the D peak to the G peak of graphene is 0.1:1. The high diffraction intensity of the G peak indicates that the C element in graphene is mainly in the form of SP 2 The existence of hybridized form and the low diffraction intensity of the D peak indicate that the defects of graphene are very low and the impurities are basically well removed, which further verifies that the purity of graphene is very high.
[0059] Table 1 Content of each element in graphene in Example 2 (mass concentration, %)
[0060] Mass concentration% O 1s C 1s 3.8 96.2
[0061] Embodiment 3:
[0062] The method for preparing graphene provided by the present invention comprises the following specific steps:
[0063] (1) Graphite purification: Soak the waste lithium-ion battery in a saturated sodium chloride solution for 1 to 3 days to release the charge stored in the battery; disassemble the battery to remove the negative electrode copper foil with graphite attached, put it in an organic solvent, and perform ultrasonic treatment for 60 minutes to separate the negative electrode copper foil and the graphite negative electrode; collect the separated graphite negative electrode, repeatedly rinse the collected graphite negative electrode filter cake with distilled water for 5 times through a vacuum filter, then place the filter cake in a drying oven at 60°C to dry for 30 minutes, and then grind the filter cake into powder; after the powder is sieved, it is calcined and impurities are removed in a tubular furnace with inert protective gas, the calcination temperature is 450°C, and the time is 4 hours to obtain purified graphite powder.
[0064] (2) tabletting: using a powder tabletting machine to press the purified graphite powder into graphite sheets with a thickness of 0.5 to 3 mm;
[0065] (3) Electrolytic stripping treatment: The electrolyte is placed in an electrolytic cell, and then the pressed graphite sheet is bound with a nickel mesh and placed in the electrolytic cell as a cathode, and the platinum sheet is used as an anode. The graphite sheet as the cathode is first pre-electrolyzed at a voltage of 18 V for 60 min, and then electrolytically stripped at a voltage of 30 V. The graphite sheet gradually expands and strips to produce graphene, which is suspended on the surface of the electrolyte.
[0066] (4) Vacuum filtration treatment: The electrolyte after electrolytic stripping is cleaned by a vacuum filtration device, and the cathode-stripped graphene is cleaned in sequence with N,N-dimethylformamide DMF, DMF and H2O with a volume ratio of 1:1, DMF and 5 wt.% HCl solution with a volume ratio of 1:1, and DMF and C2H5OH with a volume ratio of 1:1, and then repeatedly rinsed with distilled water for 5 times to obtain a graphene solution;
[0067] (5) Ultrasonic treatment: The graphene solution is subjected to ultrasonic treatment, and the process parameters of the ultrasonic treatment are power 70 W, ultrasonic frequency 45 Hz, and ultrasonic time 30 min;
[0068] (6) Freeze drying: The graphene solution after ultrasonic treatment is placed in an evaporating dish, and the outlet of the evaporating dish is sealed with filter paper, and then the evaporating dish is placed in the tray of the freeze dryer. The freezing button is turned on, and the pre-freezing is performed for 8 hours. Then, the vacuum gauge and the vacuum button are turned on for drying. The drying time is 30 hours. Finally, the dried graphene is placed in a powder pulverizer for powdering. The powder is sieved to prepare the final graphene product.
[0069] The graphite negative electrode recovered from the waste lithium-ion battery in step (1) is waste high-temperature pyrolytic graphite, artificial graphite or natural flake graphite.
[0070] The organic solvent in step (1) is NMP, anhydrous ethanol or DMF.
[0071] The protective gas used for calcination in step (1) is nitrogen, argon or helium.
[0072] The electrolyte in step (3) is mainly composed of propylene carbonate PC, N,N-dimethylformamide DMF, dimethyl sulfoxide DMSO, lithium perchlorate LiClO4 and tetrabutylammonium hexafluorophosphate TBAPF6.
[0073] The organic solvent in the electrolyte of step (3) is propylene carbonate PC, N,N-dimethylformamide DMF or dimethyl sulfoxide DMSO.
[0074] The concentration of lithium perchlorate LiClO4 in the electrolyte of step (3) is 0.1 mol / L, and the concentration of tetrabutylammonium hexafluorophosphate TBAPF6 is 0.1 mol / L.
[0075] The vacuum degree of the freeze-drying in step (6) is 2-10 Pa.
[0076] The graphene prepared by the method for preparing graphene by recycling graphite negative electrodes of waste lithium-ion batteries can be applied to the fields of new energy batteries, industrial catalysts, and biomedical materials.
[0077] The properties of the graphene obtained in Example 3 are as follows: the conductivity of the graphene is 17819 S / cm, the number of layers is 1 to 3, and the specific surface area is 896.5 m 2 / g.
[0078] Comparative Example 1: The difference from Examples 1-3 is that step (3) uses an anodic stripping method to strip graphene and subsequently performs thermal reduction treatment of graphene. The specific steps are as follows:
[0079] (1) Graphite purification: Soak the waste lithium-ion battery in a saturated sodium chloride solution for 1 to 3 days to release the charge stored in the battery; disassemble the battery to remove the negative electrode copper foil with graphite attached, put it in an organic solvent, and perform ultrasonic treatment for 60 minutes to separate the negative electrode copper foil and the graphite negative electrode; collect the separated graphite negative electrode, repeatedly rinse the collected graphite negative electrode filter cake with distilled water for 5 times through a vacuum filter, then place the filter cake in a drying oven at 60°C to dry for 30 minutes, and then grind the filter cake into powder; after the powder is sieved, it is calcined and impurities are removed in a tubular furnace with inert protective gas, the calcination temperature is 450°C, and the time is 4 hours to obtain purified graphite powder.
[0080] (2) tabletting: using a powder tabletting machine to press the purified graphite powder into graphite sheets with a thickness of 0.5 to 3 mm;
[0081] (3) Electrolytic stripping: 1M sulfuric acid electrolyte is placed in an electrolytic cell, and then the pressed graphite sheet is bound with a nickel mesh and placed in the electrolytic cell as an anode, and a platinum sheet is used as a cathode. The graphite sheet as the anode is electrolytically stripped at a voltage of 6V (the starting voltage of graphene stripping in the sulfuric acid electrolyte system is 3V). The graphite sheet gradually expands and strips to produce graphene, and the graphene sinks into the electrolyte;
[0082] (4) Vacuum filtration treatment: The electrolyte after electrolytic stripping is cleaned using a vacuum filtration device and repeatedly rinsed with distilled water for 5 times to obtain a graphene solution;
[0083] (5) Ultrasonic treatment: The graphene solution is subjected to ultrasonic treatment, and the process parameters of the ultrasonic treatment are power 70 W, ultrasonic frequency 45 Hz, and ultrasonic time 30 min;
[0084] (6) Freeze drying: Place the graphene solution after ultrasonic treatment into an evaporating dish, seal the outlet of the evaporating dish with filter paper, and then place the evaporating dish into the tray of the freeze dryer. Turn on the freeze button and pre-freeze for 8 hours, then turn on the vacuum gauge and vacuum button for drying, the drying time is 30 hours, and finally put the dried graphene into a powder pulverizer for powdering, ready for thermal reduction treatment;
[0085] (7) Thermal reduction treatment of graphene: The freeze-dried graphene semi-finished product is placed in a ceramic ark, and the ark is placed in a tubular furnace with argon protective gas, and kept at 300°C for 5 to 7 hours. After the reaction is completed, it is cooled to room temperature and the powder is sieved to obtain the graphene finished product.
[0086] The properties of the graphene of Comparative Example 1 are as follows: the conductivity of the graphene is 13524 S / cm, the number of layers is 1 to 5, and the specific surface area is 456.5 m 2 / g.
[0087] Comparative Example 2:
[0088] The difference from Example 1-3 is that step (3) does not use a pre-electrolysis step, and the specific steps are as follows:
[0089] (1) Graphite purification: Soak the waste lithium-ion battery in a saturated sodium chloride solution for 1 to 3 days to release the charge stored in the battery; disassemble the battery to remove the negative electrode copper foil with graphite attached, put it in an organic solvent, and perform ultrasonic treatment for 30 minutes to separate the negative electrode copper foil and the graphite negative electrode; collect the separated graphite negative electrode, repeatedly rinse the collected graphite negative electrode filter cake with distilled water for 4 times through a vacuum filter, then place the filter cake in a drying oven at 60°C and dry it for 60 minutes, and then grind the filter cake into powder; after the powder is sieved, it is calcined and impurities are removed in a tubular furnace with inert protective gas, the calcination temperature is 600°C, and the time is 2 hours to obtain purified graphite powder.
[0090] (2) tabletting: using a powder tabletting machine to press the purified graphite powder into graphite sheets with a thickness of 0.5 to 3 mm;
[0091] (3) Electrolytic stripping treatment: The electrolyte is placed in the electrolytic cell, and then the pressed graphite sheet is bound with a nickel mesh and placed in the electrolytic cell as the cathode. The platinum sheet is used as the anode. The graphite sheet as the cathode is electrolytically stripped at a voltage of 28V. The graphite sheet gradually expands and strips to produce graphene, which is suspended on the surface of the electrolyte.
[0092] (4) Vacuum filtration treatment: The electrolyte after electrolytic stripping is cleaned by a vacuum filtration device, and the cathode-stripped graphene is cleaned in sequence with N,N-dimethylformamide DMF, DMF and H2O with a volume ratio of 1:1, DMF and 5 wt.% HCl solution with a volume ratio of 1:1, and DMF and C2H5OH with a volume ratio of 1:1, and then repeatedly rinsed with distilled water for 5 times to obtain a graphene solution;
[0093] (5) Ultrasonic treatment: The graphene solution is subjected to ultrasonic treatment, and the process parameters of the ultrasonic treatment are power 120 W, ultrasonic frequency 60 Hz, and ultrasonic time 30 min;
[0094] (6) Freeze drying: The graphene solution after ultrasonic treatment is placed in an evaporating dish, and the outlet of the evaporating dish is sealed with filter paper, and then the evaporating dish is placed in the tray of the freeze dryer. The freezing button is turned on, and the pre-freezing is performed for 8 hours. Then, the vacuum gauge and the vacuum button are turned on for drying. The drying time is 28 hours. Finally, the dried graphene is placed in a powder pulverizer for powdering. The powder is sieved to prepare the final graphene product.
[0095] The properties of the graphene obtained in Comparative Example 2 are as follows: the conductivity of the graphene is 14312 S / cm, the number of layers is 1 to 5, and the specific surface area is 836.23 m 2 / g.
[0096] The ultrasonic treatment in step (1) of Examples 1-3 is carried out using an ultrasonic micro-nano bubble device, the principle of which is to make the organic solvent and air highly miscible and mixed, and ultrasonic cavitation diffusion occurs to release high-density, uniform nano- and micron-sized bubbles, which are inserted into the interface between graphite and copper foil, allowing the graphite powder to be easily separated without damaging the copper foil.
[0097] The voltage in step (3) in Example 1-3 is set to between 26V and 30V, mainly considering that the starting potentials at which graphene begins to peel off are different under different electrolyte systems (the starting potential of the electrolyte of the present invention is 20V), and the magnitude of the voltage directly affects the magnitude of the driving force of the electrochemical intercalation reaction. The greater the voltage, the stronger the driving force of the intercalation reaction, and the easier it is to peel off the graphene. In addition, the purpose of pre-electrolysis is to allow cations to fully intercalate into the graphite interlayer spacing, so that the graphene after the voltage is increased can be slowly peeled off without producing large pieces of peeled graphite, thereby affecting the graphene yield. The pre-electrolysis voltage is set to 18V because, under the condition of 18V, sporadic graphene begins to float on the surface of the electrolyte, indicating that the cations are fully intercalated into the graphite interlayer spacing at this time close to the starting voltage. In the present invention, when the voltage is between 20 and 26 V, the amount of graphene peeled off is very small, which directly affects the yield, while when it is between 26 and 30 V, both the quality and yield of graphene can be guaranteed. When it is greater than 30 V, although the peeling speed increases, the number of graphene layers also increases to multiple layers (6-10 layers), and few-layer graphene cannot be produced.
Claims
1. A method for preparing graphene by recycling graphite negative electrodes from waste lithium-ion batteries, characterized in that: The specific steps are as follows: (1) Graphite purification: soak the waste lithium-ion battery in a saturated sodium chloride solution until the charge stored in the battery is released; disassemble the battery to remove the negative electrode copper foil with graphite attached, put it in an organic solvent, and perform ultrasonic treatment for 30 to 60 minutes to separate the negative electrode copper foil and the graphite negative electrode; collect the separated graphite negative electrode, vacuum filter it, dry it, and grind it into powder; after screening the powder, calcine it in an inert protective gas environment to remove impurities, the calcination temperature is 400 to 600°C, and the time is 2 to 4 hours to obtain purified graphite powder; (2) Tableting: The purified graphite powder is pressed into graphite sheets with a thickness of 0.5 to 3 mm; (3) Electrolytic stripping treatment: The electrolyte is placed in an electrolytic cell, and the graphite sheet is bound by a nickel mesh and placed in the electrolytic cell as a cathode, and the platinum sheet is used as an anode; the graphite sheet as the cathode is first pre-electrolyzed at 18V for 30 to 60 minutes, and then electrolytically stripped at a voltage of 20 to 30V. The graphite sheet gradually expands and strips to produce graphene, which is suspended on the surface of the electrolyte; The electrolyte is mainly composed of an organic solvent, lithium perchlorate LiClO4 and tetrabutylammonium hexafluorophosphate TBAPF6; The organic solvent is propylene carbonate PC, N,N-dimethylformamide DMF or dimethyl sulfoxide DMSO; (4) Vacuum filtration treatment: The electrolyte after electrolytic stripping is cleaned by a vacuum filtration device, and the cathode-stripped graphene is cleaned in sequence with N,N-dimethylformamide DMF, DMF and H2O with a volume ratio of 1:1, DMF and 5 wt.% HCl solution with a volume ratio of 1:1, and DMF and C2H5OH with a volume ratio of 1:1, and then repeatedly rinsed with distilled water to obtain a graphene solution; (5) Ultrasonic treatment: The graphene solution is subjected to ultrasonic treatment, and the process parameters of the ultrasonic treatment are power 70 to 120 W, ultrasonic frequency 45 to 60 Hz, and ultrasonic time 30 to 60 min; (6) Freeze drying: freeze-dry the graphene solution after ultrasonic treatment; pre-freeze for 8 to 10 hours, then dry for 24 to 30 hours, and finally grind the dried graphene into powder, and sieve the powder to prepare the final graphene product.
2. The method for preparing graphene by recycling graphite negative electrodes of waste lithium-ion batteries according to claim 1, characterized in that: The graphite negative electrode recovered from the waste lithium-ion battery in step (1) is waste high-temperature pyrolytic graphite, artificial graphite or natural flake graphite.
3. The method for preparing graphene by recycling graphite negative electrode of waste lithium ion batteries according to claim 1 or 2, characterized in that: The organic solvent in step (1) is NMP, anhydrous ethanol or DMF.
4. The method for preparing graphene by recycling graphite negative electrode of waste lithium-ion batteries according to claim 3, characterized in that: The inert protective gas used for calcination in step (1) is nitrogen, argon or helium.
5. The method for preparing graphene by recycling graphite negative electrodes of waste lithium-ion batteries according to claim 4, characterized in that: The concentration of lithium perchlorate LiClO4 in the electrolyte of step (3) is 0.1 mol / L, and the concentration of tetrabutylammonium hexafluorophosphate TBAPF6 is 0.1 mol / L.
6. The method for preparing graphene by recycling graphite negative electrode of waste lithium ion batteries according to claim 1, 2, 4 or 5, characterized in that: The electrolytic stripping voltage of step (3) is 26 to 30V.
7. The method for preparing graphene by recycling graphite negative electrodes of waste lithium-ion batteries according to claim 1, characterized in that: The vacuum degree of the freeze-drying in step (6) is 2-10 Pa.
8. Graphene prepared by the method for preparing graphene by recycling graphite negative electrodes of waste lithium-ion batteries as claimed in any one of claims 1 to 7, characterized in that: The prepared graphene is used in the fields of new energy batteries, industrial catalysts, and biomedical materials.
Citation Information
Patent Citations
Method for preparing graphene in alkali metal organic solution through electrochemical cathodic disbonding
CN108793141A
Method for recycling negative electrode graphite of lithium ion battery
CN114597533A