Small molecule donor material for organic solar cells and preparation method and application thereof
The small-molecular donor material DI-BDP-CZ is prepared by the condensation reaction of BODIPY derivatives with terephthalaldehyde and N-n-butyl-3-carbazolealdehyde, which solves the low performance and stable morphology of existing organic solar cell devices. The problem of insufficient performance has achieved efficient photoelectric conversion efficiency and good stability, and expanded the application prospects of organic solar cells.
Patent Information
- Application Number
- CN202310050914.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-13
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-01-13
AI Technical Summary
The existing organic solar cell devices have low performance, especially small-molecule organic solar cells have insufficient morphological stability under high temperature conditions, and there is a difficulty in purifying polymer materials, uncertain molecular weight and low purity during the synthesis process. The problem of poor batch repetition limits its application prospects.
The small molecule donor material DI-BDP-CZ is prepared by two-step Knoevenagel condensation reaction with BODIPY derivatives, terephthalaldehyde and N-n-butyl-3-carbazoledehyde. The reaction steps are simple, the conditions are mild, and the cost is low. Blend with fullerene receptors as active layers to form efficient organic solar cells.
It realizes efficient preparation of small molecule donor materials, improves the photoelectric conversion efficiency of organic solar cells, up to 14.97%, and maintains good morphological stability, broadening the application prospects of materials.
Smart Images

Figure CN115960122B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the fields of organic compound synthesis, organic solar energy and fine chemical technology, and specifically relates to the preparation and application of a small molecule solar cell donor. Background Art
[0002] As the rapid economic development leads to the destruction of the environment, the requirements for environmental protection are getting higher and higher. People must find clean renewable energy to replace fossil fuels. Clean energy has attracted great attention from governments around the world for its advantages such as non-geographical restrictions, no noise, no pollution, and low cost. The types of solar cells currently being studied and developed include single crystal silicon, polycrystalline silicon, amorphous silicon, perovskite solar cells, and organic solar cells. Most of the commercialized solar cells are inorganic semiconductors. Their disadvantages are high device preparation costs and high energy consumption in the production process of raw materials. These disadvantages greatly limit their promotion and application. Among various organic solar cells, organic solar cells (OSCs) based on bulk heterojunction (BHJ) active layers are an important part of solar cells and are a promising photovoltaic technology. They have many unique advantages, such as adjustable color, light weight, wide material sources, low manufacturing cost, and large-area manufacturing on flexible substrates. Therefore, they have attracted widespread attention from researchers. In the early stage of developing OSC-based BHJ active layers, the active layer is a mixture of polymer or small molecule donors and fullerene acceptors. As a light-absorbing active layer, its energy conversion efficiency exceeds 10%. However, high-efficiency organic solar cells mainly use conjugated polymers as electron donors. The energy conversion efficiency of organic solar cells prepared using polymer materials is also high, but polymer materials still have problems such as difficulty in purification, large and uncertain molecular weight, low purity, and poor batch reproducibility during the synthesis process. Compared with polymer donor materials, small molecule materials have simpler structures and are easier to prepare, modify and optimize. They also have higher Voc and FF. Therefore, in order to study the relationship between material structure and photovoltaic performance, molecular design work using small molecules as donor materials is crucial.
[0003] Small molecule donor organic solar cells are active layers composed of a blend of small molecule donor materials and acceptor materials. Compared with other types of organic solar cells, the development of small molecule donor organic solar cells is relatively lagging, and the device performance is relatively low. The current highest PCE is 9.5%. However, it is found in multiple systems that small molecule donor organic solar cells usually have excellent morphological stability, especially under high temperature conditions, they can still maintain good morphology and maintain high device performance. Considering the stability requirements of organic solar cells for practical applications, small molecule donor organic solar cells with excellent morphological stability are worthy of in-depth study.
[0004] BODIPY derivatives are a class of good photosensitizers. They have good stability, good modifiability, high molar extinction coefficient and high oxidation potential. The spectral absorption of BODIPY is relatively narrow, but its good modifiability can overcome this shortcoming. Achieving red shift and broadening of spectral absorption is conducive to improving the efficiency of the battery. At present, dye-sensitized solar cell materials based on BODIPY derivatives have achieved high photoelectric conversion efficiency and show good application prospects. In particular, its photophysical and electrochemical properties can be modified by simple synthesis of α-, β-, meso- and boron sites to meet the different requirements of different applications. Therefore, by introducing electron-withdrawing or electron-donating groups at different positions on BODIPY, its absorption wavelength and energy level are regulated to make it well matched with the absorption spectrum and energy level of the acceptor molecule, thereby improving the energy conversion efficiency of organic solar cells. This is of great significance for the development of new small molecule donor materials for organic solar cells.
[0005] The present invention relates to the preparation and application of a small molecule donor for an organic solar cell, wherein a BODIPY derivative is used to sequentially react with terephthalaldehyde and N-n-butyl-3-carbazolealdehyde to undergo a two-step Knoevenagel condensation reaction to obtain a small molecule donor material. The synthesis method of the present invention has not only simple reaction steps, mild reaction conditions, good selectivity, but also low synthesis cost; the small molecule donor material is used as an active layer electron donor in an organic solar cell to obtain a good effect, and plays an important role in expanding and enriching the field of organic solar cells. Summary of the invention
[0006] Purpose of the invention: In view of the deficiencies in the prior art, the purpose of the present invention is to provide a small molecule donor for an organic solar cell and a preparation method and application thereof.
[0007] Technical solution: In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention is:
[0008] The present invention discloses an organic solar cell small molecule donor material and a preparation method and application thereof, characterized in that the compound has a structural formula as shown in formula (I):
[0009]
[0010] A method for preparing a small molecule donor material DI-BDP-CZ for an organic solar cell, comprising the following steps:
[0011] 1) Under anhydrous conditions, terephthalaldehyde and BODIPY derivative (II) are dissolved in a mixed solution of methanol and dichloromethane, to which a 1M methanol solution of sodium methoxide is added dropwise, and the mixture is reacted at room temperature for 6 to 8 hours, and water is added to quench the reaction, and the mixture is extracted with dichloromethane. The organic layer is dried over anhydrous sodium sulfate, the solvent is evaporated under reduced pressure, and then separated and purified by silica gel column chromatography, with the eluent being dichloromethane-petroleum ether (v:v=9:1), to obtain compound (III).
[0012] 2) Under anhydrous conditions, compound (III), N-n-butyl-3-carbazole aldehyde and freshly dried p-toluenesulfonic acid are added to a 100 mL two-necked reaction bottle equipped with a Dean-Stark apparatus, and then 10 mL of toluene is added to dissolve, and 0.2 mL of piperidine is added as a catalyst, and stirred and heated to reflux for 4 to 6 hours. After the reaction is completed, it is cooled to room temperature, extracted with dichloromethane, washed with water, dried, and the solvent is evaporated under reduced pressure and separated and purified by silica gel column chromatography, and the eluent is dichloromethane-petroleum ether (v:v=2:3), to obtain the organic solar cell small molecule donor material DI-BDP-CZ. The specific chemical reaction formula is as follows:
[0013]
[0014] In the above step 1), the molar ratio of terephthalaldehyde, BODIPY derivative (II) and sodium methoxide is 1:2.2-2.5:8-10, and the volume ratio of methanol to dichloromethane is 2:1.
[0015] In the above step 2), the molar ratio of compound (III), p-toluenesulfonic acid and N-n-butyl-3-carbazole carbaldehyde is 1:0.5:4.0-6.0, and the volume and molar ratio of toluene, piperidine and compound (II) is 50 mL:1 mL:1 mmol.
[0016] A method for preparing a small molecule donor material for an organic solar cell, comprising the following steps:
[0017] The ITO glass was first ultrasonically cleaned with detergent, deionized water, acetone, and isopropanol, and then vacuum dried; PEDOT:PSS was spin-coated on the ITO glass at a spin-coating speed of 2500 rpm / min to prepare a hole transport layer with a thickness of 35 to 40 nm; the electron donor and the electron acceptor were dissolved in a chloroform solvent according to a certain mass ratio to prepare an active layer precursor solution (16 mg / mL), which was spin-coated on the hole PEDOT:PSS transport layer at room temperature and a nitrogen atmosphere at a spin-coating speed of 2500 rpm / min for 1 min, and then treated by solvent vapor annealing (SVA) and exposed to tetrahydrofuran vapor for 40 s annealing; PFN-Br methanol solution was spin-coated on the top of the active layer at a spin-coating speed of 3000 rpm / min for 1 min; in a temperature less than 10 -5 Aluminum (Al) is deposited on top of the PFN layer by thermal evaporation under pressure.
[0018] The organic solar cell described in the present invention comprises, from bottom to top, a transparent conductive substrate, a hole transport layer, an organic active layer, an electron transport layer, and a metal electrode Al. The organic active layer comprises a small molecule donor DI-BDP-CZ (I) and a fullerene acceptor small molecule PC 71 BM or non-fullerene acceptor Y6.
[0019] The small molecule donor DI-BDP-CZ (I) and the fullerene acceptor small molecule PC in the organic active layer of the present invention 71 The molecular structures of BM or Y6 are shown below:
[0020]
[0021] The organic binary active layer is DI-BDP-CZ:PC 71 BM or Y6;
[0022] The binary active layer DI-BDP-CZ:PC 71 The mass ratio of BM is 1:0.4-1.4, preferably 1:1.4;
[0023] The mass ratio of DI-BDP-CZ:Y6 in the binary active layer is 1:0.4-1.6, preferably 1:1.2;
[0024] The organic ternary active layer is DI-BDP-CZ:PC 71 BM: Y6;
[0025] The organic ternary active layer is a donor DI-BDP-CZ and an acceptor (PC 71 BM:Y6), DI-BDP-CZ:PC 71The mass ratio of BM:Y6 is 1:0.1:1.1, 1:0.2:1.0, 1:0.3:0.9, 1:04:0.8, preferably DI-BDP-CZ:PC 71 The mass ratio of BM:Y6 is 1:0.3:0.9;
[0026] The structural layers of the forward device of the organic solar cell are, from bottom to top, ITO glass, poly(3,4-ethylenedioxythiophene) (PEDOT): poly(styrene sulfonic acid) (PSS) hole transport layer, organic active layer, polyfluorene derivative (PFN) electron transport layer, and metal Al electrode.
[0027] The method for preparing an organic solar cell according to the present invention comprises the following steps:
[0028] (1) The ITO glass was first ultrasonically cleaned with detergent, deionized water, acetone, and isopropanol, and then vacuum dried;
[0029] (2) Spin coating PEDOT:PSS on ITO glass to prepare a hole transport layer with a thickness of 35-40 nm;
[0030] (3) dissolving the electron donor and the electron acceptor material in a chloroform solvent at a mass ratio of 1:0.4 to 1:1.6, and spin-coating the material on the hole PEDOT:PSS transport layer at room temperature and in a nitrogen atmosphere to form a bulk heterojunction; and then annealing the layer by exposing it to tetrahydrofuran vapor for a certain period of time;
[0031] (4) dissolving PFN in methanol solvent and spin coating it on the active layer to form an electron transport layer;
[0032] (5) Under vacuum conditions, a metal Al electrode is evaporated onto the PFN electron transport layer.
[0033] The spin coating speed in step (2) is 3000 rpm / min;
[0034] In step (3), the spin coating speed is 2500 rpm / min, the spin coating time is 1 min, and the concentration of the active layer is 16 mg / mL;
[0035] In step (4), the spin coating speed is 3000 rpm / min and the spin coating time is 1 min;
[0036] In the step (5), the vacuum degree is less than 10 -5 Torr.
[0037] Beneficial Effects of the Invention
[0038] Compared with the prior art, the organic solar cell small molecule donor material of the present invention and its preparation method and application have the following advantages: (1) the donor reaction steps of this type of small molecule solar cell are simple, the reaction conditions are mild, the selectivity is good, and the synthesis cost is low; (2) by simultaneously introducing thiophene and carbazole groups into the conjugated structure of the BODIPY matrix, the energy level of the material molecule is reduced, the planarity and solubility of the molecule are guaranteed, the conjugated system of the molecule is broadened, and the π-π stacking between molecules is promoted, so that the small molecule donor material has a lower molecular energy level and higher carrier performance; (3) the small molecule donor material of this type of organic solar cell has good compatibility with the acceptor material, can form good absorption complementarity and energy level matching to broaden the absorption band of the material, thereby facilitating the improvement of the performance of the organic solar cell device; (4) the small molecule donor material has good photovoltaic performance, and the photoelectric conversion efficiency of the solar cell prepared as the electron donor material can reach up to 14.97%, so that it has good application prospects in solar cells. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 It is a small molecule donor material DI-BDP-CZ and an acceptor material PC 71 BM and Y6 thin films - electronic absorption spectra, where the horizontal axis is wavelength (wavelength), the unit is nm, and the vertical axis is absorbance (Abs).
[0040] Figure 2 The present invention is used to prepare the donor material DI-BDP-CZ and the acceptor material PC in the organic solar cell 71 Energy level diagram of BM and Y6, the vertical axis is energy level (Energy level), the unit is ev.
[0041] Figure 3 In the application of the small molecule donor of the present invention in organic solar cells, under preferred conditions, the DI-BDP-CZ:PC 71 BM, DI-BDP-CZ:Y6 and DI-BDP-CZ:PC 71 BM: Y6 device current (J sc )-Voltage(V oc )picture. DETAILED DESCRIPTION
[0042] The present invention will be further described below in conjunction with the specific drawings.
[0043] The instruments used for the detection are: 1H-NMR and MALDI-TOF-MS were used to characterize and confirm the donor structure of a small molecule solar cell. The instruments used for the detection are: Bruker ARX400 nuclear magnetic resonance instrument, Bruker ARX600 nuclear magnetic resonance instrument (both use deuterated chloroform as solvent), Shimadzu UV-3100 ultraviolet-visible spectrophotometer (scanning range 300-900nm, optical path slit 2nm), and the fluorescence spectrum was tested using the American Amico Bowman Series 2 Luminescence Spectrometer.
[0044] Dissolve PFN in methanol and stir at room temperature until the solution becomes clear and transparent to prepare a PFN methanol solution with a concentration of 2 mg / mL for later use.
[0045] Press DI-BDP-CZ: PC 71 The donor DI-BDP-CZ and the fullerene acceptor PC were weighed at a mass ratio of 1:0.4, 1:0.8, 1:1.2, 1:1.4, and 1:1.6, respectively. 71 BM, and then add chloroform to dissolve them respectively to prepare an active layer solution with a concentration of 16 mg / mL, which is used for preparing bulk heterojunction devices.
[0046] According to the mass ratio of DI-BDP-CZ:Y6 of 1:0.4, 1:0.8, 1:1.2 and 1:1.4, the donor DI-BDP-CZ and the non-fullerene acceptor Y6 were weighed respectively, and then dissolved in chloroform to prepare an active layer solution with a concentration of 16 mg / mL, which was set aside for use in the preparation of bulk heterojunction devices.
[0047] Press DI-BDP-CZ: PC 71 The BM:Y6 mass ratio is 1:0.1:1.1, 1:0.2:1.0, 1:0.3:0.9, 1:04:0.8, and the donors DI-BDP-CZ and PC 71 BM and Y6 were then dissolved in chloroform to prepare an active layer solution with a concentration of 16 mg / mL for use in preparing bulk heterojunction devices.
[0048] Example 1 Preparation of Compound (III)
[0049] Under anhydrous conditions, terephthalaldehyde (80 mg, 0.6 mmol) and BODIPY derivative (II) (672 mg, 1.4 mmol) were dissolved in a mixed solution of methanol and dichloromethane (v / v, 16 mL / 8 mL), and a methanol solution of sodium methoxide (1 M, 6 mL) was added dropwise thereto. After the addition was completed, the mixture was reacted at room temperature for 6 hours. Water was added to quench the reaction, and the mixture was extracted with dichloromethane. The organic layer was dried over anhydrous sodium sulfate, the solvent was evaporated under reduced pressure, and then separated and purified by silica gel column chromatography, with dichloromethane-petroleum ether (v1:v2=9:1) as the eluent, to obtain compound (III) (244 mg, 38%). 1 H NMR (400MHz, CDCl3): δ7.91 (s, 4H), 7.38-7.39 (d, J=3.6Hz, 2H), 7.28 (s, 2H), 6.97 (s, 4H), 6.83-6.84 (d, J =3.6Hz, 2H), 6.04(s, 2H), 2.64(s, 6H), 2.60(s, 6H), 2.34(s, 6H), 2.13(s, 12H), 1.44(s, 6H), 1.41(s, 6H).
[0050] Example 2 Preparation of compound DI-BDP-CZ
[0051] Under anhydrous conditions, compound (III) (37 mg, 0.03 mmol), N-n-butyl-3-carbazole aldehyde (45 mg, 0.18 mmol) and freshly dried p-toluenesulfonic acid (10 mg, 0.05 mmol) were added to a 100 mL two-necked reaction bottle equipped with a Dean-Stark apparatus, and then 10 mL of toluene and 0.1 mL of piperidine were added, and the mixture was stirred and heated to reflux for 4 hours; after the reaction was completed, it was cooled to room temperature, extracted with dichloromethane, washed with water, dried, and the solvent was evaporated under reduced pressure and then separated and purified by silica gel column chromatography, with the eluent being dichloromethane-petroleum ether (v1:v2=2:3), to obtain a small molecule donor DI-BDP-CZ (I) (33 mg, 55%). 11H NMR (CDCl3, 600 MHz, ppm) δ 8.35 (s, 2H), 8.18 - 8.21 (t, J = 8.4 Hz, 4H), 8.13 (s, 2H), 7.91 (s, 4H), 7.85 - 7.88 (m, 4H), 7.83 (s, 1H), 7.80 (s, 1H), 7.63 - 7.64 (d, J = 8.4 Hz, 2H), 7.59 (s, 1H), 7.56 (s, 1H), 7.48 - 7.51 (m, 4H), 7.45 - 7.47 (d, J = 7.8 Hz, 2H), 7.42 - 7.44 (m, 4H), 7.37 - 7.40 (t, J = 9.0 Hz, 4H), 7.28 - 7.30 (d, J = 11.4 Hz, 4H), 7.24 - 7.25 (d, J = 7.2 Hz, 2H), 7.11 - 7.14 (d, J = 16.2 Hz, 2H), 7.01 - 7.02 (d, J = 3.6 Hz, 2H), 6.99 (s, 4H), 6.77 (s, 2H), 4.29 - 4.34 (m, 8H), 2.37 (s, 6H), 2.20 (s, 12H), 1.83 - 1.91 (m, 8H), 1.51 (s, 6H), 1.40 - 1.46 (m, 8H), 1.38 (s, 6H), 0.93 - 0.98 (m, 12H). 13 13C NMR (CDCl3, 100 MHz, ppm) δ 154.99, 149.12, 142.56, 141.42, 141.10, 141.04, 140.97, 140.01, 139.40, 139.25, 139.10, 138.92, 138.84, 137.97, 137.57, 135.62, 135.18, 133.63, 131.52, 131.20, 129.71, 129.66, 129.12, 128.55, 128.43, 127.84, 126.15, 125.97, 125.93, 125.58, 123.46, 123.34, 123.02, 120.93, 120.85, 120.73, 120.02, 119.58, 119.37, 118.40, 116.69, 116.45, 115.93, 109.26, 109.13, 109.08, 108.98, 107.37, 43.14, 43.06, 32.03, 31.23, 30.24, 29.80, 29.46, 21.36, 20.64, 19.93, 13.98, 11.37.
[0052] Example 3
[0053] The ITO glass sheet was cleaned with detergent, deionized water, acetone, and isopropanol for 30 minutes each, and then vacuum dried; PEDOT:PSS was spin-coated on the cleaned ITO glass at a rotation speed of 3000 rpm / min to prepare a hole transport layer with a thickness of 35 to 40 nm, and then transferred to a glove box with a nitrogen atmosphere; according to the above DI-BDP-CZ:PC 71 The active layer chloroform solution prepared in an amount of BM with a mass ratio of 1:0.4 to 1.6 is spin-coated on the hole transport layer at a spin coating speed of 2500rpm / min and a spin coating time of 1min to form a bulk heterojunction thin film; the device is then exposed to tetrahydrofuran vapor for 40s for annealing; the above-mentioned PFN methanol solution is spin-coated on the bulk heterojunction active layer to obtain a PFN electron transport layer thin film, at a spin coating speed of 3000rpm / min and a spin coating time of 1min; finally, under vacuum conditions, a metal Al electrode is evaporated onto the PFN electron transport layer.
[0054] Example 4
[0055] The ITO glass sheet was cleaned with detergent, deionized water, acetone, and isopropanol in turn, each ultrasonically for 30 minutes, and then vacuum dried; PEDOT:PSS was spin-coated on the cleaned ITO glass at a rotation speed of 3000rpm / min to prepare a hole transport layer with a thickness of 35-40nm, and it was transferred to a glove box with a nitrogen atmosphere; the active layer chloroform solution prepared according to the mass ratio of DI-BDP-CZ:Y6 of 1:0.4-1.4 was spin-coated on the hole transport layer at a spin coating speed of 2500rpm / min for 1min to form a bulk heterojunction film; the device was then exposed to tetrahydrofuran vapor for 40s for annealing; the above-mentioned PFN methanol solution was spin-coated on the bulk heterojunction active layer to obtain a PFN electron transport layer film at a spin coating speed of 3000rpm / min for 1min; finally, a metal Al electrode was evaporated onto the PFN electron transport layer under vacuum conditions.
[0056] Example 5
[0057] The ITO glass sheet was cleaned with detergent, deionized water, acetone, and isopropanol for 30 minutes each, and then vacuum dried; PEDOT:PSS was spin-coated on the cleaned ITO glass at a rotation speed of 3000 rpm / min to prepare a hole transport layer with a thickness of 35 to 40 nm, and then transferred to a glove box with a nitrogen atmosphere; according to the above DI-BDP-CZ:PC 71The active layer chloroform solutions prepared with the mass ratio of BM:Y6 of 1:0.1:1.1, 1:0.2:1.0, 1:0.3:0.9 and 1:04:0.8 were spin-coated on the hole transport layer at a speed of 2500 rpm / min for 1 min to form a bulk heterojunction film; the device was then exposed to tetrahydrofuran vapor for 40 s for annealing; the above-mentioned PFN methanol solution was spin-coated on the bulk heterojunction active layer to obtain a PFN electron transport layer film at a speed of 3000 rpm / min for 1 min; finally, a metal Al electrode was evaporated onto the PFN electron transport layer under vacuum conditions.
[0058] Example 6 Small molecule solar cell donor material DI-BDP-CZ and acceptor material PC 71 Thin film electronic absorption spectra of BM and Y6
[0059] The donor material DI-BDP-CZ and the acceptor material PC 71 BM and acceptor material Y6 were dissolved in chloroform solution and spin-coated to prepare thin films, and their electronic absorption spectra were measured.
[0060] Figure 1 Small molecule solar cell donor material DI-BDP-CZ and acceptor material PC 71 Thin film electronic absorption spectra of BM and Y6
[0061] Photovoltaic performance testing of devices
[0062] The light source is AM 1.5G, and the sunlight intensity is 100mW / cm 2 The intensity of the light source is tested and calibrated by a standard silicon cell, and the test instrument is a Keithley 2400 source meter.
[0063] The active layer DI-BDP-CZ∶PC was obtained by testing 71 The mass ratio of BM is 1:1.4, the mass ratio of active layer DI-BDP-CZ:Y6 is 1:1.2, and the mass ratio of active layer DI-BDP-CZ:PC 71 Device current (J) in solar cells with a BM:Y6 mass ratio of 1:0.3:0.9 sc )-Voltage(V oc ) curve, as shown in the following table and Figure 3 shown.
[0064]
Claims
1. An organic solar cell small molecule donor material DI-BDP-CZ, characterized in that: Its structural formula is shown in formula (I):
2. A method for preparing the small molecule donor material DI-BDP-CZ for an organic solar cell according to claim 1, characterized in that: The preparation method is as follows: firstly, a BODIPY derivative (II) is subjected to a Knoevenagel condensation reaction with terephthalaldehyde to obtain a compound (III), and then a Knoevenagel condensation reaction is carried out with the compound (III) and N-n-butyl-3-carbazole aldehyde to obtain a small molecule donor material DI-BDP-CZ (I). The reaction formula of the preparation process is as follows:
3. The preparation method according to claim 2, characterized in that: The characteristic method includes the following steps: 1) Under anhydrous conditions, terephthalaldehyde and BODIPY derivative (II) are dissolved in a mixed solution of methanol and dichloromethane in a certain proportion, and a 1M methanol solution of sodium methoxide is added dropwise thereto. After the addition is completed, the mixture is reacted at room temperature for 6 to 8 hours, water is added to quench the reaction, and the mixture is extracted with dichloromethane. The organic layer is dried over anhydrous sodium sulfate, the solvent is evaporated under reduced pressure, and then separated and purified by silica gel column chromatography, with the eluent being dichloromethane-petroleum ether in a ratio of v:v=9:1, to obtain compound (III); 2) Under anhydrous conditions, compound (III), N-n-butyl-3-carbazole aldehyde and freshly dried p-toluenesulfonic acid are added to a 100 mL two-necked reaction bottle equipped with a Dean-Stark apparatus, and then 10 mL of toluene is added to dissolve, and 0.2 mL of piperidine is added as a catalyst, and stirred and heated to reflux for 4 to 6 hours. After the reaction is completed, it is cooled to room temperature, extracted with dichloromethane, washed with water, dried, and the solvent is evaporated under reduced pressure and separated and purified by silica gel column chromatography, with the eluent being dichloromethane-petroleum ether in a ratio of v:v=2:3, to obtain a small molecule donor material DI-BDP-CZ (I).
4. The preparation method according to claim 3, characterized in that In the step 1), the molar ratio of terephthalaldehyde, BODIPY derivative (II) and sodium methoxide is 1:2.2-2.5:8-10, and the volume ratio of methanol to dichloromethane is 2:
1.
5. The preparation method according to claim 3, characterized in that In the step 2), the molar ratio of compound (III), p-toluenesulfonic acid and N-n-butyl-3-carbazole carbaldehyde is 1:0.5:4.0-6.0, and the volume and molar ratio of toluene, piperidine and compound (III) is 50 mL:1 mL:1 mmol.
6. An application of the small molecule donor material DI-BDP-CZ for organic solar cells according to claim 1, characterized in that: The organic solar cell device is manufactured using the structure of indium tin oxide (ITO) / polyethoxythiophene (PEDOT):polystyrene sulfonic acid (PSS) / active layer / polyfluorene derivative (PFN) / A1, wherein the active layer comprises a donor material and an acceptor material, and the donor material is a small molecule donor material DI-BDP-CZ (I).
7. The use according to claim 6, characterized in that The active layer acceptor material is PC 71 One or both of BM and Y6, PC 71 The structure of BM is The structure of Y6 is 8. The use according to claim 6, characterized in that: The binary active layer is a small molecule donor material DI-BDP-CZ(I):PC 71 BM, or, the binary active layer is the small molecule donor material DI-BDP-CZ(I):Y6, and the ternary active layer is (I):PC 71 BM:Y6,PC 71 The structure of BM is The structure of Y6 is 9. The use according to claim 6, characterized in that: The best photovoltaic performance of the cell is achieved by mixing the ternary active layer with a small molecule donor material DI-BDP-CZ(I):PC 71 BM:Y6=1:0.3:0.9, the photoelectric conversion efficiency can reach 14.97%, PC 71 The structure of BM is The structure of Y6 is
Citation Information
Patent Citations
Organic solar cell material with wide spectrum absorption
CN103333185A
Median alkoxy phenyl substituted and 2, 6 site strong electron donating group substituted BODIPY (4,4'-difluoro-4-bora-3a,4a-diaza-sindacene) derivative and preparation method thereof
CN105732680A
2-thienyl-substituted unsymmetric boron dipyrromethene (BODIPY) derivatives and preparation method thereof
CN106188112A
Double-BODIPY near-infrared fluorescent dye with AIE effect and preparation method of double-BODIPY near-infrared fluorescent dye
CN113461722A
Preparation and application of D-A type BODIPY micromolecular non-fullerene solar cell receptor
CN114989203A