Preparation method and application of quaternized polyethyleneimine zinc oxide or cuprous oxide particles

The modification of zinc oxide or cuprous oxide through hydrothermal synthesis method is made to form quaternized zinc oxide or cuprous oxide nanoparticles, solving the problem of the ineffectiveness of existing antibacterial materials in liquid media, and realizing the dual antibacterial mechanism and widespread application Antibacterial effect.

CN115960367BActive Publication Date: 2024-11-19ZHEJIANG KEMANQI BIOTECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211673934.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-26
Publication Date
2024-11-19
Estimated Expiration
2042-12-26

AI Technical Summary

Technical Problem

The existing antibacterial materials are ineffective against bacteria in the air without liquid media, and the material fails after the release antibacterial agent is depleted, which poses environmental risks.

Method used

The hydrothermal synthesis method is used to modify zinc oxide or cuprous oxide, and the preparation of polyethylene imidated zinc oxide or cuprous oxide particles is formed to form quaternized zinc oxide or cuprous oxide particles, combined with alkylation modification, forming double Antibacterial mechanism of nanoparticles.

Benefits of technology

It realizes the dual bactericidal activity of uniform dispersion in polar and non-polar solvents, which can effectively kill bacteria from air and solution, prolong the antibacterial effect, and is suitable for a variety of materials and instruments, including paint, masks, catheters, etc.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115960367B_ABST
    Figure CN115960367B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing quaternized polyethyleneimine zinc oxide or cuprous oxide particles, which is characterized by the following steps: polyethyleneimine (PEI) is modified onto zinc oxide or cuprous oxide by a hydrothermal synthesis method, and then modified into quaternized polyethyleneimine zinc oxide or cuprous oxide particles by alkylation. The preparation method has simple process, low cost and wide application range; the prepared quaternized polyethyleneimine zinc oxide or cuprous oxide particles have long-lasting antibacterial stability and good reusability; the synthetic product has high biological safety and can be applied to the fields of urinary catheters, which will greatly promote the development of the antibacterial field.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of antibacterial materials, and in particular to a preparation method and application of quaternized zinc oxide or cuprous oxide particles. Background Art

[0002] In daily life, various surfaces are vulnerable to invasion by microorganisms (bacteria, viruses, etc.) in the air and solutions, which may endanger human health. Potentially harmful bacteria are everywhere around us. For example, talking, coughing, sneezing, and even breathing can produce water vapor droplets containing bacteria. Similarly, bacteria present in liquids (for example, drinking water and catheter fluids in hospitals) can attach to the inner surfaces of blood vessels and pipes and grow and multiply. When the number of cells increases on the surface, microbial cells usually begin to form biofilms, which are composed of a polysaccharide matrix in which the cells are embedded. This biofilm allows microbial cells to survive in harsh conditions, and the embedded cells can be up to 1,000 times less sensitive to most antibiotics and other biocides, which can become a source of stubborn infections.

[0003] To develop an antibacterial surface, antimicrobial agents such as antibiotics, silver ions or iodine can be impregnated into the material. For example, the invention patent application with application number 202010139005.8 discloses a silver ion bactericidal film, which is characterized by: it is composed of a bottom layer and a surface layer, the bottom layer is a polymer material layer and a tape adhered to the back thereof, and the surface layer is a silver ion bactericidal layer; the polymer material layer is made of PE, PP, PET and silica gel; the silver ion bactericidal layer is made of a carrier resin added with bactericidal silver ions; in the silver ion bactericidal layer, the amount of bactericidal silver ions added is 20 to 10,000 ppm; the bactericidal silver ions are one or more of micron silver powder, nano silver powder, silver zeolite and silver activated carbon; the carrier resin is silicone resin or elastomeric rubber; the tape is acrylic tape or polyurethane tape. However, over time, these antimicrobial agents are gradually released into the surrounding solution and kill the microorganisms therein, eventually exhausting the material and rendering it ineffective, and forming a potential environmental risk. While these strategies have been validated in aqueous solutions containing bacteria, they are not expected to be effective against airborne bacteria in the absence of a liquid medium. This is particularly true for release-based materials, which can easily become ineffective when the leached antimicrobial agent is exhausted. Summary of the invention

[0004] In view of the shortcomings of the background technology, the technical problem to be solved by the present invention is to provide a method for preparing quaternary ammonium zinc oxide or cuprous oxide particles with dual antibacterial mechanisms.

[0005] To this end, the present invention is implemented by adopting the following technical solutions:

[0006] The preparation method of quaternized polyethyleneimine zinc oxide or cuprous oxide particles is characterized by the following steps: polyethyleneimine (PEI) is modified onto zinc oxide or cuprous oxide by a hydrothermal synthesis method, and then modified into quaternized polyethyleneimine zinc oxide or cuprous oxide particles by alkylation.

[0007] Furthermore, the preparation method of the polyethyleneimine zinc oxide particles comprises the following steps:

[0008] S1: Disperse zinc acetate powder into distilled water to prepare zinc acetate solution;

[0009] S2: Place the prepared zinc acetate solution on a magnetic stirrer, add sodium hydroxide solution dropwise to adjust the pH, and stir the adjusted solution at 60°C for 30 minutes;

[0010] S3: Weigh polyethyleneimine (PEI) and dissolve it in distilled water, slowly add it dropwise, stir evenly, transfer the liquid to a polytetrafluoroethylene reactor, and react at 160°C for 12h;

[0011] S4: After the polytetrafluoroethylene reactor is cooled, the precipitate generated by the reaction is washed 2-3 times with deionized water by centrifugation, and then washed 2-3 times with anhydrous ethanol;

[0012] S5: placing the precipitated material in an oven and drying it at 60° C. to obtain the prepared polyethyleneimine zinc oxide powder, which is recorded as ZnO-PEI.

[0013] Furthermore, the amount of zinc acetate powder added to every 20 mL of zinc acetate solution is 0.5-0.6 g, the amount of sodium hydroxide added is 0.07 g, the solution pH is adjusted to 7, and the solution is in the form of a milky white colloidal liquid. The mass ratio of the zinc acetate powder to polyethyleneimine (PEI) is 1:1. After stirring evenly, the mixture is transferred to a polytetrafluoroethylene reactor.

[0014] Furthermore, the preparation method of the quaternized polyethyleneimine zinc oxide particles comprises the following steps:

[0015] S1: Weigh polyethyleneimine zinc oxide powder and ultrasonically disperse it in a conical flask containing a certain amount of anhydrous ethanol solvent;

[0016] S2: Add a certain amount of 1-bromohexane (CH3(CH2)5Br) and stir with a magnetic stirrer for 12 hours;

[0017] S3: Continue to add iodomethane (CH3I) in an amount equal to 1-bromohexane, and continue stirring the reaction for 12 hours;

[0018] S4: After the reaction is completed, the particles are thoroughly washed and centrifuged with anhydrous ethanol and distilled water. After the supernatant is discarded, the particles are placed in a vacuum drying oven (40° C.) for drying and weighing for later use. The reaction product obtained is quaternized polyethyleneimine zinc oxide nanoparticles, recorded as ZnO-QPEI.

[0019] Furthermore, 20 mL of anhydrous ethanol was added to every 20 mg of polyethyleneimine zinc oxide powder, and the ratio of the zinc oxide particles modified with polyethyleneimine to 1-bromohexane (CH3(CH2)5Br) and methyl iodide (CH3I) was 1 g:15 ml:15 ml. After the reaction was completed, the particles were washed with anhydrous ethanol and centrifuged three times, and the particles were washed with distilled water and centrifuged three times.

[0020] Furthermore, the method for preparing the polyethyleneimine cuprous oxide particles comprises the following steps:

[0021] S1: Disperse copper sulfate into distilled water to prepare a copper sulfate solution;

[0022] S2: Place the prepared copper sulfate solution on a magnetic stirrer, add sodium hydroxide solution dropwise, and stir the adjusted solution;

[0023] S3: Weigh polyethyleneimine (PEI) and dissolve it in distilled water, slowly add it dropwise, stir evenly, transfer the liquid to a polytetrafluoroethylene reactor, and react at 140°C for 12h;

[0024] S4: After the polytetrafluoroethylene reactor is cooled, the precipitate generated by the reaction is washed 2-3 times with deionized water by centrifugation, and then washed 2-3 times with anhydrous ethanol;

[0025] S5: placing the precipitated material in an oven and drying it at 60° C. to obtain the prepared polyethyleneimine cuprous oxide powder, which is recorded as Cu2O-PEI.

[0026] Furthermore, the amount of copper sulfate added to every 20 mL of copper sulfate solution is 0.1 g, the mass ratio of copper sulfate to polyethyleneimine is 1:0.5 g, and the mixture is stirred evenly and then transferred to a polytetrafluoroethylene reactor.

[0027] Furthermore, the preparation method of the quaternized polyethyleneimine cuprous oxide particles comprises the following steps:

[0028] S1: Weigh polyethyleneimine cuprous oxide powder and ultrasonically disperse it in a conical flask containing a certain amount of anhydrous ethanol solvent;

[0029] S2: Add a certain amount of 1-bromohexane (CH3(CH2)5Br) and stir with a magnetic stirrer for 12 hours;

[0030] S3: Continue to add iodomethane (CH3I) in an amount equal to 1-bromohexane, and continue stirring the reaction for 12 hours;

[0031] S4: After the reaction is completed, the particles are thoroughly washed and centrifuged with anhydrous ethanol and distilled water. After the supernatant is discarded, the particles are placed in a vacuum drying oven (40° C.) for drying and weighing for later use. The reaction product obtained is quaternized polyethyleneimine cuprous oxide particles, recorded as Cu2O-QPEI.

[0032] Furthermore, 20 mL of anhydrous ethanol was added to every 20 mg of polyethyleneimine-doped cuprous oxide powder, and the ratio of the cuprous oxide particles doped with polyethyleneimine to 1-bromohexane (CH3(CH2)5Br) and iodomethane (CH3I) was 1 g:15 ml:15 ml; after the reaction, the particles were washed with anhydrous ethanol and centrifuged three times, and the particles were washed with distilled water and centrifuged three times.

[0033] After adopting the above technical scheme, the present invention utilizes that polyethyleneimine contains a large number of coordination functional groups (amino groups) and can form complexes with divalent metal ions. Most of the zinc ions / copper ions interact with PEI molecules and are evenly distributed in the PEI matrix. Therefore, ZnO / Cu2O may preferentially nucleate and crystal grow in PEI and be evenly distributed. In addition, due to the interaction of intramolecular and intermolecular hydrogen bonds, a template can be provided for crystal growth, crystal growth can be delayed, and particle size can be reduced.

[0034] The quaternary ammonium molecules have contact bactericidal activity, and the zinc oxide particles have release bactericidal activity, which are used to create a bactericidal surface. Such particles with dual bactericidal activity can be evenly dispersed in polar / non-polar solvents, thereby being compatible with polar / non-polar film-forming matrices (such as TPU, PP, etc.). The solid surface formed by the blending of the two can effectively utilize contact, release, or a synergistic mechanism of the two to kill bacteria from the air and solution, prevent the adsorption and adhesion of bacteria on the surface, and prevent the formation of biofilms that are prone to infection. The bactericidal surface has been proven to kill most bacteria deposited on it through gas and attached from aqueous solutions, including Gram-positive bacteria, Gram-negative bacteria, fungi, etc. Specifically, the antibacterial performance is evaluated by spraying an aqueous suspension of bacterial cells on the surface, then air-drying and counting the number of cells that remain alive (i.e., able to grow colonies). The resulting surface can kill up to 99% of Gram-positive and Gram-negative bacteria deposited in aerosols or aqueous suspensions.

[0035] The present invention also provides the use of quaternized polyethyleneimine zinc oxide or cuprous oxide particles in the preparation of antibacterial materials or antibacterial devices or composite antibacterial films of organic polymers. The antibacterial material can serve as an antibacterial coating and be applied to paints, masks, and gas masks; it can be combined with organic polymer materials to form antibacterial composite materials; it can be combined with resins and applied to paint coatings; it can be combined with plastics and polymer resins and applied to filter screens, electrical appliance shells, food materials and transmission, reverse osmosis membranes, microfiltration membranes, ultrafiltration membranes, and nanofiltration membranes; it can be combined with silicone rubber and latex and applied to interventional catheters (such as cardiovascular and cerebrovascular interventional catheters, urinary catheters), and implantable catheters; it can also be combined with rubber and fibers and applied to clothing and masks; it can also be used to coat the surfaces of common objects (such as door handles, children's toys, computer keyboards, telephones, etc.) that people come into contact with in daily life, and can be used in medical consumables (such as urinary catheters, esophageal tubes, endotracheal intubations, etc.), textiles, coatings, packaging materials and other fields to make them antibacterial and thus prevent the spread of bacterial infections. The material has a very wide range of applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] The present invention has the following accompanying drawings:

[0037] Figure 1 The schematic diagram of the synthesis route of the quaternized polyethyleneimidate zinc oxide or cuprous oxide particles involved in the present invention;

[0038] Figure 2 is the transmission electron microscope image of ZnO-PEI;

[0039] Figure 3 Fourier transform infrared spectra of ZnO (a), ZnO-PEI (b), and ZnO-QPEI (c);

[0040] Figure 4 X-ray diffraction patterns of ZnO (a), ZnO-PEI (b), and ZnO-QPEI (c);

[0041] Figure 5 is the scanning electron microscope image of Cu2O-QPEI;

[0042] Figure 6 Zeta diagrams of Cu2O (a), Cu2O-PEI (b), and Cu2O-QPEI (c);

[0043] Figure 7 X-ray diffraction patterns of CuO / Cu2O (a), Cu2O-PEI (b), and Cu2O-QPEI (c);

[0044] Figure 8The bacterial survival rates of Staphylococcus aureus (S. aureus), Escherichia coli (E. coli), Candida albicans (C. albicans), and methicillin-resistant Staphylococcus aureus (MRSA) treated with different concentrations of ZnO-PEI and ZnO-QPEI were shown in PBS phosphate buffer.

[0045] Fig. 9 PBS phosphate buffer (a), the growth of ZnO-PEI colonies at 3mg / ml (b), 2mg / ml (c), 1mg / ml (d), 0.5mg / ml (e), 0.1mg / ml (f), 0.05mg / ml (g), 0.01mg / ml (h); the growth of ZnO-QPEI colonies at 3mg / ml (i), 2mg / ml (j), 1mg / ml (k), 0.5mg / ml (l), 0.1mg / ml (m), 0.05mg / ml (n), 0.01mg / ml (o);

[0046] Fig.10 The pictures of inhibition zones after contact between PBS phosphate buffer (a), ZnO-PEI (b), and ZnO-QPEI (c) and MRSA;

[0047] Fig.11 The bacterial survival rate of Staphylococcus aureus (S. aureus), Escherichia coli (E. coli), Candida albicans (C. albicans), and methicillin-resistant Staphylococcus aureus (MRSA) treated with different concentrations of Cu2O-PEI and Cu2O-QPEI using PBS phosphate buffer;

[0048] Fig.12 PBS phosphate buffer (a), the growth of the colony when Cu2O-PEI is 50μg / ml (b), 20μg / ml (c), 10μg / ml (d), 5μg / ml (e), and 1μg / ml (f); the growth of the colony when Cu2O-QPEI is 50μg / ml (g), 20μg / ml (h), 10μg / ml (i), 5μg / ml (j), and 1μg / ml (k);

[0049] Fig.13 These are pictures of the inhibition zones after contact between PBS phosphate buffer (a), Cu2O-PEI (b), and Cu2O-QPEI (c) and MRSA. DETAILED DESCRIPTION

[0050] In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation mode, structure, characteristics and effects of the present invention are described in detail below in combination with the accompanying drawings and preferred embodiments.

[0051] Reference Figure 1 As shown, the present invention provides a method for preparing quaternized polyethyleneimine zinc oxide or cuprous oxide particles, the steps of which are:

[0052] 1. Preparation of polyethyleneimine zinc oxide particles (ZnO-PEI):

[0053] Zinc acetate powder is dispersed in distilled water to prepare a zinc acetate solution; the prepared zinc acetate solution is placed on a magnetic stirrer, sodium hydroxide solution is added dropwise to adjust the pH to 7, and the adjusted solution is stirred at 60° C. for 30 minutes; polyethyleneimine (PEI) is weighed and dissolved in distilled water, and the solution is slowly added dropwise, and after stirring evenly, the liquid is transferred to a polytetrafluoroethylene reactor and reacted at 160° C. for 12 hours; after the polytetrafluoroethylene reactor is cooled, a precipitate generated by the reaction is centrifugally washed with deionized water for 2-3 times, and then washed with anhydrous ethanol for 2-3 times; the precipitate is placed in an oven and dried at 60° C. to obtain the prepared polyethyleneimine zinc oxide powder, which is recorded as ZnO-PEI.

[0054] 2. Preparation of quaternized polyethyleneimine zinc oxide particles (ZnO-QPEI):

[0055] Weigh the polyethyleneimine zinc oxide powder, ultrasonically disperse it in a conical flask containing a certain amount of anhydrous ethanol solvent, then add a certain amount of 1-bromohexane (CH3(CH2)5Br), add a magnetic stirring reaction time of 12h, continue to add iodomethane (CH3I) equal to 1-bromohexane, continue stirring the reaction time for 12h, after the reaction is completed, wash the particles thoroughly with anhydrous ethanol and distilled water, centrifuge, discard the supernatant, put it in a vacuum drying oven (40℃) to dry and weigh it for later use. The reaction product is quaternized polyethyleneimine zinc oxide nanoparticles, recorded as ZnO-QPEI.

[0056] The obtained products were characterized by transmission electron microscopy (TEM). Figure 2 This is the transmission electron microscope image of ZnO-QPEI. Figure 2 It can be clearly observed that the average particle size of ZnO-QPEI particles is 100 nm. The results show that the preparation of quaternized polyethyleneimine zinc oxide particles is successful.

[0057] The present invention is characterized by Fourier transform infrared spectrometer (FTIR), Figure 3 FTIR spectra of ZnO (a), ZnO-PEI (b), and ZnO-QPEI (c). From the figure, we can see that primary amine groups (1635 cm -1 ) and at 2924cm-1 The clear signal at the alkylation site belongs to the stretching vibration of the methyl and methylene CH of polyethyleneimine, indicating that polyethyleneimine has been successfully doped into the material and ZnO-PEI has been successfully synthesized. Compared with ZnO-PEI, the primary amine signal in ZnO-QPEI disappears and a new signal is observed: 1635cm -1 The characteristic absorption peak of quaternary ammonium salt appeared, proving that the quaternization modification of this material was successful.

[0058] The obtained product was characterized by X-ray diffraction (XRD). Figure 4 Figure 2 is the XRD spectra of ZnO (a), ZnO-PEI (b) and ZnO-QPEI (c). In the figure, (100), (002), (101), (102), (110), (103), (200), (112) and (201) are the peaks of ZnO. The detected structure is very similar to that of ZnO, indicating the successful synthesis of ZnO-PEI and ZnO-QPEI.

[0059] 3. Preparation of polyethyleneimine cuprous oxide particles (Cu2O-PEI):

[0060] Copper sulfate is dispersed in distilled water to prepare a copper sulfate solution; the prepared copper sulfate solution is placed on a magnetic stirrer for stirring; polyethylene imine (PEI) is weighed and dissolved in distilled water, slowly added dropwise, and after stirring evenly, the liquid is transferred to a polytetrafluoroethylene reactor and reacted at 140° C. for 12 hours; after the polytetrafluoroethylene reactor is cooled, the precipitate generated by the reaction is centrifugally washed with deionized water for 2-3 times, and then washed with anhydrous ethanol for 2-3 times; the precipitate is placed in an oven and dried at 60° C. to obtain the prepared polyethylene imide cuprous oxide powder, which is recorded as Cu2O-PEI.

[0061] 4. Preparation of quaternized polyethyleneimine polyethyleneimine cuprous oxide particles (Cu2O-QPEI):

[0062] Weigh polyethyleneimine cuprous oxide powder, ultrasonically disperse it in a conical flask containing a certain amount of anhydrous ethanol solvent, then add a certain amount of 1-bromohexane (CH3(CH2)5Br), add a magnetic stirring reaction time of 12h, continue to add iodomethane (CH3I) in an amount equal to 1-bromohexane, continue to stir the reaction time for 12h, after the reaction is completed, wash the particles thoroughly with anhydrous ethanol and distilled water, centrifuge, discard the supernatant, put it in a vacuum drying oven (40°C) to dry and weigh it for later use, the reaction product obtained is quaternized polyethyleneimine cuprous oxide particles, recorded as Cu2O-QPEI.

[0063] The obtained products were characterized by scanning electron microscopy (SEM). Figure 5This is the scanning electron microscope image of Cu2O-QPEI. Figure 5 It can be clearly observed that the average particle size of Cu2O-QPEI particles is about 200nm. The results show that the preparation of quaternized polyethyleneimine cuprous oxide particles is successful.

[0064] The obtained products were characterized by zeta potential. Figure 6 The zeta potential diagrams of Cu2O, Cu2O-PEI, and Cu2O-QPEI. Since polyethyleneimine carries a large number of imine groups, the particles modified with polyethyleneimine have a positive charge of 21.1mv. The quaternized polyethyleneimine cuprous oxide particles carry a large amount of positive charge, which is 40.1mv. The results show that the preparation of quaternized polyethyleneimine cuprous oxide particles is successful.

[0065] The obtained product was characterized by X-ray diffraction (XRD). Figure 6 Figure 2 is the XRD spectrum of CuO / Cu2O (a), Cu2O-PEI (b), and Cu2O-QPEI (c). In the figure, (110), (111), (200), and (220) are the peaks of Cu2O. The detected structure is very similar to Cu2O, indicating that Cu2O-PEI and Cu2O-QPEI are successfully synthesized.

[0066] Application Examples

[0067] Antibacterial tests of ZnO-PEI, ZnO-QPEI, Cu2O-PEI and Cu2O-QPEI prepared by the above preparation method on Staphylococcus aureus, Escherichia coli, Candida albicans and methicillin-resistant Staphylococcus aureus:

[0068] The samples were mixed with 10 6 CFU mL -1 The bacterial suspension was incubated in PBS phosphate buffer for 24 h, and 100 μL of the suspension was spread on solid culture medium and cultured for 24 h. After incubation at 37 °C for 24 h, the colonies on the agar medium were counted. The bacterial survival rate was defined as the colony forming unit on the agar plate relative to the control group. 6 CFU mL -1 The bacterial suspension in PBS phosphate buffer was used as blank control.

[0069] The experimental results are shown in Figure 8-9The bacterial killing rate of the ZnO-PEI group was 99%, the lethal dose for Staphylococcus aureus was 2 mg / ml, the lethal dose for Escherichia coli was 2 mg / ml, the lethal dose for Candida albicans was 2 mg / ml, and the lethal dose for methicillin-resistant Staphylococcus aureus was 2 mg / ml; the bacterial killing rate of the ZnO-QPEI group was 99%, the lethal dose for Staphylococcus aureus was 1 mg / ml, the lethal dose for Escherichia coli was 1 mg / ml, the lethal dose for Candida albicans was 1 mg / ml, and the lethal dose for methicillin-resistant Staphylococcus aureus was 1 mg / ml; it shows that after quaternary ammonium modification, ZnO-QPEI particles not only have a broad-spectrum antibacterial effect, but also have a strong antibacterial ability. The inhibition zone is used to confirm that ZnO-QPEI is a zinc ion release mechanism, and its bactericidal mechanism is release and sterilization. The experimental results are shown in Fig.10 Images of inhibition zones after contact between PBS phosphate buffer (a), ZnO-PEI (b), and ZnO-QPEI (c) and MRSA.

[0070] The experimental results are shown in Figure 11-12 The bacterial killing rate of the Cu2O-PEI group was 99%, the lethal dose for Staphylococcus aureus was 20μg / ml, the lethal dose for Escherichia coli was 20μg / ml, the lethal dose for Candida albicans was 20μg / ml, and the lethal dose for methicillin-resistant Staphylococcus aureus was 20μg / ml; the bacterial killing rate of the Cu2O-QPEI group was 99%, the lethal dose for Staphylococcus aureus was 10μg / ml, the lethal dose for Escherichia coli was 10μg / ml, the lethal dose for Candida albicans was 10μg / ml, and the lethal dose for methicillin-resistant Staphylococcus aureus was 10μg / ml; it shows that after quaternary ammonium modification, Cu2O-QPEI particles not only have a broad-spectrum antibacterial effect, but also have a strong antibacterial ability. The inhibition zone is used to confirm that Cu2O-QPEI is a zinc ion release mechanism, and its bactericidal mechanism is release and sterilization. The experimental results are shown in Fig.13 Images of inhibition zones after contact between PBS phosphate buffer (a), Cu2O-PEI (b), and Cu2O-QPEI (c) and MRSA.

[0071] The present invention shows a method for constructing quaternized polyethyleneimine zinc oxide or cuprous oxide particles. Through a dual antibacterial mechanism mode, bacteria can be killed through a contact sterilization mechanism and a release sterilization mechanism. Here, Staphylococcus aureus, Escherichia coli, Candida albicans, methicillin-resistant Staphylococcus aureus and other bacteria are used to verify the antibacterial effect and antibacterial spectrum. The results show that the quaternized polyethyleneimine zinc oxide / cuprous oxide has a good antibacterial effect. Not only can zinc ions be released for sterilization, but also the quaternary ammonium salt shows the same excellent performance in contact sterilization. Figure 8-13It can be seen that the quaternized polyethyleneimine zinc oxide or cuprous oxide particles provided by the present invention have a dual antibacterial effect; the synthesis method is simple in process, low in cost, and has a wide range of applications; the antibacterial long-lasting stability and good reusability; the synthetic product has high biological safety and can be applied to the fields of urinary catheters, which will greatly promote the development of the antibacterial field; in addition, the quaternized polyethyleneimine zinc oxide or cuprous oxide particles provided by the present invention have uniform particle size distribution, good monodispersity, strong positive charge, and are easy to coat.

[0072] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A method for preparing quaternized polyethyleneimine zinc oxide or cuprous oxide particles, characterized in that the steps are: The method is as follows: polyethyleneimine (PEI) is modified onto zinc oxide or cuprous oxide by a hydrothermal synthesis method, and then modified into quaternized polyethyleneimine zinc oxide or cuprous oxide particles by alkylation; The preparation method of the quaternized polyethyleneimine zinc oxide particles comprises the following steps: S1: Disperse zinc acetate powder into distilled water to prepare zinc acetate solution; S2: Place the prepared zinc acetate solution on a magnetic stirrer, add sodium hydroxide solution dropwise to adjust the pH, and stir the adjusted solution at 60°C for 30 min; S3: Weigh polyethyleneimine (PEI) and dissolve it in distilled water, slowly add it dropwise, stir evenly, transfer the liquid to a polytetrafluoroethylene reactor, and react at 160°C for 12h; S4: After the polytetrafluoroethylene reactor is cooled, the precipitate generated by the reaction is washed 2-3 times with deionized water by centrifugation, and then washed 2-3 times with anhydrous ethanol; S5: placing the precipitated material in an oven and drying it at 60° C. to obtain prepared polyethyleneimine zinc oxide particles, which are referred to as ZnO-PEI; The preparation method of the quaternized polyethyleneimine cuprous oxide particles comprises the following steps: S1: Disperse copper sulfate into distilled water to prepare a copper sulfate solution; S2: Place the prepared copper sulfate solution on a magnetic stirrer, add sodium hydroxide solution dropwise, and stir the adjusted solution; S3: Weigh polyethyleneimine (PEI) and dissolve it in distilled water, slowly add it dropwise, stir evenly, transfer the liquid to a polytetrafluoroethylene reactor, and react at 140°C for 12h; S4: After the polytetrafluoroethylene reactor is cooled, the precipitate generated by the reaction is washed 2-3 times with deionized water by centrifugation, and then washed 2-3 times with anhydrous ethanol; S5: placing the precipitated material in an oven and drying it at 60° C. to obtain the prepared polyethyleneimine cuprous oxide powder, which is recorded as Cu2O-PEI.

2. The preparation method according to claim 1, characterized in that: The amount of zinc acetate powder added to every 20 mL of zinc acetate solution is 0.5-0.6 g, and the amount of sodium hydroxide added is 0.07 g. The solution pH is adjusted to 7, and the solution is in the form of a milky white colloidal liquid. The mass ratio of the zinc acetate powder to polyethyleneimine (PEI) is 1:

1. After stirring evenly, the solution is transferred to a polytetrafluoroethylene reactor.

3. The preparation method according to claim 2, characterized in that: The preparation method of the quaternized polyethyleneimine zinc oxide particles comprises the following steps: S1: Weigh polyethyleneimine zinc oxide powder and ultrasonically disperse it in a conical flask containing a certain amount of anhydrous ethanol solvent; S2: Add a certain amount of 1-bromohexane (CH3(CH2)5Br) and stir with a magnetic stirrer for 12 h; S3: Continue to add iodomethane (CH3I) in an amount equal to 1-bromohexane, and continue stirring the reaction for 12 h; S4: After the reaction is completed, the particles are thoroughly washed and centrifuged with anhydrous ethanol and distilled water. After the supernatant is discarded, they are placed in a vacuum drying oven (40°C) for drying and weighing for later use. The reaction product obtained is quaternized polyethyleneimine zinc oxide nanoparticles, recorded as ZnO-QPEI.

4. The preparation method according to claim 3, characterized in that: 20 mL of anhydrous ethanol was added to every 20 mg of polyethyleneimine zinc oxide powder. The ratio of the polyethyleneimine-modified zinc oxide particles to 1-bromohexane (CH3(CH2)5Br) and iodomethane (CH3I) was 1g:15ml:15ml. After the reaction was completed, the particles were washed with anhydrous ethanol and centrifuged 2-3 times, and the particles were washed with distilled water and centrifuged 2-3 times.

5. The preparation method according to claim 1, characterized in that: The amount of copper sulfate added to each 20 mL of copper sulfate solution is 0.1 g, and the mass ratio of copper sulfate to polyethyleneimine is 1:0.5 g. After stirring evenly, the mixture is transferred to a polytetrafluoroethylene reactor.

6. The preparation method according to claim 5, characterized in that: The preparation method of the quaternized polyethyleneimine cuprous oxide particles comprises the following steps: S1: Weigh polyethyleneimine cuprous oxide powder and ultrasonically disperse it in a conical flask containing a certain amount of anhydrous ethanol solvent; S2: Add a certain amount of 1-bromohexane (CH3(CH2)5Br) and stir with a magnetic stirrer for 12 h; S3: Continue to add iodomethane (CH3I) in an amount equal to 1-bromohexane, and continue stirring the reaction for 12 h; S4: After the reaction is completed, the particles are thoroughly washed and centrifuged with anhydrous ethanol and distilled water. After the supernatant is discarded, the particles are placed in a vacuum drying oven (40°C) for drying and weighing for later use. The reaction product obtained is quaternized polyethyleneimine cuprous oxide particles, recorded as Cu2O-QPEI.

7. The preparation method according to claim 6, characterized in that: 20 mL of anhydrous ethanol is added to every 20 mg of polyethyleneimine cuprous oxide powder, and the ratio of the polyethyleneimine cuprous oxide particles to 1-bromohexane (CH3(CH2)5Br) and iodomethane (CH3I) is 1g:15ml:15ml; after the reaction is completed, the particles are washed with anhydrous ethanol and centrifuged 2-3 times, and the particles are washed with distilled water and centrifuged 2-3 times.

8. Quaternized polyethyleneimidized zinc oxide particles prepared by the preparation method according to claim 4.

9. Quaternized polyethyleneimidized cuprous oxide particles prepared by the preparation method according to claim 7.

10. Use of the quaternized polyethyleneimine zinc oxide particles according to claim 8 in the preparation of antibacterial devices or composite antibacterial films of organic polymers.

11. Use of the quaternized polyethyleneimidized cuprous oxide particles according to claim 9 in the preparation of antibacterial devices or composite antibacterial films of organic polymers.