Preparation method and application of silver-carbon coated Prussian blue material
By coating the surface of the Prussian blue material with a conductive protective layer of nanosilver and carbon, the problems of poor conductivity and easy water absorption are solved, the rate performance and cycle performance of the sodium-ion battery are improved, and the stability and energy density of the battery are enhanced.
Patent Information
- Application Number
- CN202211674854.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-26
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2042-12-26
AI Technical Summary
Prussian blue material has poor conductivity and cycle performance, and is prone to water absorption, which limits its application in sodium-ion batteries.
The surface of the Prussian blue material is coated with a conductive protective layer composed of nano-silver and carbon to improve the conductivity and avoid direct contact with air and electrolyte, and enhance the hydrophobic performance and stability of the material.
It significantly improves the rate performance and cycle performance of the material, enhances the energy density and stability of the battery, and reduces the probability of side reactions without adding additional conductive agents.
Smart Images

Figure CN115974102B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of materials, and in particular to a preparation method and application of a silver-carbon coated Prussian blue material. Background Art
[0002] With the large-scale application of lithium-ion batteries in various fields such as portable electronic devices and electric vehicles, the shortcomings of lithium resources shortage and high price of lithium batteries have gradually been exposed. It is of great significance to find new secondary batteries to replace lithium-ion batteries. Sodium is extremely abundant in the earth's crust, and sodium-ion batteries have a similar energy storage mechanism as lithium-ion batteries, and are expected to become a new generation of commercial secondary batteries. As an important component of sodium-ion batteries, positive electrode materials are the main bottleneck restricting the performance of sodium-ion batteries, and relevant research is urgently needed to make breakthroughs.
[0003] Among the many positive electrode materials for sodium ion batteries, Prussian blue materials have shown great application prospects due to their high theoretical capacity, low cost, simple synthesis, and easy large-scale production. However, the Prussian blue material has poor conductivity, which seriously limits the rate performance of the Prussian blue material. Metallic silver has excellent conductivity and is stable in air and electrolyte, making it an excellent material that can be used as an electrode conductor. A patent discloses a technology for modifying Prussian blue materials using silver ammonia solution and nitrogen-doped graphene to improve conductivity, thereby enhancing its electrochemical detection response. However, the complex preparation process of silver ammonia solution and the high cost of nitrogen-doped graphene make it difficult to apply to industrial production. In response to these problems, this patent proposes a method for constructing a conductive network using nanosilver and carbon. While improving the conductivity of Prussian blue, the protective layer composed of nanosilver and carbon can prevent Prussian blue from direct contact with air and electrolyte, prevent Prussian blue from absorbing water, inhibit the decomposition of electrolyte on the electrode, and improve the battery cycle performance. Summary of the invention
[0004] The purpose of the present invention is to solve the problems of poor electrical conductivity, poor cycle performance, easy water absorption and the like existing in the prior art Prussian blue materials, thereby providing a silver-carbon coated Prussian blue material and a preparation method thereof, wherein a conductive protective layer composed of nano silver and carbon is coated on the surface of the Prussian blue to improve the electrical conductivity while avoiding direct contact between the Prussian blue and the air and electrolyte, thereby preparing a high-performance Prussian blue material.
[0005] In order to solve the above technical problems, the present invention is implemented through the following technical solutions.
[0006] The first aspect of the present invention provides a method for preparing a silver-carbon coated Prussian blue material, comprising the following steps:
[0007] (1) Fully mixing a hexacyanometallate AM′(CN)6 solution with a metal ion M salt solution; wherein A is selected from one or more of Li, Na, K, Mg, Ca, Zn, and Al; M′ is selected from one or more of Mn, Fe, Co, Ni, Cu, Zn, V, and Cr; and M is selected from one or more of Mn, Fe, Co, Ni, Cu, Zn, V, and Cr;
[0008] (2) The mixed solution of step (1) is aged, and the precipitate is washed and dried to obtain a Prussian blue material intermediate having the structural formula A x M[M′(CN)6] y □ 1-y zH2O, where □ is a hole, 0<x≤2, 0.8<y≤1, 0<z≤20;
[0009] (3) dispersing the Prussian blue material intermediate obtained in step (2) and the dispersant in deionized water, and forming a slurry using ultrasonic oscillation;
[0010] (4) Adding nanosilver and carbon source, mixing well and evaporating to obtain a solid precursor;
[0011] (5) The solid precursor obtained in step (4) is sintered at a constant temperature under a protective gas atmosphere, and after cooling, the material is crushed and sieved to obtain a product.
[0012] Preferably, the hexacyanometallate AM′(CN)6 in step (1) is selected from one or more of Li4Fe(CN)6, Na4Fe(CN)6, K4Fe(CN)6, Na3Fe(CN)6, K3Fe(CN)6, K4Mn(CN)6, K3Co(CN)6, K4V(CN)6, K4Cr(CN)6, K4Ni(CN)6, Na4Mn(CN)6, Na3Co(CN)6, Na4V(CN)6, Na4Cr(CN)6, and Na4Ni(CN)6.
[0013] Preferably, the metal ion M salt in step (1) is selected from one or more of MnCl2, NiNO3, FeSO4, (CH3COO)2Zn, CoCl2, CuSO4, Fe(NO3)3, FeCl3, Fe(CH3COO)2, FeCl2, Cu(NO3)2, CuCl2, Cu(CH3COO)2, Ni(NO3)2, NiSO4, Ni(CH3COO)2, NiCl2, Mn(NO3)2, MnSO4, Mn(CH3COO)2, MnCl2, Zn(NO3)2, ZnSO4, ZnCl2, Co(NO3)2, CoSO4, and Co(CH3COO)2.
[0014] Preferably, the mixing in step (1) is selected from any one of the following methods:
[0015] ① Directly mix the hexacyanometallate AM′(CN)6 solution with the metal ion M salt solution;
[0016] ② Add the hexacyanometallate AM′(CN)6 solution and the metal ion M salt solution dropwise into the sodium citrate dihydrate solution and mix them.
[0017] Preferably, the washing condition in step (2) is: washing with deionized water.
[0018] Preferably, the drying conditions in step (2) are: vacuum drying at 150° C. for 12 h.
[0019] Preferably, the specific surface area of the Prussian blue material intermediate in step (2) is 1-30 m 2 / g, average particle size D 50 0.3-8μm.
[0020] Preferably, the dispersant in step (3) is selected from polyvinyl pyrrolidone.
[0021] Preferably, the amount of the dispersant in step (3) is 5-8% of the mass of the Prussian blue material intermediate.
[0022] Preferably, the ultrasonic oscillation time in step (3) is 10-20 minutes.
[0023] Preferably, the carbon source in step (4) is selected from glucose.
[0024] Preferably, the amount of nanosilver used in step (4) is 0.25-5% of the mass of the Prussian blue material intermediate.
[0025] Preferably, the amount of the carbon source in step (4) is 4-23.75% of the mass of the Prussian blue material intermediate.
[0026] Preferably, the evaporation to dryness in step (4) is carried out at 80°C.
[0027] Preferably, the protective gas in step (5) is selected from one or more of nitrogen, argon, helium and carbon dioxide.
[0028] Preferably, the constant temperature firing in step (5) is performed at a temperature of 200-300° C. and a time of 6-8 hours.
[0029] The second aspect of the present invention provides a silver-carbon coated Prussian blue material prepared according to the above preparation method.
[0030] The third aspect of the present invention provides the use of the above silver-carbon coated Prussian blue material in the preparation of battery electrode materials.
[0031] Preferably, the battery is selected from one or more of a sodium ion battery and a lithium ion battery.
[0032] The fourth aspect of the present invention provides a positive electrode material, comprising the above-mentioned silver-carbon coated Prussian blue material, carbon nanotubes (CNT), conductive carbon black (Super P), polyvinylidene fluoride (PVDF), and N-methylpyrrolidone (NMP).
[0033] Preferably, the positive electrode material comprises the following components in weight proportions: 70-100 parts of silver-carbon coated Prussian blue material, 1-3 parts of CNT, 5-12 parts of Super P, 5-15 parts of PVDF, and 10-30 parts of NMP; most preferably, the positive electrode material comprises the following components in weight proportions: 80 parts of silver-carbon coated Prussian blue material, 2 parts of CNT, 8 parts of Super P, 10 parts of PVDF, and 20 parts of NMP.
[0034] A fifth aspect of the present invention provides a method for preparing the above-mentioned positive electrode material, comprising the following steps:
[0035] (1) Stir and disperse NMP and PVDF evenly to prepare a binder slurry;
[0036] (2) Add CNT to the binder slurry and stir to disperse evenly; add Super P and stir to disperse evenly, then stop the machine and scrape the edges, then continue stirring to disperse;
[0037] (3) Add silver-carbon coated Prussian blue material, stir at a low speed and then increase the stirring speed to eliminate bubbles in a vacuum environment;
[0038] (4) Stop the machine and scrape the edges, stir under vacuum high-speed stirring conditions, check the slurry viscosity, then stir at a low speed and sieve the slurry to obtain the main material;
[0039] (5) The main material prepared in step (4) is coated on the current collector and the solvent is dried.
[0040] Preferably, the stirring and dispersing in step (1) is performed at a rotation speed of 700 rpm and for 30 minutes.
[0041] Preferably, in step (2), the speed of stirring and dispersing CNT is 700 rpm for 30 min; the speed of stirring and dispersing Super P is 700 rpm for 10 min; and the speed of stirring and dispersing after stopping the machine for scraping the edges is 700 rpm for 50 min.
[0042] Preferably, the low-speed stirring in step (3) is performed at a speed of 1900 rpm for 5 min; the stirring speed after increasing is 2500 rpm for 10 min.
[0043] Preferably, in step (4), the rotation speed of the high-speed stirring is 2000 rpm, and the time is 1 hour; the rotation speed of the low-speed stirring is 1500 rpm, and the time is 15 minutes; and the sieve size used for the sieving is 200 mesh.
[0044] Preferably, the current collector in step (5) is selected from aluminum foil.
[0045] A sixth aspect of the present invention provides an electrochemical device, comprising the above-mentioned positive electrode material, a separator, a negative electrode material, and an electrolyte.
[0046] Preferably, the negative electrode material is selected from hard carbon negative electrode sheets.
[0047] Preferably, the electrochemical device is selected from one or more of an aluminum-plastic film soft package, a square aluminum shell, and a cylindrical steel shell.
[0048] Preferably, the electrochemical device is prepared by the following method: a positive electrode material, a separator and a negative electrode material are combined to form a core and then an electrolyte is added.
[0049] Compared with the prior art, the present invention has the following technical effects:
[0050] (1) The present invention can effectively prevent the direct contact between the Prussian blue material and external water by coating a conductive protective layer composed of nanosilver and carbon on the surface of the Prussian blue, thereby improving the hydrophobicity of the material itself, greatly reducing the problem of reduced sodium content and gram capacity caused by water binding, and improving the energy density of the battery.
[0051] (2) The silver-carbon coating layer can also prevent Prussian blue from directly contacting the electrolyte, significantly reducing the probability of side reactions, greatly increasing the stability of the material, and improving the material's cycle performance. At the same time, the Prussian blue material prepared according to the present invention effectively solves the problems of unstable crystal structure and poor conductivity of the Prussian blue material, and the rate performance of the battery prepared therefrom is significantly improved without the need to add a large amount of conductive agent for improvement. BRIEF DESCRIPTION OF THE DRAWINGS
[0052] Figure 1 This is a scanning electron micrograph of the silver-carbon coated Prussian blue material prepared in Example 1.
[0053] Figure 2 This is the X-ray diffraction image of the silver-carbon coated Prussian blue material prepared in Example 1.
[0054] Figure 3 The charge and discharge curves of the button batteries prepared in Example 1 and Comparative Example 1 are shown.
[0055] Figure 4 This is a comparison chart of the rate performance of the soft-pack batteries prepared in Example 2 and Comparative Example 2.
[0056] Figure 5 The figure is a comparison chart of the cycle performance of the soft-pack batteries prepared in Example 2 and Comparative Example 2.
[0057] Figure 6 The figure is a comparison chart of the cycle performance of the soft-pack batteries prepared in Example 2 and Comparative Example 3. DETAILED DESCRIPTION
[0058] In order to make the purpose, technical scheme and effect of the present invention clearer and more specific, the present invention is further described in detail with reference to the following embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0059] Example 1
[0060] A silver-carbon coated Prussian blue material, the preparation method of which comprises the following steps:
[0061] (1) 24.2 g of Na4Fe(CN)6·10H2O was dissolved in 100 mL of deionized water to prepare a solution with a concentration of 0.5 mol / L, 20 g of sodium citrate dihydrate was added, and the mixture was stirred to obtain a Na4Fe(CN)6 solution; 9.9 g of MnCl2·4H2O was dissolved in 100 mL of deionized water to prepare a solution with a concentration of 0.5 mol / L, 20 g of sodium citrate dihydrate was added, and the mixture was stirred to obtain a MnCl2 solution; at 50°C, the MnCl2 solution was slowly added dropwise to the Na4Fe(CN)6 solution under stirring to mix well;
[0062] (2) The mixed solution of step (1) was aged for 6 hours, the precipitate was collected by centrifugation, washed with deionized water, and dried in a drying oven at 150° C. for 12 hours to obtain a Prussian blue material intermediate; the obtained Prussian blue material intermediate was tested by ICP and TG, and the results showed that its molecular formula was Na 1.9 Mn[Fe(CN)6] 0.98 □ 0.02 1.2H2O, BET specific surface area test results show that its specific surface area is 1.5m 2 / g, the particle size test results show that D 50 5.2μm;
[0063] (3) 20 g of the Prussian blue material intermediate obtained in step (2) and 1.0 g of polyvinyl pyrrolidone were dispersed in deionized water and ultrasonically vibrated for 15 min to form a slurry;
[0064] (4) Add 0.2 g of nanosilver and 4.8 g of glucose, mix well, and evaporate to dryness at 80 °C to obtain a solid precursor;
[0065] (5) The solid precursor obtained in step (4) was calcined at 200°C for 8 h in a nitrogen atmosphere. After cooling, the material was crushed and sieved to obtain a silver-carbon coated Prussian blue material. The scanning electron micrograph and X-ray diffraction pattern of the material are shown in FIG. Figure 1-2 shown.
[0066] Subsequently, the silver-carbon coated Prussian blue material prepared above is used to prepare a positive electrode material, including the following steps:
[0067] (1) Take polyvinylidene fluoride (PVDF) with a molecular weight of 800,000 to 1,000,000, bake it under vacuum at 80°C for 10 hours, then slowly add it to 5g of N-methylpyrrolidone, stir it under vacuum at 700 rpm for 30 minutes, and let it stand to obtain a binder slurry; the amount of PVDF added after baking is 2.5g;
[0068] (2) Add 0.5 g CNT to the binder slurry, stir and disperse at 700 rpm for 30 min, then add 2 g conductive carbon black (Super P) that has been baked at 120 °C under vacuum for 12 h, stir and disperse at 700 rpm for 10 min, then stop the machine and scrape the edges. The stirrer speed is 700 rpm and disperse for 50 min.
[0069] (3) Add 20 g of silver-carbon coated Prussian blue material that had been baked at 120°C under vacuum for 12 h, and stir at 1900 rpm for 5 min; increase the stirrer speed to 2500 rpm and stir under vacuum for 10 min to eliminate bubbles;
[0070] (4) Stop the machine and scrape the edges, stir at 2000 rpm under vacuum for 1 hour, and check the viscosity of the slurry. If the viscosity is too thick, add a small amount of NMP (0.2-1g) to adjust the viscosity to about 5000 mPa·s, and continue stirring at 2000 rpm under vacuum for 1.5 hours. Then stir at 1500 rpm for 15 minutes, and then pass the slurry through a 200-mesh sieve to obtain the main material.
[0071] (5) The main material prepared in step (4) is coated on an aluminum foil with a thickness of 12 μm and dried to remove the solvent. After rolling and slitting, a composite positive electrode sheet is obtained.
[0072] Furthermore, the preparation of a button full battery using the composite positive electrode sheet obtained above comprises the following steps:
[0073] (1) Hard carbon, styrene-butadiene rubber (SBR), and sodium carboxymethyl cellulose (CMC) are dissolved in deionized water at a mass ratio of 90:5:5, stirred evenly to form a slurry, coated on a copper current collector, and dried, and then rolled and cut to obtain a negative electrode sheet;
[0074] (2) In a glove box, the positive electrode, separator, and negative electrode are cut into discs and assembled into CR2032 button cells, wherein the electrolyte sodium salt is a binary electrolyte of ethylene carbonate and propylene carbonate containing 1 mol / L sodium hexafluorophosphate.
[0075] Example 2
[0076] A method for preparing a silver-carbon coated Prussian blue material comprises the following steps:
[0077] (1) 24.2 g of Na4Fe(CN)6·10H2O was dissolved in 100 mL of deionized water to prepare a solution with a concentration of 0.5 mol / L, 20 g of sodium citrate dihydrate was added, and the mixture was stirred to obtain a Na4Fe(CN)6 solution; 11.9 g of CoCl2·6H2O was dissolved in 100 mL of deionized water to prepare a solution with a concentration of 0.5 mol / L, 20 g of sodium citrate dihydrate was added, and the mixture was stirred to obtain a CoCl2 solution; at 50°C, the CoCl2 solution and the Na4Fe(CN)6 solution were slowly added dropwise to 20 mL of a solution containing 20 g of sodium citrate dihydrate and the mixture was stirred to obtain a CoCl2 solution;
[0078] (2) The mixed solution of step (1) was aged for 6 hours, the precipitate was collected by centrifugation, washed with deionized water, and dried in a drying oven at 150° C. for 12 hours to obtain a Prussian blue material intermediate; the obtained Prussian blue material intermediate was tested by ICP and TG, and the results showed that its molecular formula was Na 1.8 Co[Fe(CN)6] 0.95 □ 0.05 1.3H2O, BET specific surface area test results show that its specific surface area is 1.8m 2 / g, the particle size test results show that D 50 4.5μm;
[0079] (3) 20 g of the Prussian blue material intermediate obtained in step (2) and 1 g of polyvinyl pyrrolidone were dispersed in deionized water and ultrasonically vibrated for 15 min to form a slurry;
[0080] (4) Add 0.2 g of nanosilver and 4.8 g of glucose, mix well, and evaporate to dryness at 80 °C to obtain a solid precursor;
[0081] (5) The solid precursor obtained in step (4) is calcined at 200° C. for 8 h under a nitrogen atmosphere. After cooling, the material is crushed and sieved to obtain a product.
[0082] Subsequently, the silver-carbon coated Prussian blue material prepared above is used to prepare a positive electrode material, including the following steps:
[0083] (1) Take polyvinylidene fluoride (PVDF) with a molecular weight of 800,000 to 1,000,000, bake it under vacuum at 80°C for 10 hours, then slowly add it to 5g of N-methylpyrrolidone, stir it under vacuum at 700 rpm for 30 minutes, and let it stand to obtain a binder slurry; the amount of PVDF added after baking is 2.5g;
[0084] (2) Add 0.5 g CNT to the binder slurry, stir and disperse at 700 rpm for 30 min, then add 2 g conductive carbon black (Super P) that has been baked at 120 °C under vacuum for 12 h, stir and disperse at 700 rpm for 10 min, then stop the machine and scrape the edges. The stirrer speed is 700 rpm and disperse for 50 min.
[0085] (3) Add 20 g of silver-carbon coated Prussian blue material that had been baked at 120°C under vacuum for 12 h, and stir at 1900 rpm for 5 min; increase the stirrer speed to 2500 rpm and stir under vacuum for 10 min to eliminate bubbles;
[0086] (4) Stop the machine and scrape the edges, stir at 2000 rpm under vacuum for 1 hour, and check the viscosity of the slurry. If the viscosity is too thick, add a small amount of NMP (0.2-1g) to adjust the viscosity to about 5000 mPa·s, and continue stirring at 2000 rpm under vacuum for 1.5 hours. Then stir at 1500 rpm for 15 minutes, and then pass the slurry through a 200-mesh sieve to obtain the main material.
[0087] (5) The main material prepared in step (4) is coated on an aluminum foil with a thickness of 12 μm and dried to remove the solvent. After rolling and slitting, a composite positive electrode sheet is obtained.
[0088] Furthermore, the preparation of a soft-pack battery using the composite positive electrode sheet obtained above comprises the following steps:
[0089] (1) hard carbon, styrene-butadiene rubber (SBR), and sodium carboxymethyl cellulose (CMC) are dissolved in deionized water at a mass ratio of 90:5:5, stirred evenly to form a slurry, coated on a copper current collector, and dried, and then rolled and cut to obtain a negative electrode sheet;
[0090] (2) The positive electrode sheet, negative electrode sheet and separator are made into a core by adopting the lamination process. After packaging, liquid injection, formation, evacuation and sealing, a 15Ah aluminum-plastic film soft-pack battery is obtained.
[0091] Comparative Example 1
[0092] A Prussian blue material, the preparation method of which comprises the following steps:
[0093] (1) 24.2 g of Na4Fe(CN)6·10H2O was dissolved in 100 mL of deionized water to prepare a solution with a concentration of 0.5 mol / L, 20 g of sodium citrate dihydrate was added, and the mixture was stirred to obtain a Na4Fe(CN)6 solution; 9.9 g of MnCl2·4H2O was dissolved in 100 mL of deionized water to prepare a solution with a concentration of 0.5 mol / L, 20 g of sodium citrate dihydrate was added, and the mixture was stirred to obtain a MnCl2 solution; at 50°C, the MnCl2 solution was slowly added dropwise to the Na4Fe(CN)6 solution under stirring to mix well;
[0094] (2) The mixed solution of step (1) was aged for 6 h, the precipitate was collected by centrifugation, washed with deionized water, and dried in a drying oven at 150° C. for 12 h to obtain a Prussian blue material; the obtained Prussian blue material was tested by ICP and TG, and the results showed that its molecular formula was Na 1.9 Mn[Fe(CN)6] 0.98 □ 0。02 1.2H2O.
[0095] Subsequently, the Prussian blue material prepared above is used to prepare a positive electrode material, including the following steps:
[0096] (1) Take polyvinylidene fluoride (PVDF) with a molecular weight of 800,000 to 1,000,000, bake it under vacuum at 80°C for 10 hours, then slowly add it to 5g of N-methylpyrrolidone, stir it under vacuum at 700 rpm for 30 minutes, and let it stand to obtain a binder slurry; the amount of PVDF added after baking is 2.5g;
[0097] (2) Add 0.5 g CNT to the binder slurry, stir and disperse at 700 rpm for 30 min, then add 2 g conductive carbon black (Super P) that has been baked at 120 °C under vacuum for 12 h, stir and disperse at 700 rpm for 10 min, then stop the machine and scrape the edges. The stirrer speed is 700 rpm and disperse for 50 min.
[0098] (3) Add 20 g of Prussian blue material that had been baked at 120 °C under vacuum for 12 h, and stir at 1900 rpm for 5 min; increase the stirrer speed to 2500 rpm and stir under vacuum for 10 min to eliminate bubbles;
[0099] (4) Stop the machine and scrape the edges, stir at 2000 rpm under vacuum for 1 hour, and check the viscosity of the slurry. If the viscosity is too thick, add a small amount of NMP (0.2-1g) to adjust the viscosity to about 5000 mPa·s, and continue stirring at 2000 rpm under vacuum for 1.5 hours. Then stir at 1500 rpm for 15 minutes, and then pass the slurry through a 200-mesh sieve to obtain the main material.
[0100] (5) The main material prepared in step (4) is coated on an aluminum foil with a thickness of 12 μm and dried to remove the solvent. After rolling and slitting, a composite positive electrode sheet is obtained.
[0101] Furthermore, the preparation of a button full battery using the composite positive electrode sheet obtained above comprises the following steps:
[0102] (1) hard carbon, styrene-butadiene rubber (SBR), and sodium carboxymethyl cellulose (CMC) are dissolved in deionized water at a mass ratio of 90:5:5, stirred evenly to form a slurry, coated on a copper current collector, and dried, and then rolled and cut to obtain a negative electrode sheet;
[0103] (2) In a glove box, the positive electrode, separator, and negative electrode are cut into discs and assembled into CR2032 button cells, wherein the electrolyte sodium salt is a binary electrolyte of ethylene carbonate and propylene carbonate containing 1 mol / L sodium hexafluorophosphate.
[0104] Comparative Example 2
[0105] (1) 24.2 g of Na4Fe(CN)6·10H2O was dissolved in 100 mL of deionized water to prepare a solution with a concentration of 0.5 mol / L, 20 g of sodium citrate dihydrate was added, and the mixture was stirred to obtain a Na4Fe(CN)6 solution; 11.9 g of CoCl2·6H2O was dissolved in 100 mL of deionized water to prepare a solution with a concentration of 0.5 mol / L, 20 g of sodium citrate dihydrate was added, and the mixture was stirred to obtain a CoCl2 solution; at 50°C, the CoCl2 solution and the Na4Fe(CN)6 solution were slowly added dropwise to 20 mL of a solution containing 20 g of sodium citrate dihydrate and the mixture was stirred to obtain a CoCl2 solution;
[0106] (2) The mixed solution of step (1) was aged for 6 hours, the precipitate was collected by centrifugation, washed with deionized water, and dried in a drying oven at 150° C. for 12 hours to obtain a Prussian blue material intermediate; the obtained Prussian blue material intermediate was tested by ICP and TG, and the results showed that its molecular formula was Na 1.8 Co[Fe(CN)6] 0.95 □ 0.05 ·1.3H2O.
[0107] Subsequently, the Prussian blue material prepared above is used to prepare a positive electrode material, including the following steps:
[0108] (1) Take polyvinylidene fluoride (PVDF) with a molecular weight of 800,000 to 1,000,000, bake it under vacuum at 80°C for 10 hours, then slowly add it to 5g of N-methylpyrrolidone, stir it under vacuum at 700 rpm for 30 minutes, and let it stand to obtain a binder slurry; the amount of PVDF added after baking is 2.5g;
[0109] (2) Add 0.5 g CNT to the binder slurry, stir and disperse at 700 rpm for 30 min, then add 2 g conductive carbon black (Super P) that has been baked at 120 °C under vacuum for 12 h, stir and disperse at 700 rpm for 10 min, then stop the machine and scrape the edges. The stirrer speed is 700 rpm and disperse for 50 min.
[0110] (3) Add 20 g of Prussian blue material that had been baked at 120 °C under vacuum for 12 h, and stir at 1900 rpm for 5 min; increase the stirrer speed to 2500 rpm and stir under vacuum for 10 min to eliminate bubbles;
[0111] (4) Stop the machine and scrape the edges, stir at 2000 rpm under vacuum for 1 hour, and check the viscosity of the slurry. If the viscosity is too thick, add a small amount of NMP (0.2-1g) to adjust the viscosity to about 5000 mPa·s, and continue stirring at 2000 rpm under vacuum for 1.5 hours. Then stir at 1500 rpm for 15 minutes, and then pass the slurry through a 200-mesh sieve to obtain the main material.
[0112] (5) The main material prepared in step (4) is coated on an aluminum foil with a thickness of 12 μm and dried to remove the solvent. After rolling and slitting, a composite positive electrode sheet is obtained.
[0113] Furthermore, the preparation of a soft-pack battery using the composite positive electrode sheet obtained above comprises the following steps:
[0114] (1) hard carbon, styrene-butadiene rubber (SBR), and sodium carboxymethyl cellulose (CMC) are dissolved in deionized water at a mass ratio of 90:5:5, stirred evenly to form a slurry, coated on a copper current collector, and dried, and then rolled and cut to obtain a negative electrode sheet;
[0115] (2) The positive electrode sheet, negative electrode sheet and separator are made into a core by adopting the lamination process. After packaging, liquid injection, formation, evacuation and sealing, a 15Ah aluminum-plastic film soft-pack battery is obtained.
[0116] Comparative Example 3
[0117] (1) 24.2 g of Na4Fe(CN)6·10H2O was dissolved in 100 mL of deionized water to prepare a solution with a concentration of 0.5 mol / L, 20 g of sodium citrate dihydrate was added, and the mixture was stirred to obtain a Na4Fe(CN)6 solution; 11.9 g of CoCl2·6H2O was dissolved in 100 mL of deionized water to prepare a solution with a concentration of 0.5 mol / L, 20 g of sodium citrate dihydrate was added, and the mixture was stirred to obtain a CoCl2 solution; at 50°C, the CoCl2 solution and the Na4Fe(CN)6 solution were slowly added dropwise to 20 mL of a solution containing 20 g of sodium citrate dihydrate and the mixture was stirred to obtain a CoCl2 solution;
[0118] (2) The mixed solution of step (1) was aged for 6 hours, the precipitate was collected by centrifugation, washed with deionized water, and dried in a drying oven at 150° C. for 12 hours to obtain a Prussian blue material intermediate; the obtained Prussian blue material intermediate was tested by ICP and TG, and the results showed that its molecular formula was Na 1.8 Co[Fe(CN)6] 0.95 □ 0.05 ·1.3H2O.
[0119] (3) Disperse 20 g of the obtained Prussian blue in 300 mL of deionized water, add 10 g of glucose and stir for 30 min to obtain a Prussian blue dispersion;
[0120] (4) Prepare silver ammonia solution: Disperse 25 g of AgNO3 in 200 mL of deionized water, and add ammonia water until the precipitate disappears to obtain a silver ammonia solution;
[0121] (5) Add 1 mL min to the Prussian blue dispersion. -1 Add silver ammonia solution at a speed of 100 μg / min, heat in a water bath at 35°C for 30 min, and let stand for 1 h; then centrifuge and wash to obtain a silver-Prussian blue material;
[0122] (6) Take 20 g of silver-Prussian blue material and add it to 200 ml of nitrogen-doped graphene (1 mg / mL) dispersed in N,N-dimethylformamide. After ultrasonic treatment for 30 min and centrifugal drying, the silver-Prussian blue-loaded nitrogen-doped graphene composite material can be obtained.
[0123] Subsequently, the Prussian blue material prepared above is used to prepare a positive electrode material, including the following steps:
[0124] (1) Take polyvinylidene fluoride (PVDF) with a molecular weight of 800,000 to 1,000,000, bake it under vacuum at 80°C for 10 hours, then slowly add it to 5g of N-methylpyrrolidone, stir it under vacuum at 700 rpm for 30 minutes, and let it stand to obtain a binder slurry; the amount of PVDF added after baking is 2.5g;
[0125] (2) Add 0.5 g CNT to the binder slurry, stir and disperse at 700 rpm for 30 min, then add 2 g conductive carbon black (Super P) that has been baked at 120 °C under vacuum for 12 h, stir and disperse at 700 rpm for 10 min, then stop the machine and scrape the edges. The stirrer speed is 700 rpm and disperse for 50 min.
[0126] (3) Add 20 g of Prussian blue material that had been baked at 120 °C under vacuum for 12 h, and stir at 1900 rpm for 5 min; increase the stirrer speed to 2500 rpm and stir under vacuum for 10 min to eliminate bubbles;
[0127] (4) Stop the machine and scrape the edges, stir at 2000 rpm under vacuum for 1 hour, and check the viscosity of the slurry. If the viscosity is too thick, add a small amount of NPM (0.2-1g) to adjust the viscosity to about 5000 mPa·s, and continue stirring at 2000 rpm under vacuum for 1.5 hours. Then stir at 1500 rpm for 15 minutes, and then pass the slurry through a 200-mesh sieve to obtain the main material.
[0128] (5) The main material prepared in step (4) is coated on an aluminum foil with a thickness of 12 μm and dried to remove the solvent. After rolling and slitting, a composite positive electrode sheet is obtained.
[0129] Furthermore, the preparation of a soft-pack battery using the composite positive electrode sheet obtained above comprises the following steps:
[0130] (1) hard carbon, styrene-butadiene rubber (SBR), and sodium carboxymethyl cellulose (CMC) are dissolved in deionized water at a mass ratio of 90:5:5, stirred evenly to form a slurry, coated on a copper current collector, and dried, and then rolled and cut to obtain a negative electrode sheet;
[0131] (2) The positive electrode sheet, negative electrode sheet and separator are made into a core by adopting the lamination process. After packaging, liquid injection, formation, evacuation and sealing, a 15Ah aluminum-plastic film soft-pack battery is obtained.
[0132] Verification Example 1
[0133] The CR2032 button batteries prepared in Example 1 and Comparative Example 1 were placed in a battery charge and discharge tester, charged to 4.0V at 0.1C current, left for 10 minutes, and then discharged to 2.0V at 0.1C. The discharge capacity and first-cycle coulomb efficiency of the battery in the range of 2.0-4.0V were measured. The test results are shown in Table 1. Figure 3 shown.
[0134] Table 1 CR2032 button battery discharge capacity and first week coulomb efficiency test results
[0135]
[0136] Subsequently, the soft-pack batteries prepared in Example 2 and Comparative Example 2 were placed on a battery charge and discharge tester, charged to 4.0V at 0.1C, 0.5C, and 1C, and left for 10 minutes. Then, they were discharged to 2.0V at the same current of 0.1C, 0.5C, and 1C. The discharge capacity of the battery at different charge and discharge currents in the range of 2.0-4.0V was measured, and the test results are shown in Table 2. Figure 4 shown.
[0137] Table 2 CR2032 button battery charge and discharge test results
[0138]
[0139] Furthermore, the soft-pack batteries prepared in Example 2 and Comparative Example 2 were placed on a battery charge and discharge tester, and a charge and discharge cycle test was performed at 1C / 1C current at 25°C. The cycle stability and mass energy density test results are shown in Table 3. Figure 5 shown.
[0140] Table 3 Test results of soft pack battery cycle stability and mass energy density
[0141]
[0142] Furthermore, the soft-pack batteries prepared in Example 2 and Comparative Example 3 were placed on a battery charge and discharge tester, and a charge and discharge cycle test was performed at 1C / 1C current at 25°C. The cycle stability and mass energy density test results are shown in Table 4. Figure 6 shown.
[0143]
[0144] According to the above, for the Prussian blue material without silver-carbon coating treatment, due to its poor electrical conductivity, the capacity of the battery at high rate is low. At the same time, the direct contact between the Prussian blue material and the electrolyte in the battery is prone to cause various side reactions, resulting in a decrease in the battery gram capacity and a decrease in cycle performance. When the silver-carbon coating layer of the present invention is used to coat the Prussian blue material, a conductive network can be effectively constructed, while avoiding direct contact between the Prussian blue material and external water, thereby improving the hydrophobicity of the material itself, greatly reducing the problem of sodium content and gram capacity reduction caused by water binding, and improving the energy density of the battery. At the same time, the silver-carbon coating layer can also avoid direct contact between Prussian blue and the electrolyte, significantly reducing the probability of side reactions, greatly increasing the stability of the material, and improving the cycle performance of the material. In addition, the Prussian blue material prepared according to the present invention effectively solves the problems of unstable crystal structure and poor electrical conductivity of the Prussian blue material, and the rate performance of the battery prepared therefrom is significantly improved, without the need to add a large amount of conductive agent for improvement.
[0145] The above specific implementation method part specifically introduces the analytical method involved in the present invention. It should be noted that the above introduction is only to help those skilled in the art better understand the method and ideas of the present invention, rather than limiting the relevant content. Without departing from the principle of the present invention, those skilled in the art may also make appropriate adjustments or modifications to the present invention, and the above adjustments and modifications shall also fall within the scope of protection of the present invention.
Claims
1. A method for preparing a silver-carbon coated Prussian blue material, comprising the following steps: (1) Hexacyanometallate AM′(CN) 6 The solution is fully mixed with a metal ion M salt solution; wherein A is selected from one or more of Li, Na, K, Mg, Ca, Zn, and Al; M′ is selected from one or more of Mn, Fe, Co, Ni, Cu, Zn, V, and Cr; and M is selected from one or more of Mn, Fe, Co, Ni, Cu, Zn, V, and Cr; (2) The mixed solution of step (1) is aged, and the precipitate is washed and dried to obtain a Prussian blue material intermediate having the structural formula A x M[M′(CN) 6 ] y □ 1-y ·zH 2 O, where □ is a hole, 0<x≤2, 0.8<y≤1, 0<z≤20; (3) dispersing the Prussian blue material intermediate obtained in step (2) and the dispersant in deionized water, and forming a slurry using ultrasonic oscillation; (4) adding nanosilver and a carbon source, mixing well and evaporating to obtain a solid precursor; the carbon source is selected from glucose; (5) The solid precursor obtained in step (4) is sintered at a constant temperature under a protective gas atmosphere, and after cooling, the material is crushed and sieved to obtain a product.
2. The preparation method according to claim 1, It is characterized in that The hexacyanometallate AM′(CN) in step (1) 6 Selected from Li 4 Fe(CN) 6 、Na 4 Fe(CN) 6 , K 4 Fe(CN) 6 、Na 3 Fe(CN) 6 , K 3 Fe(CN) 6 , K 4 Mn(CN) 6 , K 3 Co(CN) 6 , K 4 V (CN) 6 , K 4 Cr(CN) 6 , K 4 Ni(CN) 6 、Na 4 Mn(CN) 6 、Na 3 Co(CN) 6 、Na 4 V (CN) 6 、Na 4 Cr(CN) 6 、Na 4 Ni(CN) 6 One or more of .
3. The preparation method according to claim 1, It is characterized in that The metal ion M salt in step (1) is selected from MnCl 2 、FeSO 4 , (CH 3 COO 2 Zn、CoCl 2 ,CuSO 4 、Fe(NO 3 ) 3 、FeCl 3 , Fe(CH 3 COO 2 、FeCl 2 、Cu(NO 3 ) 2 , CuCl 2 ,Cu(CH 3 COO 2 , Ni (NO 3 ) 2 、NiSO 4 、Ni(CH 3 COO 2 、NiCl 2 、Mn(NO 3 ) 2 、MnSO 4 、Mn(CH 3 COO 2 、Zn(NO 3 ) 2 、ZnSO 4 、ZnCl 2 、Co(NO 3 ) 2 、CoSO 4 、Co(CH 3 COO 2 One or more of .
4. The preparation method according to claim 1, It is characterized in that The dispersant in step (3) is selected from polyvinyl pyrrolidone.
5. The preparation method according to claim 1, It is characterized in that The constant temperature firing in step (5) is performed at a temperature of 200-300° C. and a time of 6-8 hours.
6. The silver-carbon coated Prussian blue material prepared according to the preparation method according to any one of claims 1 to 5.
7. Use of the silver-carbon coated Prussian blue material prepared according to the preparation method according to any one of claims 1 to 5 in the preparation of battery electrode materials.
8. A positive electrode material, It is characterized in that The invention comprises a silver-carbon coated Prussian blue material prepared by the preparation method according to any one of claims 1 to 5, carbon nanotubes, conductive carbon black, polyvinylidene fluoride and N-methylpyrrolidone.
9. An electrochemical device, It is characterized in that It comprises the positive electrode material, the separator, the negative electrode material and the electrolyte according to claim 8.