A cobalt-free positive electrode material and preparation method thereof, and a lithium-ion battery
By controlling the angle of repose and airflow pulverization conditions of nickel-manganese hydroxide during the preparation process of lithium-ion battery cathode materials, a cobalt-free cathode material with high fluidity is prepared, which solves the problem of poor fluidity of cathode materials in the existing technology. , improving preparation efficiency.
Patent Information
- Application Number
- CN202211726297.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-30
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-12-30
AI Technical Summary
The current cathode materials for lithium-ion batteries have poor fluidity, which affects their screening speed and preparation efficiency, resulting in a decline in the performance of lithium-ion batteries.
By uniformly mixing nickel manganese hydroxide and lithium source and then sintering for the first time, followed by airflow crushing and sieving, controlling the classification frequency, feeding frequency and grinding pressure during the airflow crushing process, a product with an angle of repose between 30° and 30° is prepared. 50° cobalt-free cathode material, with optional addition of dopants and coatings to improve fluidity.
The fluidity and screening speed of cobalt-free cathode materials are improved, thereby improving the preparation efficiency of cathode materials and solving the problem of poor fluidity.
Smart Images

Figure CN115974178B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a cobalt-free positive electrode material and a preparation method thereof, and a lithium ion battery. Background Art
[0002] Lithium-ion batteries have the advantages of high voltage platform, good cycle performance, no memory effect and high specific energy, and are currently the most widely used power batteries. With the development of smart grid energy storage and the continuous promotion of new energy vehicles, lithium-ion batteries have developed rapidly, and the market's performance requirements for lithium-ion batteries are also getting higher and higher. As a commonly used positive electrode material, lithium nickel manganese cobalt oxide has the advantages of high energy density and good cycle performance; however, due to the high price of cobalt and its high environmental pollution, its application in lithium-ion batteries is limited. Therefore, the development of cobalt-free lithium nickel manganese oxide materials is of great significance.
[0003] If the particle size of the positive electrode material is too large, it will puncture the separator of the lithium-ion battery, causing a short circuit in the lithium-ion battery and affecting the rate performance of the lithium-ion battery. For this reason, the positive electrode material is usually sieved after sintering to remove the positive electrode material with too large particle size. At the same time, sieving can also remove impurities in the positive electrode material and improve the purity of the positive electrode material.
[0004] However, the positive electrode material prepared by the existing method has poor fluidity, which reduces the screening speed of the positive electrode material and thus affects the preparation efficiency of the positive electrode material. Summary of the invention
[0005] Therefore, the technical problem to be solved by the present invention is how to improve the fluidity of the positive electrode material, thereby providing a cobalt-free positive electrode material and a preparation method thereof, and a lithium-ion battery.
[0006] The invention provides a method for preparing a cobalt-free positive electrode material, comprising: uniformly mixing nickel manganese hydroxide and a lithium source to obtain a mixture, wherein the angle of repose β1 of the nickel manganese hydroxide is 40°-60°; performing a first sintering on the mixture to obtain an initial cobalt-free positive electrode material; performing airflow pulverization on the initial cobalt-free positive electrode material, wherein during the airflow pulverization, the grading frequency is 110HZ-150HZ, the feeding frequency is 6.5HZ-10.5HZ, and the grinding pressure is 0.2Mpa-0.5Mpa to obtain the cobalt-free positive electrode material, wherein the angle of repose β2 of the cobalt-free positive electrode material is 30°-50°, and β2≤β1; and the cobalt-free positive electrode material is screened.
[0007] Optionally, the particle size D50 of the cobalt-free positive electrode material is 1 μm-5 μm; the particle size D50 of the nickel manganese hydroxide is 2 μm-4 μm.
[0008] Optionally, the preparation of the nickel manganese hydroxide includes the following steps: preparing a nickel source, a manganese source, a complexing agent and a precipitant into a reaction solution for a coprecipitation reaction to obtain nickel manganese hydroxide; the pH value of the reaction solution is 10-12, and during the coprecipitation reaction, the reaction temperature is 45°C-60°C, the reaction time is 60h-120h, and the stirring speed is 500rad / min-1200rad / min; after the reaction is completed, the nickel manganese hydroxide is washed and dried in sequence.
[0009] Optionally, the ratio of the molar amount of lithium element in the lithium source to the total molar amount of nickel element and manganese element in the nickel manganese hydroxide is 1-1.15.
[0010] Optionally, the chemical formula of the nickel manganese hydroxide is Ni x Mn 1-x (OH)2(0.50≤x≤1.0).
[0011] Optionally, the first sintering temperature is 800°C-1000°C, the time is 10h-20h, the sintering atmosphere is an oxygen atmosphere, and the heating rate is 1°C / min-5°C / min.
[0012] Optionally, a dopant is added while the nickel manganese hydroxide is mixed with a lithium source, and the dopant includes at least one of ZrO2, TiO2, Al2O3, Ta2O5, WO3, Nb2O5, and MoO3.
[0013] Optionally, the mass ratio of the dopant to the nickel manganese hydroxide is 0.1%-0.5%.
[0014] Optionally, the method for preparing the cobalt-free positive electrode material also includes: after air flow pulverizing the initial cobalt-free positive electrode material and before the screening, mixing the cobalt-free positive electrode material with a coating agent evenly, and performing a second sintering to form a coating layer on the surface of the cobalt-free positive electrode material, the material of the coating agent includes at least one of Al2O3, ZrO2, TiO2, and WO3.
[0015] Optionally, the second sintering temperature is 600° C.-800° C., the time is 4 h-8 h, and the sintering atmosphere is an oxygen atmosphere.
[0016] Optionally, the coating layer has a thickness of 10nm-20nm.
[0017] The present invention also provides a cobalt-free positive electrode material, which is prepared by the method for preparing the cobalt-free positive electrode material.
[0018] The present invention also provides a lithium ion battery, which comprises the above-mentioned cobalt-free positive electrode material.
[0019] The technical solution of the present invention has the following advantages:
[0020] The method for preparing a cobalt-free positive electrode material provided by the present invention limits the repose angle of nickel manganese hydroxide, and the grading frequency, feeding frequency and grinding pressure in the air flow pulverization process to specific ranges, thereby obtaining a cobalt-free positive electrode material with a repose angle β2 of 30°-50°. The cobalt-free positive electrode material has high fluidity, improves the screening speed of the cobalt-free positive electrode material, and thus improves the preparation efficiency of the positive electrode material. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0022] Figure 1 This is a SEM image of the nickel manganese hydroxide prepared in Example 1 of the present invention;
[0023] Figure 2 This is the SEM image of the cobalt-free positive electrode material prepared in the sixth step of this Example 1. DETAILED DESCRIPTION
[0024] The technical solution of the present invention is described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.
[0026] Furthermore, the terms “first”, “second”, and “third” are used for descriptive purposes only and should not be understood as indicating or implying relative importance.
[0027] As described in the background art, the positive electrode material prepared by the existing method has poor fluidity. The applicant found that this is mainly related to the particle size of the positive electrode material. When the particle size of the positive electrode material is too large, its fluidity is bound to be poor; and when the particle size of the positive electrode material is too large, the positive electrode material is prone to agglomeration to form larger agglomerates, resulting in poor fluidity of the positive electrode material.
[0028] To this end, this embodiment provides a method for preparing a cobalt-free positive electrode material, comprising:
[0029] Step S1, uniformly mixing nickel manganese hydroxide and a lithium source to obtain a mixture, wherein the repose angle β1 of the nickel manganese hydroxide is 40°-60°;
[0030] Step S2, performing a first sintering on the mixture to obtain an initial cobalt-free positive electrode material;
[0031] Step S3, the initial cobalt-free positive electrode material is subjected to airflow pulverization, during which the grading frequency is 110HZ-150HZ, the feeding frequency is 6.5HZ-10.5HZ, and the grinding pressure is 0.2Mpa-0.5Mpa to obtain a cobalt-free positive electrode material, and the repose angle β2 of the cobalt-free positive electrode material is 30°-50°, and β2≤β1; illustratively, the grading frequency can be 110HZ, 120HZ, 130HZ, 140HZ or 150HZ, the feeding frequency can be 6.5HZ, 7.5HZ, 8.5HZ, 9.5HZ or 10.5HZ, and the grinding pressure can be 0.2Mpa, 0.3Mpa, 0.4Mpa or 0.5Mpa.
[0032] Step S4, screening the cobalt-free positive electrode material.
[0033] The above-mentioned method for preparing the cobalt-free positive electrode material obtains a cobalt-free positive electrode material with a repose angle β2 of 30°-50° by limiting the repose angle of nickel manganese hydroxide, and the grading frequency, feeding frequency and grinding pressure in the air flow crushing process within a specific range. The cobalt-free positive electrode material has high fluidity, improves the screening speed of the cobalt-free positive electrode material, and thus improves the preparation efficiency of the positive electrode material.
[0034] Specifically, the particle size D50 of the nickel manganese hydroxide is 2 μm-4 μm. The nickel manganese hydroxide in the above specific particle size range has a repose angle of 40°-60°; illustratively, the particle size D50 of the nickel manganese hydroxide may be 2.0 μm, 2.5 μm, 3.0 μm, 3.5 μm or 4.0 μm.
[0035] Furthermore, in this embodiment, the preparation of the nickel manganese hydroxide includes the following steps: preparing a nickel source, a manganese source, a complexing agent and a precipitant into a reaction solution for a coprecipitation reaction to obtain nickel manganese hydroxide; the pH value of the reaction solution is 10-12, and during the coprecipitation reaction, the reaction temperature is 45°C-60°C, the reaction time is 60h-120h, and the stirring speed is 500rad / min-1200rad / min; after the reaction is completed, washing the nickel manganese hydroxide with water, and drying the nickel manganese hydroxide at 110°C-180°C for 5h-15h.
[0036] It should be understood that if the reaction temperature is too high, the growth of nickel manganese hydroxide is dominant during the reaction, and the nucleation of nickel manganese hydroxide is secondary, which leads to the nickel manganese hydroxide having too large a particle size and low sphericity, resulting in the nickel manganese hydroxide having too large an angle of repose β1, and having poor fluidity; if the reaction temperature is too low, the nucleation of nickel manganese hydroxide is dominant during the reaction, and the growth of nickel manganese hydroxide is secondary, which leads to the slow growth rate of nickel manganese hydroxide, and it is easy to prepare nickel manganese hydroxide with too small a particle size. At this time, nickel manganese hydroxide is easy to agglomerate to form agglomerates of larger size, resulting in the nickel manganese hydroxide having too large an angle of repose β1, and having poor fluidity. If the reaction time is too long, the particle size of nickel manganese hydroxide is too large, resulting in the nickel manganese hydroxide having too large an angle of repose β1; if the reaction time is too short, the nickel manganese hydroxide particles are too small, and it is easy to agglomerate, resulting in the nickel manganese hydroxide having too large an angle of repose β1. If the stirring speed is too fast, the particle size of nickel manganese hydroxide will be too large; if the stirring speed is too slow, the sphericity of nickel manganese hydroxide will deteriorate, resulting in a large repose angle β1 of nickel manganese hydroxide and poor fluidity. If the pH is too high, the growth rate of nickel manganese hydroxide will be slow, which will result in the nickel manganese hydroxide particles being too small and prone to agglomeration, resulting in a large repose angle β1 of nickel manganese hydroxide; if the pH is too low, the nucleation rate will be affected, thereby affecting the quality of nickel manganese hydroxide.
[0037] By limiting the pH value, reaction temperature, reaction time and stirring speed of the reaction solution within a specific range, the nickel manganese hydroxide with a specific particle size range of the present embodiment is prepared, that is, the nickel manganese hydroxide with a specific repose angle range is prepared. Exemplarily, the pH value of the reaction solution can be 10, 10.2, 10.5, 11.0, 11.2, 11.5, 11.8 or 12, the reaction temperature can be 45°C, 48°C, 50°C, 55°C or 60°C, the reaction time can be 60h, 70h, 80h, 90h, 100h, 110h or 120h, and the stirring speed can be 500rad / min, 700rad / min, 900rad / min, 1100rad / min or 1200rad / min.
[0038] Specifically, the total molar concentration of the nickel source and the manganese source in the reaction solution is 1 mol / L-10 mol / L; the ratio of the total molar amount of the nickel element in the nickel source to the total molar amount of the nickel element and the manganese element in the reaction solution is 0.50-1.0, and the chemical formula of the nickel manganese hydroxide finally prepared is Ni x Mn 1-x (OH)2(0.50≤x≤1.0); nickel sources include but are not limited to NiSO4·6H2O, manganese sources include but are not limited to MnSO4·H2O, precipitants include but are not limited to 5 mol / L NaOH aqueous solution, and complexing agents include but are not limited to NH3·H2O.
[0039] In step S1, nickel manganese hydroxide and a lithium source are first weighed according to a stoichiometric ratio; then the nickel manganese hydroxide and the lithium source are placed in a mixer for mixing, the mixer speed is 600rpm-900rpm, the mixing time is 15min-30min, and the material filling efficiency in the mixer is 40%-80%; illustratively, the mixer speed can be 600rpm, 700rpm, 800rpm or 900rpm, the mixing time can be 15min, 20min, 25min or 30min, and the material filling efficiency can be 40%, 50%, 60%, 70% or 80%.
[0040] Furthermore, in the mixture, the ratio of the molar amount of lithium in the lithium source to the total molar amount of nickel and manganese in the nickel manganese hydroxide is 1-1.15, and the chemical formula of the finally prepared cobalt-free positive electrode material is Li y Ni x Mn 1-x O2 (1≤y≤1.15); lithium salt includes but is not limited to at least one of LiNO3, CH3COOLi, LiOH, and Li2CO3.
[0041] In step S2, the first sintering temperature is 800℃-1000℃, the time is 10h-20h, the sintering atmosphere is an oxygen atmosphere, and the heating rate is 1℃ / min-5℃ / min; exemplarily, the first sintering temperature can be 800℃, 820℃, 840℃, 860℃, 880℃, 900℃, 920℃, 940℃, 960℃, 980℃ or 1000℃, the time can be 10h, 12h, 14h, 16h, 18h or 20h, the heating rate can be 1℃ / min, 2℃ / min, 3℃ / min, 4℃ / min or 5℃ / min, and the higher the sintering temperature, the shorter the sintering time.
[0042] In this embodiment, the particle size D50 of the cobalt-free positive electrode material finally prepared is 1μm-5μm, and the cobalt-free positive electrode material in the above-mentioned specific particle size range has a repose angle β2 of 30°-50°. That is, the particle size of the cobalt-free positive electrode material is controlled by controlling the particle size of the nickel manganese hydroxide, as well as the grading frequency, feeding frequency and grinding pressure in the air flow milling process; the particle size of the cobalt-free positive electrode material is controlled within an appropriate range so that it is not easy to agglomerate, thereby controlling the repose angle of the cobalt-free positive electrode material, and finally achieving control over the fluidity of the cobalt-free positive electrode material. The cobalt-free positive electrode material finally prepared in this embodiment is a single crystal with a residual alkali content of 0.05wt%-0.6wt%, and 0.2m 2 / g-1.5m 2 / g.
[0043] Further, in step S1, while the nickel manganese hydroxide is mixed with the lithium source, a dopant is added, the dopant includes at least one of ZrO2, TiO2, Al2O3, Ta2O5, WO3, Nb2O5, and MoO3, and the mass ratio of the dopant to the nickel manganese hydroxide is 0.1%-0.5%. Exemplarily, the molar ratio of the dopant to the nickel manganese hydroxide can be 0.1%, 0.2%, 0.3%, 0.4% or 0.5%. The addition of the dopant does not affect the repose angle of the nickel manganese hydroxide.
[0044] Furthermore, the method for preparing the cobalt-free positive electrode material further includes: after the initial cobalt-free positive electrode material is subjected to airflow pulverization and before screening, that is, after step S3 and before step S4, the cobalt-free positive electrode material is mixed evenly with a coating agent and subjected to a second sintering to form a coating layer on the surface of the cobalt-free positive electrode material, wherein the material of the coating agent includes at least one of Al2O3, ZrO2, TiO2, and WO3, the mass ratio of the coating agent to the cobalt-free positive electrode material is 0.2%-0.4%, and the thickness of the coating layer is 10nm-20nm. It should be understood that since the thickness of the coating layer is nanometer-level, the effect of the existence of the coating layer on the particle size of the cobalt-free positive electrode material can be ignored, that is, the effect of the existence of the coating layer on the fluidity of the cobalt-free positive electrode material can be ignored, that is, the fluidity of the cobalt-free positive electrode material does not change after the coating layer is formed.
[0045] Specifically, firstly, the cobalt-free positive electrode material and the coating agent are weighed according to the stoichiometric ratio; then the cobalt-free positive electrode material and the coating agent are placed in a mixer for mixing, the mixer speed is 900rpm-1200rpm, the mixing time is 20min-45min, and the equipment filling rate is 50%-80%. Exemplarily, the mixer speed can be 900rpm, 1000rpm, 1100rpm or 1200rpm, the mixing time can be 20min, 25min, 30min, 35min, 40min, 45min or 45min, and the material filling efficiency can be 50%, 60%, 70% or 80%.
[0046] Specifically, the second sintering temperature is 600°C-800°C, the time is 4h-8h, and the sintering atmosphere is an oxygen atmosphere. Exemplarily, the second sintering temperature can be 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C, 950°C or 1000°C, and the time can be 4h, 5h, 6h, 7h or 8h, and the higher the sintering temperature, the shorter the sintering time.
[0047] This embodiment also provides a cobalt-free positive electrode material, which is prepared using the above-mentioned method for preparing the cobalt-free positive electrode material.
[0048] This embodiment also provides a lithium-ion battery, which includes the above-mentioned cobalt-free positive electrode material.
[0049] Example 1
[0050] This embodiment provides a method for preparing a cobalt-free positive electrode material, comprising:
[0051] Step 1: Preparation of nickel manganese hydroxide: NiSO4·6H2O and MnSO4·H2O were prepared into a 2 mol / L aqueous solution according to a stoichiometric ratio (3:1), a 5 mol / L NaOH aqueous solution was used as a precipitant, and NH3·H2O was added as a complexing agent to obtain a reaction solution with a pH of 11.0; the reaction solution was added to a continuous reactor, the reaction temperature was controlled to be 55°C, the stirring speed was 1000 rad / min, and the reaction time was 80h; after the reaction was completed, the material was washed with deionized water, and the washed material was dried at 180°C for 12h to obtain nickel manganese hydroxide Ni 0.75 Mn 0.25( OH)2;
[0052] Step 2: Mixing: Weigh nickel manganese hydroxide, LiOH and dopant ZrO2, the stoichiometric ratio of nickel manganese hydroxide and LiOH is 1:1, the mass ratio of ZrO2 to nickel manganese hydroxide is 0.15%, and then mix them evenly in a mixer, the mixer speed is 800 rpm, the mixing time is 20 minutes, and the material filling efficiency is 60%;
[0053] Step 3: Primary sintering: Place the mixed materials in a sintering furnace with an oxygen atmosphere. The sintering furnace is heated to 950°C at a heating rate of 3°C / min, kept warm for 15 hours, and then cooled naturally to obtain the product: LiNi Zr-doped cobalt-free cathode material 0.75 Mn 0.25 O2;
[0054] Step 4: air flow pulverization: the product obtained by the primary sintering is subjected to air flow pulverization. During the air flow pulverization process, the classification frequency of the air flow pulverizer is 130HZ, the feeding frequency is 8.5HZ, and the grinding pressure is 0.32Mpa to obtain a cobalt-free positive electrode material, and the cobalt-free positive electrode material is a single crystal particle;
[0055] Step 5: Coating and secondary sintering: The cobalt-free cathode material and the coating agent Al2O3 after airflow pulverization are mixed evenly in a mixer, the mass ratio of the coating agent to the cobalt-free cathode material is 0.35%, the mixer speed is 1000rpm, the mixing time is 30min, and the equipment filling rate is 60%; the mixed materials are secondary sintered in an oxygen atmosphere at a sintering temperature of 700℃ for 6h;
[0056] Step 6: Pass the product obtained by secondary sintering through a 325-mesh sieve.
[0057] Figure 1 This is the SEM image of the nickel manganese hydroxide prepared in this example. Figure 1 It can be seen that the morphology of nickel manganese hydroxide is secondary spheres composed of flakes, and the particle size distribution of nickel manganese hydroxide is: D50 = 3.6 μm, D10 = 2.0 μm, D90 = 5.2 μm;
[0058] Figure 2 This is a SEM image of the cobalt-free positive electrode material prepared in the sixth step of this embodiment, wherein the particle size distribution of the cobalt-free positive electrode material is: D50=3.4μm, D10=1.5μm, D90=6.3μm.
[0059] Example 2
[0060] This embodiment provides a method for preparing a cobalt-free positive electrode material, which differs from the method for preparing a cobalt-free positive electrode material provided in Example 1 in that:
[0061] In the first step: the pH of the reaction solution is 10, the reaction temperature is 45°C, the stirring speed is 500 rad / min, and the reaction time is 60h;
[0062] In the fourth step: the classification frequency of the air flow mill is 110HZ, the feeding frequency is 6.5HZ, and the grinding pressure is 0.2Mpa.
[0063] Example 3
[0064] This embodiment provides a method for preparing a cobalt-free positive electrode material, which differs from the method for preparing a cobalt-free positive electrode material provided in Example 1 in that:
[0065] In the first step: the pH of the reaction solution is 12, the reaction temperature is 60°C, the stirring speed is 1200 rad / min, and the reaction time is 120 h;
[0066] In the fourth step: the classification frequency of the air flow mill is 150HZ, the feeding frequency is 10.5HZ, and the grinding pressure is 0.5Mpa.
[0067] Comparative Example 1
[0068] This comparative example provides a method for preparing a cobalt-free positive electrode material, which differs from the method for preparing a cobalt-free positive electrode material provided in Example 1 in that:
[0069] In the first step: the pH of the reaction solution is 12.5, the reaction temperature is 65°C, the stirring speed is 400 rad / min, and the reaction time is 50 h;
[0070] In the fourth step: the classification frequency of the air flow mill is 100HZ, the feeding frequency is 5HZ, and the grinding pressure is 0.15Mpa.
[0071] Test Example 1
[0072] The repose angles of the nickel manganese hydroxide and the cobalt-free positive electrode materials prepared in Examples 1-3 and Comparative Example 1 were tested, and the sieving speed of the prepared cobalt-free positive electrode materials was tested. The test results are shown in Table 1:
[0073] Table 1
[0074] Angle of repose of nickel manganese hydroxide (°) Angle of repose of cobalt-free cathode materials (°) Screening speed (kg / h) Example 1 53 43 350 Example 2 55 46 320 Example 3 60 50 300 Comparative Example 1 65 54 200
[0075] It can be seen from Table 1 that, relative to Comparative Example 1, the cobalt-free positive electrode materials prepared in Examples 1-3 have a smaller angle of repose, and the smaller the angle of repose, the smaller the friction coefficient and the better the fluidity.
[0076] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. A method for preparing a cobalt-free positive electrode material, characterized in that: include: uniformly mixing nickel manganese hydroxide and a lithium source to obtain a mixture, wherein the repose angle β1 of the nickel manganese hydroxide is 40°-60°; Performing a first sintering on the mixture to obtain an initial cobalt-free positive electrode material; The initial cobalt-free positive electrode material is subjected to airflow milling, wherein the classification frequency is 110HZ-150HZ, the feeding frequency is 6.5HZ-10.5HZ, and the grinding pressure is 0.2Mpa-0.5Mpa to obtain a cobalt-free positive electrode material, wherein the repose angle β2 of the cobalt-free positive electrode material is 30°-50°, and β2≤β1; The cobalt-free positive electrode material is screened.
2. The method for preparing a cobalt-free positive electrode material according to claim 1, characterized in that: The particle size D50 of the cobalt-free positive electrode material is 1 μm-5 μm; the particle size D50 of the nickel manganese hydroxide is 2 μm-4 μm.
3. The method for preparing a cobalt-free positive electrode material according to claim 2, characterized in that: The preparation of the nickel manganese hydroxide comprises the following steps: A nickel source, a manganese source, a complexing agent and a precipitant are prepared into a reaction solution for coprecipitation reaction to obtain nickel manganese hydroxide; the pH value of the reaction solution is 10-12, and during the coprecipitation reaction, the reaction temperature is 45° C.-60° C., the reaction time is 60 h-120 h, and the stirring speed is 500 rad / min-1200 rad / min; After the reaction is completed, the nickel manganese hydroxide is washed and dried in sequence.
4. The method for preparing a cobalt-free positive electrode material according to any one of claims 1 to 3, characterized in that: The ratio of the molar amount of lithium element in the lithium source to the total molar amount of nickel element and manganese element in the nickel manganese hydroxide is 1-1.
15.
5. The method for preparing a cobalt-free positive electrode material according to any one of claims 1 to 3, characterized in that: The chemical formula of the nickel manganese hydroxide is Ni x Mn 1-x (OH)2, 0.50≤x≤1.
0.
6. The method for preparing a cobalt-free positive electrode material according to claim 1, characterized in that: The first sintering temperature is 800° C.-1000° C., the time is 10 h-20 h, the sintering atmosphere is an oxygen atmosphere, and the heating rate is 1° C. / min-5° C. / min.
7. The method for preparing a cobalt-free positive electrode material according to any one of claims 1 to 3, characterized in that: When the nickel manganese hydroxide is mixed with the lithium source, a dopant is added, and the dopant includes at least one of ZrO2, TiO2, Al2O3, Ta2O5, WO3, Nb2O5, and MoO3.
8. The method for preparing a cobalt-free positive electrode material according to claim 7, characterized in that: The mass ratio of the dopant to the nickel manganese hydroxide is 0.1%-0.5%.
9. The method for preparing a cobalt-free positive electrode material according to any one of claims 1 to 3, characterized in that: Also includes: After the initial cobalt-free positive electrode material is subjected to air flow pulverization and before the screening, the cobalt-free positive electrode material is evenly mixed with a coating agent, and a second sintering is performed to form a coating layer on the surface of the cobalt-free positive electrode material, and the material of the coating agent includes at least one of Al2O3, ZrO2, TiO2, and WO3.
10. The method for preparing a cobalt-free positive electrode material according to claim 9, characterized in that: The second sintering temperature is 600°C-800°C, the time is 4h-8h, and the sintering atmosphere is an oxygen atmosphere; And / or, the coating layer has a thickness of 10nm-20nm.
11. A cobalt-free positive electrode material, characterized in that: The cobalt-free positive electrode material is prepared by the method for preparing the cobalt-free positive electrode material according to any one of claims 1 to 10.
12. A lithium ion battery, characterized in that: Including the cobalt-free positive electrode material as described in claim 11.