A kind of early strength ultra-high toughness cement-based material and preparation method thereof
By using additives such as silicate cement and sulfaluminate cement in ultra-high toughness cement composite and modified C-S-H nanocrystals, the problems of long settling time and slow development of strength in low temperature environments are solved, and early strength is achieved. Rapid improvement and stable growth in the later stage, suitable for low-temperature construction.
Patent Information
- Application Number
- CN202211665086.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-23
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-12-23
AI Technical Summary
Ultra-high toughness cement-based materials have long settling time in low temperature environments and slow strength development, which affects construction and performance stability.
Using silicate cement and sulfaluminate cement as the main gelling material, modified C-S-H nanocrystals, nanocalcium carbonate and micro-scale silica spherical particles are added to form a crystal core effect, promote the formation of hydration products and improve the internal Microstructure, improving early and long-term performance.
It significantly shortens the settling time, improves the early strength and later compressive strength in low-temperature environments, and ensures that the material can hydrate quickly during low-temperature construction and maintains long-term stable performance.
Smart Images

Figure CN115974500B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of building materials, and in particular to an early-strength ultra-high toughness cement-based material and a preparation method thereof. Background Art
[0002] Ultra-high toughness cement-based materials are a new type of building material that has developed rapidly in the civil engineering industry in recent years. Combining the performance characteristics of high-performance concrete and fiber composite materials, it has ultra-high mechanical properties and excellent durability, and has significantly improved performance compared to ordinary concrete. The high toughness of ultra-high performance concrete can meet the requirements of bridge deck pavement for the tensile strength of concrete materials, and is an ideal steel bridge deck pavement material. Under the same load, it can effectively slow down the growth of steel bar strain amplitude and slow down the stiffness degradation of the continuous structure of the bridge deck under fatigue load, thereby greatly improving the fatigue life of the continuous structure of the bridge deck. The composite bridge deck formed by combining with the orthotropic steel bridge deck is connected by a connector with large shear stiffness to ensure the combination of the two properties, which can significantly improve the stiffness of the bridge deck, effectively avoid fatigue cracking of the steel structure and damage to the pavement layer. When applied to railway bridge decks, it can be used as a waterproof layer and wear-resistant layer to improve the service life of the railway bridge deck structure. Ultra-high toughness cement-based materials are entering a period of rapid development of large-scale applications.
[0003] As a new type of engineering material, ultra-high toughness cement-based materials have an extremely low water-binder ratio and a large amount of admixtures and admixtures. Therefore, their setting time is longer than that of ordinary concrete. The initial setting time under standard temperature environment is generally more than 10 hours. In low-temperature or even negative-temperature application environments, ultra-high toughness cement-based materials have a longer setting time and slow strength development. On the one hand, unhardened cement-based materials are susceptible to freezing damage, and on the other hand, they are slow to set, resulting in the inability to carry out construction continuously. The ultra-long setting time in low-temperature environments seriously affects the stable growth of material performance and the normal advancement of construction applications.
[0004] Therefore, it is necessary to develop an early-strength ultra-high toughness cement-based material suitable for use in low-temperature environments, so that it has ultra-high toughness and can still undergo a relatively fast hydration reaction under low and negative temperature conditions, with good early strength and stable performance development in the later stage. Summary of the invention
[0005] The embodiments of the present application provide an early-strength ultra-high toughness cement-based material and a preparation method thereof, so as to solve the problems of long setting time and slow development of low-temperature strength of ultra-high toughness cement-based materials in the related art.
[0006] The technical solutions provided by this application are as follows:
[0007] In a first aspect, the present application provides an early-strength ultra-high toughness cement-based material, which comprises the following raw materials by mass percentage:
[0008] 25% to 35% of Portland cement, 2%-10% of sulphoaluminate cement, 20% to 40% of quartz sand, 3% to 10% of microsilica powder, 3% to 8% of fly ash beads, 2% to 10% of limestone powder, 1% to 5% of modified CSH nanocrystals, 2% to 8% of ultrafine mineral powder, 2% to 10% of quartz powder, 0.1% to 0.5% of nano calcium carbonate, 0.1% to 0.5% of silica microspheres, 0.5% to 0.8% of water reducer, 0.1% to 0.6% of defoaming agent, 3% to 10% of copper-plated steel fiber, and 7% to 10% of water.
[0009] In some embodiments, the particle size of the nano calcium carbonate is 30 to 100 nm;
[0010] And / or, the particle size of the silica microspheres is 150 to 300 μm, and the content of spherical particles is ≥ 90 wt%;
[0011] And / or, the average particle size of the modified CSH nanocrystals is 30-40 μm.
[0012] In some embodiments, the particle size distribution of the quartz sand includes 0.63-1.25 mm and 0.16-0.63 mm;
[0013] And / or, the sum of the contents of SiO2 and Al2O3 in the microsilica powder is ≥ 93wt%;
[0014] And / or, the density of the microsilica powder is ≥2200kg / m 3 , with a specific surface area of 15000~20000m 2 / kg.
[0015] In some embodiments, the fly ash beads have a spherical particle content of ≥50wt% and a relative density greater than 1;
[0016] And / or, the sum of the contents of SiO2 and Al2O3 in the fly ash beads is ≥58wt%, and the specific surface area is ≥2358m 2 / kg;
[0017] and / or, the content of CaCO3 in the limestone powder is ≥97wt%;
[0018] And / or, the particle size of the limestone powder is 200-400 meshes.
[0019] In some embodiments, the ultrafine mineral powder has a chloride ion content of ≤0.06wt% and a specific surface area of ≥600m 2 / kg, moisture content ≤1wt%;
[0020] And / or, the SiO2 content in the quartz powder is ≥ 96wt%;
[0021] And / or, the particle size of the quartz powder is 80-200 mesh.
[0022] In some embodiments, the copper-coated steel fiber has a tensile strength of ≥1700 MPa, a length of 12 to 18 mm, and a diameter of 0.18 to 0.3 mm;
[0023] And / or, the water reducing agent includes a polycarboxylic acid high performance powder water reducing agent.
[0024] In a second aspect, the present application provides a method for preparing the early-strength ultra-high toughness cement-based material as described above, comprising the following steps:
[0025] Mix and stir silicate cement, sulphoaluminate cement, quartz sand, microsilica powder, fly ash beads, limestone powder, ultrafine mineral powder, quartz powder, water reducing agent, defoaming agent and copper-plated steel fiber;
[0026] Add modified CSH nanocrystals, nano-calcium carbonate, and silicon dioxide microspheres, and stir and mix until uniform to obtain a premix;
[0027] Water is added and stirred until fluidized to obtain an early strength and ultra-high toughness cement-based material.
[0028] In some embodiments, the preparation method further comprises the following step of preparing modified CSH nanocrystals:
[0029] The calcium source aqueous solution and the silicon source aqueous solution are mixed, sodium hydroxide is added to adjust the pH value of the solution to above 13, a water reducing agent is added for dispersion, and the mixture is reacted in a reactor at 110-190° C. for 6-8 hours to obtain a hydrated calcium silicate active slurry;
[0030] Polyethylene glycol is added to the calcium silicate hydrate active slurry, and the mixture is stirred at a constant temperature, dried, and calcined to obtain modified CSH nanocrystals.
[0031] In some embodiments, the calcium source includes calcium oxide;
[0032] And / or, the silicon source comprises rice husk ash, the average particle size of the rice husk ash is 50-100 μm, and the silicon dioxide content is ≥90 wt%.
[0033] And / or, the molecular weight of the polyethylene glycol is 200 to 1600, and the mass concentration is 0.2% to 0.8%.
[0034] In some embodiments, the molar ratio of CaO in the calcium source to SiO2 in the silicon source is (1.4-1.7):1.
[0035] The beneficial effects of the technical solution provided by this application include:
[0036] The present application adopts a composite of silicate cement and sulphoaluminate cement as the main cementitious material. The addition of sulphoaluminate cement gives the cement-based material good early strength performance. By mixing modified CSH nanocrystals, nano-calcium carbonate and micron-sized silica spherical particles, on the one hand, a crystal nucleus effect is formed to further promote the formation of hydration products and improve the early and long-term performance of ultra-high toughness cement-based materials. On the other hand, the micro-nanocrystalline material is beneficial to the uniformity of distribution of hydration products of the sulphoaluminate cement structure and the stability of the hexacoordinated alumina octahedron, thereby improving the internal microstructure of the concrete material, increasing the strength, and avoiding the risk of later strength shrinkage of ordinary sulphoaluminate early-strength cement-based materials, so that the cement-based material has the advantages of ultra-high toughness, early strength, long-term stability, and low-temperature construction. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0038] Figure 1 This is a long-term drying shrinkage development diagram of the cement-based materials prepared in the examples and comparative examples of the present application. DETAILED DESCRIPTION
[0039] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be clearly and completely described below in combination with the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0040] In a first aspect, the present application provides an early-strength ultra-high toughness cement-based material, which comprises the following raw materials by mass percentage:
[0041] 25% to 35% of Portland cement, 2%-10% of sulphoaluminate cement, 20% to 40% of quartz sand, 3% to 10% of microsilica powder, 3% to 8% of fly ash beads, 2% to 10% of limestone powder, 1% to 5% of modified CSH nanocrystals, 2% to 8% of ultrafine mineral powder, 2% to 10% of quartz powder, 0.1% to 0.5% of nano calcium carbonate, 0.1% to 0.5% of silica microspheres, 0.5% to 0.8% of water reducer, 0.1% to 0.6% of defoaming agent, 3% to 10% of copper-plated steel fiber, and 7% to 10% of water.
[0042] Specifically, the water-to-cement ratio of the early-strength ultra-high toughness cement-based material provided in the present application is 0.16 to 0.18.
[0043] Specifically, the silicate cement is selected from ordinary silicate cement with a strength grade of 42.5 or above.
[0044] The sulphoaluminate cement is selected from 42.5 grade low alkalinity high aluminum sulphoaluminate cement, and the mass percentage of calcium sulphoaluminate is ≥50%.
[0045] Portland cement has high late strength, and sulphoaluminate has high early strength. The two are used in combination to give ultra-high toughness cement-based materials good early strength properties, and can still undergo relatively fast hydration reactions under low temperature and negative temperature conditions. However, if sulphoaluminate cement is simply compounded, there is a risk of later strength shrinkage. The present application mixes modified CSH nanocrystals, nano-calcium carbonate, and micron-sized silica spherical particles to form a crystal nucleus effect on the one hand, further promote the formation of hydration products, and improve the early and long-term properties of ultra-high toughness cement-based materials. On the other hand, micro-nanocrystalline materials are beneficial to the uniformity of distribution of hydration products of sulphoaluminate cement structure and the stability of hexacoordinated alumina octahedrons, thereby improving the internal microstructure of concrete materials, increasing strength, and avoiding the risk of later strength shrinkage in ordinary sulphoaluminate early-strength cement-based materials, so that cement-based materials have the advantages of ultra-high toughness, early strength, long-term stability, and low-temperature construction.
[0046] In some embodiments, the particle size of the nano calcium carbonate is 30 to 100 nm;
[0047] And / or, the particle size of the silica microspheres is 150 to 300 μm, and the content of spherical particles is ≥ 90 wt%;
[0048] And / or, the average particle size of the modified CSH nanocrystals is 30-40 μm.
[0049] The formula of the application mixes nano-scale calcium carbonate, micron-scale silicon dioxide and micron-scale modified CSH nanocrystals to form a multi-level particle size structure crystal nucleus, optimize the microstructure, achieve a dense stacking effect, further improve the hardening density of the cement-based material, and give the cement-based material long-term stability.
[0050] In some embodiments, the particle size distribution of the quartz sand includes 0.63-1.25 mm and 0.16-0.63 mm;
[0051] And / or, the sum of the contents of SiO2 and Al2O3 in the microsilica powder is ≥ 93wt%;
[0052] And / or, the density of the microsilica powder is ≥2200kg / m 3 , with a specific surface area of 15000~20000m2 / kg.
[0053] In a preferred embodiment, the SiO2 content of the quartz sand is ≥ 97wt%
[0054] The addition of quartz sand helps to reduce the use of cement and additives, which helps to reduce costs, and its final performance is more stable and has higher adhesion;
[0055] The micro-filling effect and high pozzolanic activity of microsilica can enable the particles of ultra-high toughness cement-based materials to achieve the most densely packed state and promote the secondary hydration of the cementitious system, thereby improving the matrix density and performance.
[0056] In some embodiments, the fly ash beads have a spherical particle content of ≥50wt% and a relative density greater than 1;
[0057] And / or, the sum of the contents of SiO2 and Al2O3 in the fly ash beads is ≥58wt%, and the specific surface area is ≥2358m 2 / kg;
[0058] and / or, the content of CaCO3 in the limestone powder is ≥97wt%;
[0059] And / or, the particle size of the limestone powder is 200-400 meshes.
[0060] Limestone powder can provide the expansion energy required to compensate for cement-based shrinkage, and the expansion reaction rate is controllable, which can better fit the temperature drop shrinkage and drying shrinkage process of cement-based materials.
[0061] In some embodiments, the ultrafine mineral powder has a chloride ion content of ≤0.06wt% and a specific surface area of ≥600m 2 / kg, moisture content ≤1wt%;
[0062] And / or, the SiO2 content in the quartz powder is ≥ 96wt%;
[0063] And / or, the particle size of the quartz powder is 80-200 mesh.
[0064] Ultrafine mineral powder has a small particle size and can effectively fill the pores in the mortar, reduce the cement content, reduce the hydration heat, and enhance the fluidity of the mortar.
[0065] In some embodiments, the copper-coated steel fiber has a tensile strength of ≥1700 MPa, a length of 12 to 18 mm, and a diameter of 0.18 to 0.3 mm;
[0066] And / or, the water reducing agent includes a polycarboxylic acid high performance powder water reducing agent.
[0067] In a second aspect, the present application provides a method for preparing the early-strength ultra-high toughness cement-based material as described above, comprising the following steps:
[0068] Mix and stir silicate cement, sulphoaluminate cement, quartz sand, microsilica powder, fly ash beads, limestone powder, ultrafine mineral powder, quartz powder, water reducing agent, defoaming agent and copper-plated steel fiber;
[0069] Add modified CSH nanocrystals, nano-calcium carbonate, and silicon dioxide microspheres, and stir and mix until uniform to obtain a premix;
[0070] Water is added and stirred until fluidized to obtain an early strength and ultra-high toughness cement-based material.
[0071] Specifically, the water can be clean tap water.
[0072] The above raw materials can be stirred in a blender.
[0073] In some embodiments, the preparation method further comprises the following steps of preparing modified CSH nanocrystals:
[0074] 101: Mixing the calcium source aqueous solution and the silicon source aqueous solution, adding sodium hydroxide to adjust the pH value of the solution to above 13, adding a water reducing agent for dispersion, reacting in a reactor at 110-190° C. for 6-8 hours, and obtaining a hydrated calcium silicate active slurry;
[0075] 102: Add polyethylene glycol to the calcium silicate hydrate active slurry, stir at a constant temperature, dry, and calcine to obtain modified CSH nanocrystals.
[0076] Specifically, the water reducer is selected from polycarboxylic acid high performance water reducer.
[0077] Specifically, “101: mixing the calcium source aqueous solution and the silicon source aqueous solution, adding sodium hydroxide to adjust the pH value of the solution to above 13, adding a water reducing agent for dispersion, and reacting in a reactor at 110-190° C. for 6-8 hours” includes the following steps:
[0078] The calcium source aqueous solution and the silicon source aqueous solution are mixed, sodium hydroxide is added to adjust the pH value of the solution to above 13, a water reducer is added for dispersion, and the mixture is placed in a reactor and stirred at 110-190°C for 6-8h, with a stirring speed of 80-160r / min and a reactor pressure of 1.8-2.1MPa.
[0079] Specifically, “102: adding polyethylene glycol to the calcium silicate hydrate active slurry, stirring at a constant temperature, drying, and calcining” includes the following steps:
[0080] Polyethylene glycol was added to the calcium silicate hydrate active slurry, and the mixture was placed in a 90° C. water bath and stirred for 2 h. After stirring, the mixture was dried in a 100° C. constant temperature drying oven to obtain a mixed powder, and the mixed powder was calcined at 400° C. for 2 h.
[0081] In some embodiments, the calcium source comprises calcium oxide;
[0082] And / or, the silicon source comprises rice husk ash, the average particle size of the rice husk ash is 50-100 μm, and the silicon dioxide content is ≥90 wt%.
[0083] And / or, the molecular weight of the polyethylene glycol is 200 to 1600, and the mass concentration is 0.2% to 0.8%.
[0084] Specifically, the calcium source can be selected from a high-purity calcium oxide reagent, and the purity of the calcium oxide is ≥99.5%.
[0085] The silicon source is selected from rice husk ash. The porous rice husk ash is used as the silicon source for the modified CSH nanocrystals. Combined with polyethylene glycol-modified CSH, the porous structure characteristics of the final modified CSH nanocrystal material are more significant. In the cement hydration process, it not only produces a crystal nucleus effect, but also provides water storage and release effects, thereby providing power for continuous hydration inside the high-density early-strength ultra-high toughness cement-based material.
[0086] In some embodiments, the molar ratio of CaO in the calcium source to SiO2 in the silicon source is (1.4-1.7):1.
[0087] The present application is further described below through specific examples.
[0088] Example 1
[0089] An early strength ultra-high toughness cement-based material, comprising the following raw materials by mass percentage:
[0090] 25% Portland cement, 8% sulphoaluminate cement, 30% quartz sand, 4% microsilica powder, 5% fly ash beads, 2% limestone powder, 2.4% modified CSH nanocrystals, 3% ultrafine mineral powder, 4% quartz powder, 0.3% nano calcium carbonate, 0.3% silica microspheres, 0.6% polycarboxylic acid high-performance powder water reducer, 0.4% defoaming agent, 7% copper-plated steel fiber, and 8% clean tap water.
[0091] The preparation process is as follows:
[0092] Preparation of modified CSH nanocrystals:
[0093] The calcium oxide reagent and the low-temperature rice husk ash powder aqueous solution are mixed, sodium hydroxide is added to adjust the pH value of the solution to above 13, 0.2% of a polycarboxylic acid high-performance water reducer is added for dispersion, and the mixture is placed in a reactor at 110 to 190° C. for heating, stirring and mixing for 6 to 8 hours, with a stirring speed of 80 to 160 r / min and a reactor pressure of 1.8 to 2.1 MPa to obtain a hydrated calcium silicate active slurry; polyethylene glycol is added to the active slurry, and the mixture is placed in a 90° C. water bath environment and stirred for 2 hours. After the stirring is completed, the mixture is dried in a 100° C. constant temperature drying oven to obtain a mixed powder, and the mixed powder is calcined at 400° C. for 2 hours to obtain a modified CSH nanocrystal;
[0094] Preparation of early-strength ultra-high toughness cement-based materials:
[0095] Add silicate cement, sulphoaluminate cement, quartz sand, microsilica powder, fly ash beads, limestone powder, ultrafine mineral powder, quartz powder, polycarboxylic acid high-performance powder water reducer, defoamer, and copper-plated steel fiber into a mixer and mix for 1.5 minutes;
[0096] Then, the modified CSH nanocrystals, nano-calcium carbonate and silica microspheres were added into a blender and stirred for 1 min until uniform to obtain a premix;
[0097] Add clean tap water and stir for 3 minutes until it becomes fluidized to obtain an early-strength ultra-high toughness cement-based material.
[0098] Example 2
[0099] An early strength ultra-high toughness cement-based material, comprising the following raw materials by mass percentage:
[0100] 25% Portland cement, 8% sulphoaluminate cement, 30% quartz sand, 4% microsilica powder, 3.4% fly ash beads, 2% limestone powder, 4% modified CSH nanocrystals, 3% ultrafine mineral powder, 2% quartz powder, 0.3% nano calcium carbonate, 0.3% silica microspheres, 0.6% polycarboxylic acid high-performance powder water reducer, 0.4% defoaming agent, 7% copper-coated steel fiber, and 8% clean tap water.
[0101] The preparation process is as follows:
[0102] Preparation of modified CSH nanocrystals:
[0103] The calcium oxide reagent and the low-temperature rice husk ash powder aqueous solution are mixed, sodium hydroxide is added to adjust the pH value of the solution to above 13, 0.2% of a polycarboxylic acid high-performance water reducer is added for dispersion, and the mixture is placed in a reactor at 110 to 190° C. for heating, stirring and mixing for 6 to 8 hours, with a stirring speed of 80 to 160 r / min and a reactor pressure of 1.8 to 2.1 MPa to obtain a hydrated calcium silicate active slurry; polyethylene glycol is added to the active slurry, and the mixture is placed in a 90° C. water bath environment and stirred for 2 hours. After the stirring is completed, the mixture is dried in a 100° C. constant temperature drying oven to obtain a mixed powder, and the mixed powder is calcined at 400° C. for 2 hours to obtain a modified CSH nanocrystal;
[0104] Preparation of early-strength ultra-high toughness cement-based materials:
[0105] Add silicate cement, sulphoaluminate cement, quartz sand, microsilica powder, fly ash beads, limestone powder, ultrafine mineral powder, quartz powder, polycarboxylic acid high-performance powder water reducer, defoamer, and copper-plated steel fiber into a mixer and mix for 1.5 minutes;
[0106] Then, the modified CSH nanocrystals, nano-calcium carbonate and silica microspheres were added into a blender and stirred for 1 min until uniform to obtain a premix;
[0107] Add clean tap water and stir for 3 minutes until it becomes fluidized to obtain an early-strength ultra-high toughness cement-based material.
[0108] Comparative Example 1
[0109] A conventional ultra-high toughness cement-based material, comprising the following raw materials by weight percentage:
[0110] 38% Portland cement, 30% quartz sand, 8% microsilica powder, 8% limestone powder, 0.6% polycarboxylic acid high-performance powder water reducer, 0.4% defoaming agent, 7% steel fiber, and 8% clean tap water.
[0111] The preparation process is as follows:
[0112] Add silicate cement, quartz sand, microsilica powder, limestone powder, polycarboxylic acid high-performance powder water reducer, defoamer, and steel fiber into a mixer and mix for 1.5 minutes;
[0113] Then, clean tap water was added and stirred for 3 minutes until the mixture became fluidized to obtain a conventional ultra-high toughness cement-based material.
[0114] Comparative Example 2
[0115] An ultra-high toughness cement-based material, comprising the following raw materials by mass percentage:
[0116] 25% Portland cement, 8% sulphoaluminate cement, 30% quartz sand, 4% microsilica powder, 5% fly ash beads, 2% limestone powder, 2.4% CSH nanocrystals, 3% ultrafine mineral powder, 4% quartz powder, 0.3% nano calcium carbonate, 0.3% silica microspheres, 0.6% polycarboxylic acid high performance powder water reducer, 0.4% defoamer, 7% copper-coated steel fiber, and 8% clean tap water.
[0117] The preparation process is as follows:
[0118] Preparation of CSH nanocrystals:
[0119] The calcium oxide reagent and the low-temperature rice husk ash powder aqueous solution are mixed, sodium hydroxide is added to adjust the pH value of the solution to above 13, 0.2% of a polycarboxylic acid high-performance water reducer is added for dispersion, and the mixture is placed in a reactor at 110 to 190° C. for heating, stirring and mixing for 6 to 8 hours, with a stirring speed of 80 to 160 r / min and a reactor pressure of 1.8 to 2.1 MPa to obtain a hydrated calcium silicate active slurry, and the obtained active slurry is dried in a constant temperature drying oven at 100° C. to obtain a solid mixture CSH nanocrystals;
[0120] Preparation of ultra-high toughness cement-based materials:
[0121] Add silicate cement, sulphoaluminate cement, quartz sand, microsilica powder, fly ash beads, limestone powder, ultrafine mineral powder, quartz powder, polycarboxylic acid high-performance powder water reducer, defoamer, and copper-plated steel fiber into a mixer and mix for 1.5 minutes;
[0122] Then, CSH nanocrystals, nano-calcium carbonate and silica microspheres were added into a blender and stirred for 1 min until uniform to obtain a premix;
[0123] Add clean tap water and stir for 3 minutes until it becomes fluidized to obtain an ultra-high toughness cement-based material.
[0124] Comparative Example 3
[0125] The ultra-high toughness cement-based material provided in this comparative example 3 includes most of the raw materials of Example 1, and the only difference is that:
[0126] No nano calcium carbonate is added.
[0127] Comparative Example 4
[0128] The ultra-high toughness cement-based material provided in this comparative example 4 includes most of the raw materials of Example 1, and the only difference is that:
[0129] No silica microspheres added.
[0130] Comparative Example 5
[0131] The ultra-high toughness cement-based material provided in this comparative example 5 includes most of the raw materials of Example 1, and the only difference is that:
[0132] No modified CSH nanocrystals were added.
[0133] Performance Testing
[0134] The cement-based materials prepared in Examples 1-2 and Comparative Examples 1-5 were subjected to the following performance tests:
[0135] (1) Setting time: The setting time performance under low temperature environment (5°C) was tested with reference to GB / T50080-2016 "Standard for test methods of performance of ordinary concrete mixtures". The results are shown in Table 1:
[0136] Table 1: Coagulation time performance in low temperature environment (5°C)
[0137] Example 1 Example 2 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Initial setting time / h 6.8 5.7 17.6 14.7 11.6 11.8 15.1 Final setting time / h 10.5 9.6 23.8 16.2 13.7 14.2 16.9
[0138] According to the data in Table 1, it can be seen that the initial setting time of Example 1 and Example 2 under 5°C environment is 6.8h and 5.7h respectively, and the final setting time is 10.5h and 9.6h respectively. Under low temperature environment, the initial setting time of Example 1 is shortened by 61.3%, 53.7%, 41.4%, 42.4% and 55% respectively compared with Comparative Example 1, Comparative Example 2, Comparative Example 3, Comparative Example 4 and Comparative Example 5, and the final setting time is shortened by 55.9%, 35.2%, 23.4%, 26% and 37.9% respectively. The setting time is significantly shortened. The initial setting time of Example 2 is shortened by more than 50% compared with each comparative example, and the final setting time is also greatly reduced.
[0139] It is explained that the early-strength ultra-high toughness cement-based material provided in this application can effectively shorten the setting time of the ultra-high toughness cement-based material and meet the requirements of the low-temperature construction cycle.
[0140] (2) Compressive strength: The compressive strength of each group of specimens cured in a low temperature environment (5°C) at 1d and 28d was tested with reference to GB / T50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete". The results are shown in Table 2:
[0141] Table 2: Compressive strength performance under low temperature environment (5℃)
[0142]
[0143] According to the data in Table 2, it can be seen that the 1d compressive strength of Example 1 and Example 2 under 5°C environment is 40.4MPa and 62.8MPa respectively, and the compressive strength at 28d is 134.5MPa and 144.6MPa respectively. Among them, the conventional comparative example 1 has the lowest 1d compressive strength. Since it does not contain early strength components, the 1d compressive strength develops slowly. Comparative example 2 is mixed with unmodified CSH nanocrystals. Compared with comparative example 5 without adding CSH nanocrystals, the early strength and late strength are slightly improved. However, since the CSH in comparative example 2 is not modified, the CSH dispersion is low, and the effect of improving the performance of cement-based hardened body is limited, so it is still lower than that of the embodiment. Nano calcium carbonate and silica microspheres can provide sufficient volcanic ash effect for ultra-high toughness cement-based materials with low water-binder ratio, and promote the formation of hydration products. Comparative Examples 3 and 4 did not add nano calcium carbonate and silica microspheres, respectively, and therefore lost the assistance of these two nanomaterials, resulting in their 28d compressive strength being reduced by 25.6% and 25.2% respectively compared with Example 2. Under low temperature environment, the 1d-age compressive strength of Examples 1-2 is significantly improved compared with that of Comparative Examples 1-5, and the 28d-age compressive strength also develops steadily, exceeding the compressive strength of conventional ultra-high toughness cement-based materials and other comparative examples, indicating that the early-strength ultra-high toughness cement-based materials provided by the present application can achieve rapid development of early strength of ultra-high toughness cement-based materials under low temperature environment, and stable growth of compressive strength in the later period.
[0144] (3) Flexural strength: The flexural strength of each group of specimens cured in a low temperature environment (5°C) at 1d and 28d was tested with reference to GB / T50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete". The results are shown in Table 3:
[0145] Table 3: Flexural strength performance under low temperature environment (5°C)
[0146]
[0147] According to the data in Table 3, it can be seen that the 1d flexural strength of Example 1 and Example 2 under 5°C environment are 10.5MPa and 11.3MPa respectively, and the 28d flexural strength are 28.6MPa and 31.2MPa respectively. Under low temperature environment, the 1d flexural strength of Examples 1-2 is increased by more than several times compared with that of Comparative Examples 1-5, and the 28d flexural strength is also significantly increased, which greatly improves the flexural strength of the ultra-high toughness cement-based material. This shows that the early-strength ultra-high toughness cement-based material provided in the present application can achieve rapid development of the early flexural strength of the ultra-high toughness cement-based material under low temperature environment, has certain flexural and tensile properties, and the later flexural strength increases steadily under low temperature environment.
[0148] (4) Drying shrinkage: The long-term drying shrinkage of each group of specimens was tested with reference to GB / T50082-2009 "Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete". The results are as follows: Figure 1 As shown:
[0149] See also Figure 1 As shown, the drying shrinkage rates of the ultra-high toughness cement-based materials prepared in Example 1, Example 2, and Comparative Examples 1-5 are 206×10 -6 , 180×10 -6 407×10 -6 ,245×10 -6 ,271×10 -6 ,279×10 -6 , 380×10 -6 Compared with comparative examples 1-5, the drying shrinkage at 120d of Example 1 and Example 2 is significantly reduced, indicating that the early-strength ultra-high toughness cement-based material provided by the present application has fast early hydration and a dense internal structure, which reduces the humidity difference between the inside and outside of the material, resulting in a low long-term shrinkage rate and good durability and volume stability.
[0150] In summary, the early-strength ultra-high toughness cement-based material provided in this application has a more stable performance growth in a low-temperature environment, and achieves rapid and stable development, which can meet the application needs in a low-temperature environment.
[0151] It should be noted that, in this application, the terms "include", "comprises" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, an element defined by the sentence "includes a ..." does not exclude the existence of other identical elements in the process, method, article or device including the element.
[0152] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A method for preparing an early-strength ultra-high toughness cement-based material, characterized in that: The steps include: Mix and stir silicate cement, sulphoaluminate cement, quartz sand, microsilica powder, fly ash beads, limestone powder, ultrafine mineral powder, quartz powder, polycarboxylic acid high-performance powder water reducer, defoamer, and copper-plated steel fiber; Add modified CSH nanocrystals, nano-calcium carbonate, and silicon dioxide microspheres, and stir and mix until uniform to obtain a premix; Add water and stir until fluidized to obtain an early-strength ultra-high toughness cement-based material; The early-strength ultra-high toughness cement-based material comprises the following raw materials by mass percentage: Portland cement 25%, sulphoaluminate cement 8%, quartz sand 30%, microsilica fume 4%, fly ash beads 5%, limestone powder 2%, modified CSH nanocrystals 2.4%, ultrafine mineral powder 3%, quartz powder 4%, nano calcium carbonate 0.3%, silica microspheres 0.3%, polycarboxylic acid high-performance powder water reducer 0.6%, defoamer 0.4%, copper-plated steel fiber 7%, water 8%; Wherein, the preparation method further comprises the following steps of preparing modified CSH nanocrystals: The calcium source aqueous solution and the silicon source aqueous solution are mixed, sodium hydroxide is added to adjust the pH value of the solution to above 13, a polycarboxylic acid high-performance water reducer is added for dispersion, and the mixture is reacted in a reactor at 110-190° C. for 6-8 hours to obtain a hydrated calcium silicate active slurry; Adding polyethylene glycol to the calcium silicate hydrate active slurry, stirring at a constant temperature, drying, and calcining to obtain modified CSH nanocrystals; the average particle size of the modified CSH nanocrystals is 30-40 μm; The calcium source includes calcium oxide; the silicon source includes rice husk ash, the average particle size of the rice husk ash is 50-100 μm, and the silicon dioxide content is ≥90wt%.
2. The method for preparing the early-strength ultra-high toughness cement-based material according to claim 1, characterized in that: The particle size of the nano calcium carbonate is 30-100 nm; And / or, the particle size of the silica microspheres is 150-300 μm, and the content of spherical particles is ≥90 wt%.
3. The method for preparing the early-strength ultra-high toughness cement-based material according to claim 1, characterized in that: The particle size distribution of the quartz sand includes 0.63-1.25 mm and 0.16-0.63 mm; And / or, the sum of the contents of SiO2 and Al2O3 in the microsilica powder is ≥93wt%; And / or, the density of the microsilica powder is ≥2200kg / m 3 , with a specific surface area of 15000~20000m 2 / kg.
4. The method for preparing the early-strength ultra-high toughness cement-based material according to claim 1, characterized in that: The spherical particle content of the fly ash beads is ≥50wt%, and the relative density is greater than 1; And / or, the sum of the contents of SiO2 and Al2O3 in the fly ash beads is ≥58wt%, and the specific surface area is ≥2358 m 2 / kg; and / or, the content of CaCO3 in the limestone powder is ≥97wt%; And / or, the particle size of the limestone powder is 200-400 mesh.
5. The method for preparing the early-strength ultra-high toughness cement-based material according to claim 1, characterized in that: The ultrafine mineral powder has a chloride ion content of ≤0.06wt% and a specific surface area of ≥600m 2 / kg, moisture content ≤1wt%; And / or, the SiO2 content in the quartz powder is ≥96wt%; And / or, the particle size of the quartz powder is 80-200 mesh.
6. The method for preparing the early-strength ultra-high toughness cement-based material according to claim 1, characterized in that: The copper-plated steel fiber has a tensile strength of ≥1700 MPa, a length of 12-18 mm, and a diameter of 0.18-0.3 mm.
7. The method for preparing the early-strength ultra-high toughness cement-based material according to claim 1, characterized in that: The molecular weight of the polyethylene glycol is 200-1600, and the mass concentration is 0.2%-0.8%.
8. The method for preparing the early-strength ultra-high toughness cement-based material according to claim 1, characterized in that: The molar ratio of CaO in the calcium source to SiO2 in the silicon source is (1.4-1.7):1.