A kind of heat insulation material, fire-fighting clothing fabric and preparation method thereof
By attaching zeolite imidazolate framework compound and silica airgel composite material to aramid 1313 non-woven fabric, the problem of insufficient thermal insulation performance and strength of existing fire-fighting clothing insulation materials is solved, and high-efficiency thermal insulation and strength are achieved. Improved, fire-fighting clothing fabrics suitable for high-temperature environments.
Patent Information
- Application Number
- CN202310046686.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-31
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2043-01-31
AI Technical Summary
The thermal insulation performance and strength of existing fire-fighting clothing insulation materials are insufficient, resulting in unsatisfactory use in high-temperature environments, and the low strength of silica aerogel limits the use environment of the insulation layer.
A composite material of zeolite imidazole ester skeleton compound and silica aerogel is used. The zeolite imidazole ester skeleton compound is evenly dispersed in the silica aerogel solution and attached to the aramid 1313 non-woven fabric. Chemicalization, aging, replacement modification and drying treatments form thermal insulation materials with excellent thermal insulation performance and strength.
It significantly improves the thermal insulation performance and mechanical strength of the insulation material, reduces the thermal conductivity of the material, enhances the connection and friction between fibers, increases the strength of the aerogel, and is suitable for fire-fighting clothing fabrics in high-temperature environments.
Smart Images

Figure BDA0004055802680000061 
Figure BDA0004055802680000071 
Figure BDA0004055802680000072
Abstract
Description
Technical Field
[0001] The invention specifically relates to a heat insulating material, a fire-fighting clothing fabric and a preparation method thereof. Background Art
[0002] Aramid fiber, the full name of aromatic polyamide fiber, is a new type of high-tech synthetic fiber with super high strength, high modulus, high temperature resistance, acid and alkali resistance, light weight and other excellent properties. Aramid can be divided into meta-aramid (such as aramid 1313) and para-aramid (such as aramid 1414). Among them, aramid 1313 has long-lasting thermal stability, excellent flame retardancy, electrical insulation, outstanding chemical stability, excellent mechanical properties, super radiation resistance, etc.; while aramid 1414 is a high-strength, high-modulus fiber, and also has the advantages of low density, good toughness, excellent heat resistance, good acid and alkali resistance, and chemical solvent resistance. Because of its high thermal stability, aramid 1313 is often used in high-temperature resistant and heat-insulating fields such as firefighting clothing.
[0003] At present, aerogel materials are widely used in building insulation, aerospace, military and other fields due to their advantages such as light weight and low thermal conductivity. The thermal insulation layer of firefighting suit fabrics is mainly made of three-dimensional mesh knitted fabrics or non-woven materials. In order to improve the thermal insulation effect, the number of thermal insulation layers is often increased, making the firefighting suits thicker, while the thermal conductivity of the firefighting suits will not be significantly reduced, which not only increases the design difficulty but also increases the cost. Aerogel has the characteristics of light weight, high porosity, large specific surface area, low thermal conductivity, etc., which can solve this problem well, and the wearer can move freely under high temperature.
[0004] The existing technology uses a composite material of aramid fiber and silica aerogel as the thermal insulation layer of firefighting clothing, but the thermal insulation performance of this type of thermal insulation material needs to be further improved, and the strength of silica aerogel is relatively low, which will reduce the strength of the thermal insulation layer and limit the use environment of the thermal insulation layer. That is, the strength of this type of material also needs to be further improved. Summary of the invention
[0005] In view of this, an object of the present invention is to provide a method for preparing a thermal insulation material, wherein the thermal insulation material obtained by the preparation method has excellent thermal insulation performance and strength.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] A method for preparing a heat-insulating material comprises the following steps: uniformly dispersing a zeolite imidazolate skeleton compound in a silica aerogel solution to obtain a treatment liquid, attaching the treatment liquid to an aramid 1313 nonwoven fabric, and sequentially subjecting the treatment liquid to gelation, aging, replacement modification, and drying to obtain the heat-insulating material.
[0008] The aramid 1313 selected in the present invention has excellent thermal insulation effect. At the same time, the main component of the treatment liquid used is silica aerogel, which has low thermal conductivity and excellent thermal insulation effect, and can further improve the thermal insulation performance of the thermal insulation material. The treatment liquid uses zeolite imidazolate skeleton compound as a reinforcing agent, which can improve the mechanical strength of the final thermal insulation material.
[0009] According to some preferred implementation aspects of the present invention, the mass proportion of the zeolite imidazolate skeleton compound in the treatment liquid is 0.11-0.14%, preferably 0.12%, and the zeolite imidazolate skeleton compound particles are combined with silica aerogel to support the aerogel structure. In addition, the zeolite imidazolate skeleton compound has a large specific surface area and can also synergize to further improve the thermal insulation performance of the fabric and reduce the thermal conductivity of the material. At the same time, the CO2 adsorption performance of the zeolite imidazolate skeleton compound with a two-dimensional structure is significantly better than that of the zeolite imidazolate skeleton compound with a three-dimensional structure. When applied to the fabric of firefighting clothing, it can prevent the wearer from suffering from hypoxia due to excessive CO2 content.
[0010] According to some preferred embodiments of the present invention, the zeolite imidazolate framework compound is ZIF-L.
[0011] According to some preferred embodiments of the present invention, the silica aerogel aqueous solution is prepared by the following method:
[0012] Tetraethyl orthosilicate, ethanol and water are mixed in proportion, and then hydrochloric acid is added to adjust the pH value to acidic. After heating and stirring, ammonia water is added until the solution becomes alkaline to obtain the silica aerogel aqueous solution.
[0013] According to some preferred embodiments of the present invention, the molar ratio of tetraethyl orthosilicate, ethanol and water in the solution is: 1:(1-10):1.
[0014] According to some preferred embodiments of the present invention, the molar ratio of the tetraethyl orthosilicate to the hydrochloric acid is 1:(1×10 -4 -1×10 -3 ).
[0015] According to some preferred embodiments of the present invention, the treatment liquid is attached to the aramid nonwoven fabric by dripping the treatment liquid onto the aramid nonwoven fabric, and the treatment liquid is kept in a wet state for 0.5-2 hours after dripping. By dripping rather than the traditional dipping method (submerging the nonwoven fabric as a whole in the treatment liquid), the amount of silica aerogel on the fabric can be controlled, so that the treatment liquid is more evenly and fully filled in the fabric, and the amount of silica aerogel contained in fabrics in different batches is basically the same. When dripping, the dripping path can be reasonably planned, and the entire nonwoven fabric can be in a wet state.
[0016] According to some preferred embodiments of the present invention, the gelling time is 24-72 hours.
[0017] According to some preferred implementation aspects of the present invention, the aging time is 24-48 hours.
[0018] According to some preferred embodiments of the present invention, the replacement modification time is 12-48 hours.
[0019] According to some preferred embodiments of the present invention, the drying temperature is 30-80°C.
[0020] According to some preferred implementation aspects of the present invention, the drying time is 5-15 hours.
[0021] According to some preferred embodiments of the present invention, the aramid nonwoven fabric is washed and dried before being attached with the treatment liquid, and the drying temperature is 40-70°C.
[0022] In some embodiments of the present invention, the method for preparing the thermal insulation material specifically comprises the following steps:
[0023] S1: Cut a plurality of aramid 1313 nonwoven fabric samples with a length of 10 cm and a width of 10 cm, clean them, and put them into an oven to dry at 40-70°C.
[0024] S2: Dispersing different amounts of zeolite imidazolate framework compounds uniformly in the silica aerogel solution to obtain a treatment solution, in which the mass proportion of ZIF-L in the treatment solution is 0.11%-0.14%.
[0025] S3: Add the treatment liquid dropwise onto the aramid 1313 nonwoven fabric, and keep the soaked state for 0.5-2h after the addition, so that the silica and ZIF-L in the treatment liquid are better retained in the aramid 1313, and the amount of silica aerogel contained in each sample is controlled to be the same.
[0026] S4: Let the SiO2 / ZIF-L solution and aramid 1313 nonwoven fabric stand for a period of time (standing means adding the solution and then placing it in a container to wait for gelation), waiting for the treatment liquid to gel on the fabric. After the treatment liquid gels, the sample is subjected to post-treatment such as aging, replacement modification, and drying to finally obtain the thermal insulation material.
[0027] Among them, the standing time is 24-72h, the aging time is 24-48h, the replacement modification time is 12-48h, the drying temperature is 30-80°C, and the drying time is 5-15h.
[0028] The present invention also provides a heat insulating material prepared by the preparation method as described above.
[0029] The present invention also provides a fire-fighting suit fabric, comprising an outer layer, a waterproof breathable layer and a heat-insulating layer arranged in sequence from the outside to the inside, wherein the heat-insulating layer comprises the aforementioned heat-insulating material of the present invention.
[0030] According to some preferred embodiments of the present invention, the outer layer is made of a high-performance fiber material, and the high-performance fiber material is selected from aramid 1414 fiber, aramid 1313 fiber, polybenzimidazole (PBI) fiber, polyparaphenylene benzobisoxazole (PBO) fiber, or a blended fiber of aramid 1414 (mass fraction is 1-99%) and aramid 1313 (mass fraction is 1-99%). Preferably, 98% aramid 1313 / 2% aramid 1414.
[0031] According to some preferred implementation aspects of the present invention, the waterproof and breathable layer adopts a "membrane + flame retardant base fabric / cotton fabric" compounded by a lamination process, and the membrane is selected from PTFE (polytetrafluoroethylene) membrane, PE membrane, etc. Preferably, it is 100% aramid 1313 / PTFE (polytetrafluoroethylene) membrane.
[0032] The present invention also provides a fire-fighting suit, which is made of the above-mentioned fire-fighting suit fabric.
[0033] Due to the adoption of the above technical solution, the present invention has the following advantages compared with the prior art:
[0034] The thermal insulation material of the present invention uses aramid 1313 with excellent thermal insulation effect as a substrate, and then a treatment liquid is attached thereon. The silica aerogel in the treatment liquid has low thermal conductivity and excellent thermal insulation effect, which further improves the thermal insulation performance of the thermal insulation material.
[0035] The zeolite imidazolate skeleton compound powder in the treatment liquid of the present invention is a stable skeleton structure, and exhibits excellent mechanical properties when added to silica aerogel, increases the connection between aerogel particles and fibers, and increases the friction between fibers. The zeolite imidazolate skeleton compound powder is combined with the aerogel to play a certain supporting role in the aerogel structure, thereby improving the strength of the aerogel. Therefore, the composite material has excellent mechanical properties, and the zeolite imidazolate skeleton compound has a large specific surface area, and can also synergistically enhance the thermal insulation performance of the fabric and reduce the thermal conductivity of the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0037] Figure 1These are thermal images of firefighting clothing fabrics: (a) corresponding to Comparative Example 4; (b) corresponding to Comparative Example 5; (c) corresponding to Example 1.
[0038] Figure 2 Thermocouple test results of firefighting suit fabrics corresponding to Example 1, Comparative Example 4 and Comparative Example 5: (a) 60°C; (b) 90°C; (c) 120°C; (d) average temperature of firefighting suit fabrics at different temperatures after 10 minutes.
[0039] Figure 3 These are the thermal insulation test results of the firefighting clothing fabrics corresponding to Example 1, Comparative Example 4 and Comparative Example 5.
[0040] Figure 4 These are the thermal radiation protection performance results of the firefighting clothing fabrics corresponding to Example 1, Comparative Example 4 and Comparative Example 5. DETAILED DESCRIPTION
[0041] In order to enable those skilled in the art to better understand the technical solution of the present invention, the technical solution in the embodiments of the present invention is clearly and completely described below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0042] The zeolite imidazolate framework compound ZIF-L in the present invention is prepared in the laboratory, and the other raw materials are not particularly limited in their sources, and can be purchased on the market or prepared according to conventional methods well known to those skilled in the art. There is no particular limitation on the purity of all raw materials in the present invention, and the present invention preferably uses analytical purity or purity commonly used in the field of aerogel materials.
[0043] The present invention first cuts a plurality of 10×10 cm aramid 1313 nonwoven fabric samples, cleans them, and then dries them in an oven at 40-70°C. Then, a treatment solution with different ZIF-L mass proportions is prepared, and the mass proportion of ZIF-L in the treatment solution is 0.11%-0.14%. The treatment solution is dripped onto the aramid 1313 nonwoven fabric, so that silica and ZIF-L are better retained in the fabric, and the amount of silica aerogel contained in each sample is the same. After the dripping is completed, the infiltration state is maintained for 0.5-2 hours. Finally, the treatment solution and the aramid 1313 nonwoven fabric are allowed to stand for a period of time, and after the solution is gelled, the sample is subjected to post-treatments such as aging, replacement modification, and drying, and finally a thermal insulation material is obtained.
[0044] The silica aerogel aqueous solution configured in the present invention is prepared by an acid-base two-step method using tetraethyl orthosilicate as a raw material, and then ZIF-L is added to form a treatment solution. The molar ratio of tetraethyl orthosilicate, ethanol, and water in the silica aerogel aqueous solution of the present invention is: 1: (1-10): 1.
[0045] The present invention has no particular limitation on the aging conditions, and the conventional conditions for preparing silica aerogels known to those skilled in the art may be used. Those skilled in the art may select and adjust the conditions according to actual production conditions, product quality and product performance. The aging time described in the present invention is preferably 24-48 hours.
[0046] The present invention has no particular restrictions on the solvent and conditions for the replacement modification, and conventional solvents and conditions familiar to those skilled in the art may be used. Those skilled in the art may select and adjust the replacement modification according to actual production conditions, product quality and product performance. The replacement modification time of the present invention is preferably 12-48h; the solvent is preferably n-hexane and trimethylchlorosilane.
[0047] The present invention has no particular limitation on the drying process and conditions. The normal pressure drying process and conditions of such aerogels well known to those skilled in the art may be used. Those skilled in the art may select and adjust the drying process and conditions according to actual production conditions, product quality and product performance. The drying temperature of the present invention is preferably 30-80° C., and the drying time is preferably 5-15 h.
[0048] Example 1
[0049] This embodiment provides a heat insulation layer, and the preparation method thereof is as follows:
[0050] Step 1: Cut a number of aramid 1313 nonwoven fabric samples with a length of 10 cm and a width of 10 cm, clean them, and put them in an oven for drying.
[0051] Use a micrometer to test the thickness of the sample, perform multiple tests, and take the average value, which is recorded as h1. The number of samples must ensure that there are no less than 6 groups of samples of each specification, that is, 10×10cm aramid samples are one group, and each group has 3 samples.
[0052] Step 2: Prepare a treatment solution with a ZIF-L mass percentage of 0.12%.
[0053] Configuration steps:
[0054] Firstly, a SiO2 aerogel solution is prepared. The preparation method is divided into two steps: hydrolysis and polycondensation.
[0055] Tetraethyl orthosilicate, ethanol and water are mixed in a molar ratio of 1:3:1, and then hydrochloric acid is added to adjust the pH value to acidic. After heating and stirring, ammonia water is added until the solution becomes alkaline to obtain the silica aerogel solution.
[0056] Finally, 0.12% by weight of ZIF-L powder was added to obtain a treated solution after the ZIF-L powder was evenly dispersed in the silica aerosol solution.
[0057] Step 3: Add the treatment liquid dropwise onto the aramid 1313 nonwoven fabric, so that silica and ZIF-L are better retained in the fabric, and the amount of silica aerogel contained in each sample is the same.
[0058] Step 4: let the treatment liquid and the aramid 1313 nonwoven fabric stand for a period of time, wait for the treatment liquid to gel on the fabric, and after the solution is gelled, perform post-treatment such as aging, replacement modification, and drying on it to finally obtain a thermal insulation material, which is the thermal insulation layer.
[0059] Example 2
[0060] This embodiment is basically the same as Embodiment 1, except that the mass proportion of ZIF-L powder in the treatment solution is adjusted to 0.14%.
[0061] Comparative Example 1 to Comparative Example 3
[0062] Comparative Examples 1 to 3 are basically the same as Example 1, except that the mass proportion of ZIF-L powder in the treatment solution is adjusted to 0.06%, 0.08%, and 0.10%, respectively.
[0063] Comparative Example 4
[0064] This comparative example is basically the same as Example 1, except that no ZIF-L powder is added in the second step, and only SiO2 aerogel solution is used.
[0065] Comparative Example 5
[0066] This comparative example is basically the same as Example 1, except that in the second step, 0.12% by mass of ZIF-L powder is replaced with 0.8% by mass of polyimide PI (commercially available, soluble in organic solvents such as N,N-dimethylformamide and dichloromethane, with a molecular weight of 40,000).
[0067] Tests and Results
[0068] 1) Thermal conductivity of insulation materials
[0069] The thermal conductivity of the thermal insulation materials of various embodiments and comparative examples was calculated, and the results are shown in Table 1.
[0070] Table 1 Thermal conductivity of various insulation materials
[0071]
[0072]
[0073] 2) Mechanical properties
[0074] The mechanical properties of the thermal insulation materials of the embodiments and comparative examples were tested, and the results are shown in Table 2.
[0075] Table 2 Mechanical properties of various insulation materials
[0076] Stress(MPa) Elongation at break (%) Example 1 <![CDATA[0.12%SiO2 / AF / ZIF-L]]> 2.361±0.196 0.024±0.003 Example 2 <![CDATA[0.14%SiO2 / AF / ZIF-L]]> 1.963±0.120 0.028±0.002 Comparative Example 1 <![CDATA[0.06%SiO2 / AF / ZIF-L]]> 1.024±0.059 0.022±0.001 Comparative Example 2 <![CDATA[0.08%SiO2 / AF / ZIF-L]]> 2.322±0.150 0.022±0.001 Comparative Example 3 <![CDATA[0.10%SiO2 / AF / ZIF-L]]> 1.889±0.127 0.026±0.004 Comparative Example 4 <![CDATA[SiO2 / AF]]> 1.643±0.313 0.115±0.049
[0077] It can be seen that by treating aramid 1313 with a treatment solution containing ZIF-L and SiO2 in a specific proportion, a thermal insulation material with further improved thermal insulation and mechanical properties can be obtained.
[0078] 3) Thermal insulation performance of firefighting clothing fabric
[0079] The heat-insulating materials of Example 1, Comparative Example 4, and Comparative Example 5 are respectively made into fire-fighting clothing fabrics, which include an outer layer, a waterproof breathable layer, and a heat-insulating layer arranged in sequence from the outside to the inside. Among them, the outer layer is a blended fiber of 98% by mass of aramid 1313 / 2% by mass of aramid 1414, and the waterproof breathable layer is a 100% aramid 1313 / PTFE (polytetrafluoroethylene) film laminated. The heat-insulating layer is the heat-insulating layer of Example 1, Comparative Example 4, and Comparative Example 5.
[0080] The thermal insulation performance of each firefighting suit fabric is tested.
[0081] 3.1) Thermal conductivity of firefighting clothing fabrics
[0082] The thermal conductivity of each fire suit fabric was calculated, and the results are shown in Table 3. The results are the average values after multiple measurements.
[0083] Table 3 Thermal conductivity of various fire suit fabrics
[0084]
[0085]
[0086] 3.2) Thermal imaging test
[0087] Figure 1 It is a thermal imaging picture of the firefighting suit fabric corresponding to Example 1, Comparative Examples 4 and 5. According to the image colors, it can be seen that the color corresponding to Example 1 is the darkest, indicating that its surface temperature is the lowest and the thermal insulation performance is the best.
[0088] 3.3) Thermocouple comparison
[0089] Figure 2 The average surface temperature of the firefighting clothing fabrics at different positions of Example 1, Comparative Examples 4 and 5 and the temperature change curve close to the average after 10 minutes at three temperatures of 60°C, 90°C and 120°C. It can be seen that Example 1 has the best thermal insulation performance.
[0090] 3.4) Thermal insulation performance
[0091] Figure 3 The heat insulation performance of the firefighting clothing fabrics of Example 1, Comparative Examples 4 and 5 is shown by placing them on a heating platform at 60°C, 90°C and 120°C respectively, and recording the surface temperature of the fabric with a temperature measuring gun after 10 minutes. It can be seen that the heat insulation performance of Example 1 is the best.
[0092] 3.5) Thermal radiation protection performance test
[0093] The thermal radiation protection performance test method (RPP test) is one of the commonly used methods for measuring the thermal protection performance of thermal protective clothing internationally. The RPP test is mainly used to determine the radiation thermal protection performance of thermal protective clothing. Since thermal radiation is one of the main forms of heat transfer that causes thermal damage, this method can better test and evaluate the thermal protection performance of thermal protective clothing from one aspect, and has been widely used in fields such as forest firefighting.
[0094] The RPP results of the firefighting clothing fabrics corresponding to Example 1, Comparative Examples 4 and 5 are as follows: Figure 4 As shown. The heat flux of the three is 246.04KW / m 2 、286.66KW / m 2 、273.40KW / m 2 The size of the heat flux determines the protective performance of the composite fabric. The larger the heat flux, the worse the protective performance. It can be seen that the protective performance of Example 1 is the best.
[0095] 3.6) Second degree burn time
[0096] The thermal protection performance of thermal protective clothing is evaluated by two indicators: the second-degree burn time (t2nd) and the heat absorption when the sensor is exposed (EAE). The skin bioheat transfer model and the Henriques burn integral model are used to predict the skin burn time. The skin biothermal model takes into account the effect of blood flow on skin heat transfer. The Henriques burn integral model is used to predict the degree of skin burns, and its expression is:
[0097]
[0098] Where Ω is the quantitative value of the degree of skin burn injury; P is the frequency factor; ΔE is the skin activation energy; R is the gas molar constant; T is the absolute temperature of the basal layer of the second-degree burn (K); and t is the total time that t is greater than 317.15K.
[0099] The second-degree burn time of the laminated thermal insulation composite material is shown in Table 4, and this second-degree burn time is derived according to the formula. The second-degree burn time is the time taken by the simulated skin to reach the second-degree burn. The longer the second-degree burn time is, the longer it takes to reach the second-degree burn. The material has excellent protective performance and outstanding thermal insulation performance. From the table below, it can be seen that the firefighting suit fabric with a thermal insulation layer of 0.12% SiO2 / AF / ZIF-L takes the longest time to reach the second-degree burn, that is, it has the best thermal insulation protection effect.
[0100] Table 4 Secondary burn time of each fire suit fabric
[0101]
[0102] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the contents of the present invention and implement them accordingly. They cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A fire-fighting suit fabric, comprising an outer layer, a waterproof and breathable layer and a heat-insulating layer arranged in sequence from the outside to the inside, characterized in that: The thermal insulation layer includes a thermal insulation material, and the thermal insulation material is prepared by a preparation method comprising the following steps: uniformly dispersing a zeolite imidazolate skeleton compound in a silica aerogel solution to obtain a treatment liquid, attaching the treatment liquid to an aramid 1313 non-woven fabric, and then sequentially subjecting the treatment liquid to gelation, aging, replacement modification, and drying to obtain the thermal insulation material; the mass proportion of the zeolite imidazolate skeleton compound in the treatment liquid is 0.11% to 0.12%; and the zeolite imidazolate skeleton compound is ZIF-L.
2. The firefighting clothing fabric according to claim 1, characterized in that: The silica aerogel solution is prepared by the following method: Tetraethyl orthosilicate, ethanol and water are mixed in proportion, and then hydrochloric acid is added to adjust the pH value to acidic. After heating and stirring, ammonia water is added until the solution becomes alkaline to obtain the silica aerogel solution.
3. The firefighting clothing fabric according to claim 2, characterized in that: The molar ratio of tetraethyl orthosilicate, ethanol and water is: 1:(1-10):
1.
4. The firefighting clothing fabric according to claim 1, characterized in that: The treatment liquid is added dropwise onto the aramid 1313 nonwoven fabric, and the treatment liquid is kept in a wet state for 0.5-2 h after the addition, so that the treatment liquid is attached to the aramid 1313 nonwoven fabric.
5. The firefighting clothing fabric according to claim 1, characterized in that: The gelation time is 24-72 h; and / or, the aging time is 24-48 h.
6. The firefighting clothing fabric according to claim 1, characterized in that: The replacement modification time is 12-48 h.
7. The firefighting clothing fabric according to claim 1, characterized in that: The drying temperature is 30-80° C.; and / or the drying time is 5-15 h.
8. A fire-fighting suit, characterized in that: The fire-fighting suit is made of the fire-fighting suit fabric according to any one of claims 1 to 7.
Citation Information
Patent Citations
Method for preparing graphene oxide doped silica aerogel
CN107304052A
Aerogel composite aramid non-woven fabric thermal protection material and preparation method thereof
CN109457485A
Organic-inorganic hybrid heat-insulating film based on MOF / aerogel composite modification, and preparation method of organic-inorganic hybrid heat-insulating film
CN112625288A
Preparation method of fiber-reinforced silicon dioxide aerogel thermal insulation material
CN112897980A
Silicon dioxide / zeolite imidazate framework compound / aramid fiber composite non-woven material as well as preparation method and application thereof
CN115652621A