A method for preventing silk fabric from being damaged by washing and sand washing
Through the improved silk fabric process, combined with the use of industrial washing machines and jigger dyeing machines, the crease and washing resistance problems of sand-washed silk fabrics have been solved, and the effects of no creases, no dust marks, soft luster and soft waxy feel have been achieved , suitable for high-end silk products.
Patent Information
- Application Number
- CN202211719507.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-30
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-12-30
AI Technical Summary
The existing sand washing and finishing methods of silk fabrics have problems such as creases that are difficult to eliminate and poor washing resistance, which results in damage to the fabric's feel and gloss, affecting market prospects.
Adopt the process of wet setting-dyeing-wet setting-sand washing-tentering-rolling and soaking-water washing-pickling-wet setting-winding-tenttering, combined with industrial washing machine sand washing and jigger dyeing machine rolling and soaking. Softener and anti-washing damage additives ensure full fiber infiltration and handfeel protection.
It effectively removes creases and improves the fabric's anti-washing effect, making silk fabrics crease-free and dust-free, maintaining a soft luster and soft feel. It is suitable for large-area products such as bedding.
Abstract
Description
Technical Field
[0001] The invention discloses a method for preventing silk fabric from being damaged by washing and sand washing, and belongs to the technical field of silk dyeing and finishing. Background Art
[0002] The sand washing finishing of silk fabric means that the silk fabric is in a relaxed state, sand washing agent is used, and with the help of mechanical action, slight friction is generated between the silk surface and the silk surface, and between the silk surface and the machine, so that the microfibers coated with the outer layer of silk are loose and straightened, and the silk surface produces uniform and fine fluff, so that the silk fabric has a waxy and velvety feel. The silk fabric obtained after sand washing, referred to as sand washed silk, still has the unique warm luster of silk, but the luster is softer. Sand washed silk has a good market prospect due to its special soft and waxy feel and unique soft silk luster.
[0003] The applicant found in the research that the current sand washing finishing method has the following problems:
[0004] First, sand washing will produce creases that are difficult to eliminate, and such creases cannot be completely eliminated even through the subsequent stretching step. The existing technology mostly adopts dyeing-drying-setting-sand washing-drying-stretching, and the silk fabric finally obtained has many gray scratches and creases, which seriously affects the silk surface effect. When the sand washed silk is rotated against the light, obvious creases can be seen, which will affect the feel of the fabric and destroy the gloss of the sand washed silk. Moreover, such creases are deep, and it is difficult for the existing technology to completely eliminate them through subsequent finishing. After being made into wide and large-area products such as bedding, the creases are obvious, resulting in downstream customers not accepting them. They are judged as defective products during inspection and can only be sold at a lower grade and price.
[0005] Second, sand-washed silk has poor washing resistance and its appearance changes greatly after washing. Consumers often complain that sand-washed silk tends to become dull and lose its luster after washing, and in severe cases, "white stripes" appear on the silk surface. This disease is commonly known as "gray damage" in the industry.
[0006] This is because a silk thread used for weaving silk is made up of 6 to 12 silk cocoons, and each silk fiber is made up of 900 to 1400 fine fibers with a diameter of about 0.2 to 0.4 microns. Each fiber is made up of about 1000 microfibers with a diameter of about 100 to 150 angstroms. It looks like a thin thread, but it is actually made up of countless very fine single fibers. Such fine silk is easy to break and fall apart when the silk surface is rubbed against the silk surface and the silk surface and the object during household washing. This is because it is easy to break and fall apart when the silk surface is rubbed against the silk surface and the silk surface and the object during household washing. Because the scattered silk ends are very fine and there are many of them, the fiber surface is fibrillated, and the appearance is a fuzzy, gray and misty form. This is why real silk is easy to turn gray, lose its luster, and be damaged by gray after washing. If the laundry gets tangled and knotted during the washing and preparation process, forming wrinkles, and the loose ends are broken and distributed along the wrinkles, "white stripes" will be formed. The fibers of silk fabrics after sand washing are more fragile and more prone to washing damage, which cannot be repaired. According to the survey, 54% of consumers choose to wash silk in a washing machine, 35% choose to wash by hand, and 10% choose to go to a laundromat. Regardless of the washing method used, sand washed silk generally has the aforementioned "washing damage" problem, giving consumers the impression that "sand washed silk feels good, but is not easy to take care of", resulting in unsatisfactory sales of sand washed silk.
[0007] In the prior art, post-finishing is often performed by adding an anti-washing damage agent, but the anti-washing damage agent will destroy the soft and waxy feel of the sand-washed silk, and the anti-washing damage agent will also make the creases of the sand-washed silk more difficult to smooth out. Summary of the invention
[0008] The technical problem to be solved by the present invention is: to overcome the shortcomings of the prior art and provide a method for sand-washing finishing of silk fabric to prevent washing damage. The method can effectively solve the creases generated in the preparation process of sand-washed silk, and can also improve the subsequent anti-washing damage effect of the fabric. The obtained sand-washed silk has no creases or gray damage, is soft, glutinous, smooth, and has a soft luster.
[0009] The technical solution of the method adopted by the present invention to solve the technical problem is: the method for preventing silk fabric from being damaged by washing and sand washing comprises the following steps:
[0010] 1) Wet setting - 2) Dyeing - 3) Wet setting - 4) Sand washing - 5) Tentering - 6) Curling and soaking - 7) Water washing - 8) Acid washing - 9) Wet setting - 10) Air blowing - 11) Tentering;
[0011] 4) Sand washing: Use industrial washing machine for washing, 25~35℃ water temperature, sand washing 3~4 times, 4~5 minutes / time, the sand washing solution used is water, soda ash (chemical name sodium carbonate) 50~100g / L and softener 52~78g / L;
[0012] 6) Rolling and impregnation: put the silk fabric on the roller dyeing machine, add the solution into the dyeing tank of the roller dyeing machine, set the water temperature to 25-35℃, roll and run for 30-60min, and the speed to 40-60m / min, so that the silk fabric is impregnated with the solution; the solution is water and an anti-washing damage auxiliary agent, and the concentration of the anti-washing damage auxiliary agent is 3-5g / L.
[0013] The specific operation of step 1) wet setting is: setting the wet silk fabric after degumming at a setting temperature of 95-100°C; the specific operation of step 3) wet setting is: setting the wet silk fabric at a setting temperature of 100-105°C.
[0014] Step 9) The specific operation of wet setting is: setting the wet silk fabric at a setting temperature of 100~110℃.
[0015] The specific operation of the tentering in step 5) is: tentering by spraying steam at 100-110°C; the specific operation of the tentering in step 11) is: tentering by spraying steam at 110-120°C.
[0016] Step 10) The specific operation of drying is: pat and dry the silk fabric in a relaxed state, with the hot air temperature at 70-80°C and the drying time at 1-3 hours.
[0017] The dye used in step 2) is a reactive dye. Reactive dyes have a stable dyeing effect and are not easy to react with high concentrations of soda ash in subsequent sand washing, which can avoid discoloration of the silk fabric after sand washing. Preferably, the reactive dye in step 2) is an SE type reactive dye, which has the most stable dyeing effect and does not change color after sand washing.
[0018] The anti-washing damage aid in step 6) is anti-washing damage aid W-08. Anti-washing damage aid W-08 is produced by Japan Heian Oil Co., Ltd., and in conjunction with the operation of step 6) of the present invention, the anti-washing damage aid can be fully immersed in the silk fiber tow within a relatively low concentration range, achieving long-term anti-washing damage and avoiding affecting the feel of the fabric.
[0019] Step 9) The softener is a mixture of softener 3165 and finishing agent 6820 in a mass ratio of 10:3. After finishing in this ratio, the silk fabric feels the most fluffy, soft, and smooth, and can reduce the damage to the fabric during the sand washing process.
[0020] The specific operation of step 7) water washing is: 25~35°C water temperature, 2~3 times of water washing; the specific operation of step 8) acid washing is: 25~35°C water temperature, 1g / L acetic acid, 2~3 times of acid washing.
[0021] The present invention is described as follows:
[0022] Preferably, the sand washing time in step 4) is 12 to 16 minutes, and each sand washing is performed continuously.
[0023] Preferably, the dyeing method in step 2) is one of jig dyeing, pad dyeing and overflow dyeing; preferably, the dyeing method in step 2) is jig dyeing. The specific operation of step 2) is: jig dyeing the silk fabric, the dyeing temperature is 60-65°C, the pH value of the dye solution is 10-11, and the dyeing time is 120-180 minutes; the dye solution includes: water, 10-25 g / L of reactive dye, 30-50 g / L of sodium sulfate, and 4-8 g / L of soda ash;
[0024] Preferably, the industrial washing machine in step 4) is a horizontal drum type industrial washing machine.
[0025] Preferably, the specific operation of step 4) sand washing is: washing with an industrial washing machine, at a water temperature of 25-35° C., sand washing 3 times, 5 minutes per time, and the sand washing solution used is water, 80 g / L soda ash, and 65 g / L softener;
[0026] Preferably, step 6) rolling and soaking: adding solution to the dyeing tank of the roller dyeing machine, putting the silk fabric on the roller dyeing machine, 25~35℃ water temperature, rolling operation for 50min, speed 40m / min, so that the silk fabric is soaked in the solution; the solution is water and 4g / L of anti-washing damage auxiliary agent. Step 6) uses a roller dyeing machine because the applicant found that the roller dyeing process is to soak the silk fabric in the solution in the water tank through the cloth guide roller, and then the silk fabric leaves the solution, the wet silk fabric is rolled, and then the process is repeated. The rolling process does not go through the liquid squeezing, so the silk fabric is saturated with the solution and can be soaked in the solution for a long time, so that the anti-washing damage auxiliary agent can fully penetrate into the silk fiber, and the silk is more conducive to flattening creases in a wet state. In the process of rolling the layers of wet silk fabric, the deep creases on the silk fabric are naturally flattened as they are rolled.
[0027] The blowing in step 10) refers to: using the airflow to "air beat" the silk fabric, "processing the silk fabric, thereby improving its feel. "Air beating" can avoid the wrinkles or friction caused by the mechanical power of "mechanical beating" on the fabric, and will not cause damage to the fabric. Preferably, in step 10), the blowing adopts an open-width cloth feeding; preferably, in step 10), an open-width airflow softening machine is used, which can effectively avoid creases on the silk fabric during drying.
[0028] The wet state described in steps 1) wet setting, 3) wet setting, and 9) wet setting refers to the state in which the silk fabric is scooped out of the aqueous solution without dripping water. At this time, the fabric is rich in water and then directly put into the setting machine for setting, which is wet setting. In the field of silk fabrics, wet setting and dry setting are significantly different. Silk is a protein fiber, and wet setting of silk fabrics will be more conducive to flattening the fabric and removing creases.
[0029] The applicant has found that creases will continue to be generated during the preparation process. If the creases are not removed in time, they will continue to accumulate and become heavier as the preparation process proceeds, until after the sand washing step, deep creases that are difficult to remove will be formed. Steps 1) wet setting, 3) wet setting, and 9) wet setting are interspersed in the process to flatten the creases generated during the preparation process in time, avoiding the creases from becoming heavier and forming deeper creases.
[0030] Softener 3165 is a multi-polymer that can give fabrics a soft and lubricated feel, and give silk fabrics good fullness and resilience. Finishing agent 6820 can give fabrics a smooth feel, good stiffness and resilience. Softener 3165 and finishing agent 6820 are mixed in a mass ratio of 10:3, which can reduce the friction between silk surfaces and silk surfaces, and between silk surfaces and objects during washing, making the surfaces in contact with each other soft and smooth, which is conducive to reducing dust damage and improving the feel of silk fabrics.
[0031] The best dosage of the anti-washing damage additive W-08 is 3~5g / L for step 6) curling and impregnation design. Although adding too much will improve the anti-washing damage effect, the fiber bundles will have too strong a cohesive force, which will have an adverse effect on the waxy velvet feel of the silk fabric. If the amount is too little, it will not achieve a sufficient number of anti-washing damage times. The anti-washing damage additive W-08 works best when added at 3~5g / L.
[0032] Compared with the prior art, the present invention has the following beneficial effects:
[0033] 1. The sand-washing finishing method for silk fabrics of the present invention can effectively solve the creases generated in the preparation process of sand-washed silk.
[0034] The applicant found that since step 4) sand washing must be carried out in an industrial washing machine, the interval between forward and reverse sand washing is long, and the silk fabric is entangled and twisted on itself, forming creases that are difficult to remove. The prior art mostly uses direct drying and stretching after sand washing, which causes creases to remain on the silk fabric and are difficult to remove.
[0035] In the present invention, the applicant has designed the subsequent steps of 5) tentering - 6) rolling and impregnation - 7) washing - 8) acid washing - 9) wet setting. Step 5) tentering can remove shallow creases and make deep creases shallower; step 6) rolling and impregnation is to use the jigger machine usually used for dyeing as a finishing equipment, and the silk fabric can be fully flattened on the cloth roller and deep creases can be removed by rotating the jigger machine in the forward direction and rolling the impregnation solution - reverse rolling the impregnation solution; and the anti-washing damage auxiliary agent can be fully impregnated and attached to the silk fabric, so that the silk fabric has a long-term anti-washing damage effect; in addition, the removal of creases and finishing of fabrics are completed in step 6), which can save water. The obtained sand-washed silk has no creases and no ash damage, and has a soft luster.
[0036] 2. The method for preventing silk fabric from being damaged by washing and sand washing of the present invention can improve the subsequent anti-washing damage effect of the silk fabric. Consumers are less likely to suffer from washing damage after multiple washings after purchase, and the soft, glutinous and smooth feel of the sand-washed silk is not destroyed due to the anti-washing damage finishing.
[0037] The applicant discovered that the reason for washing damage is that during the washing process, the silk surfaces are easily worn off and scattered when rubbing against each other or between silk surfaces and objects. Since the scattered silk ends are very fine and numerous, the fiber surface is fibrillated, and the appearance is a fuzzy, gray and misty form. This is why real silk is easily grayish and has reduced luster and gray damage after washing. If the laundry is entangled and knotted during the washing process, wrinkles are formed, and the broken and scattered ends are distributed along the wrinkles, a "white stripe mark" is formed. Washing damage can be divided into two main aspects. The first is sand washing damage during the preparation process, and the second is caused by consumers washing by themselves after purchase.
[0038] The softener is added during the sand washing in step 4) of the present invention. The softener is added to the silk to reduce the friction between the silk surfaces and between the silk surfaces and between the silk surfaces and objects during the washing process, and the surfaces in contact with each other become soft and smooth, thereby improving the soft and glutinous hand feel after sand washing. The softener is also helpful in reducing the dust damage during the sand washing process, making the sand washing process softer, so there is no need to stop the machine for flattening during each sand washing, and each sand washing can be performed continuously.
[0039] However, the silk fibers are in a loose state after sand washing, and the cohesion of the fiber bundles decreases. Consumers buy silk products that are prone to fiber loosening and damage during washing. Therefore, the applicant designs the use of anti-washing damage additive W-08 in step 6). The main component of the anti-washing damage additive W-08 is a triazine inducer, which can covalently bond with silk fibers and cross-link itself to form a film on the fiber surface, thereby improving the cohesion of the fiber bundles and inhibiting the phenomenon of fiber opening and loosening during the washing process of silk, thereby achieving the anti-washing damage effect.
[0040] 3. The sand-washing finishing method for silk fabrics of the present invention can make the obtained silk fabrics soft, velvety and elastic; moreover, the obtained silk fabrics have good anti-washing damage effect, and at the same time will not affect the feel and gloss of the silk fabrics. DETAILED DESCRIPTION
[0041] The present invention is further described below in conjunction with specific embodiments, wherein Embodiment 1 is the best embodiment.
[0042] The equipment used in step 1) wet setting and step 3) wet setting is: German Monforts setting machine, model MONFONGS828 TWNAR 5F;
[0043] Step 4) sand washing, the equipment used is Taizhou Tongjiang Washing Machinery Factory, industrial washing machine GX-200, horizontal drum type;
[0044] The equipment used in step 5) air jet stenting and step 12) air jet stenting is: German Monforts setting machine, model MONFONGS 828 TWNAR 5F;
[0045] Step 6) The dyeing machine used for rolling and impregnation is a computerized dual-frequency normal temperature dyeing machine SMD300B-1800mm manufactured by Wuxi Gaotemei Machinery Manufacturing Co., Ltd.;
[0046] Step 9) soaking in softener and step 10) wet setting are carried out on the same equipment, and the softener is placed in a liquid tank set in front of the setting machine;
[0047] Step 11) The equipment used for air blowing is: FR2021 flat-width airflow softening machine produced by Jiangsu Fengrun Machinery Technology Co., Ltd.;
[0048] Step 2) The dye used for dyeing is produced by Huntsman Textile Dyeing Co., Ltd., and is an Acycloda SE type reactive dye. The dye used in Example 1 is Acycloda reactive light red SE, the dye used in Example 2 is Acycloda reactive golden yellow SE, and the dye used in Example 3 is Acycloda reactive light blue SE;
[0049] Step 6) The anti-washing injury aid is anti-washing injury aid W-08, produced by Japan Heian Oil & Fats Co., Ltd.
[0050] Step 9) The softener used was softener 3165, produced by Suzhou Liansheng Chemical Co., Ltd.; the finishing agent 6820, produced by Suzhou Liansheng Chemical Co., Ltd.
[0051] The silk fabric used is 15 momme silk electrospun.
[0052] Example 1
[0053] This embodiment includes the following steps:
[0054] 1) Wet setting: The wet silk fabric after degumming is set at a setting temperature of 100°C;
[0055] 2) Dyeing: Use reactive dye jig dyeing, dyeing temperature 65℃, dyeing solution pH 10, dyeing time 150 minutes; the dyeing solution includes: water, reactive dye 15 g / L, sodium sulfate 40 g / L, soda ash 5 g / L;
[0056] 3) Wet setting: Set the wet silk fabric at a setting temperature of 100°C
[0057] 4) Sand washing: Use an industrial washing machine for washing, 30°C water temperature, sand washing continuously for 3 times, 5 minutes per time, the sand washing solution used is water, 80g / L soda ash and 65g / L softener; the softener is a mixture of softener 3165 and finishing agent 6820 in a mass ratio of 10:3;
[0058] 5) Tentering: 100℃ steam spraying tentering;
[0059] 6) Rolling and impregnation: Add the solution into the dyeing tank of the roller dyeing machine, put the silk fabric on the roller dyeing machine, 30℃ water temperature, roll and run for 50 minutes, speed 50m / min, so that the silk fabric is impregnated with the solution; the solution is water and anti-washing damage auxiliary agent, and the concentration of the anti-washing damage auxiliary agent is 4g / L;
[0060] 7) Washing: 30℃ water temperature, 3 washes;
[0061] 8) Pickling: 30℃ water temperature, 1g / L acetic acid, 2 picklings;
[0062] 9) Wet setting: Set the wet silk fabric at a setting temperature of 105°C;
[0063] 10) Drying: Use hot air to pat and dry the silk fabric in a relaxed state, with the hot air temperature at 75°C and the time for 3 hours;
[0064] 11) Tentering: 115℃ steam spray tentering.
[0065] Example 2
[0066] 1) Wet setting: The wet silk fabric after degumming is set at a setting temperature of 100°C;
[0067] 2) Dyeing: Use reactive dye jig dyeing, dyeing temperature 60℃, dyeing solution pH 11, dyeing time 120~180 minutes; the dyeing solution includes: water, reactive dye 25 g / L, sodium sulfate 50 g / L, soda ash 8 g / L;
[0068] 3) Wet setting: Set the wet silk fabric at a setting temperature of 100°C
[0069] 4) Sand washing: Use an industrial washing machine for washing, 25°C water temperature, sand washing continuously for 3 times, 4 minutes per time, the sand washing solution used is water, 50g / L soda ash and 78g / L softener; the softener is a mixture of softener 3165 and finishing agent 6820 in a mass ratio of 10:3;
[0070] 5) Tentering: 110℃ steam spray tentering;
[0071] 6) Rolling and impregnation: Put the silk fabric on the roller dyeing machine, add the solution into the dyeing tank of the roller dyeing machine, the solution temperature is 25℃, and the roller runs for 30 minutes at a speed of 60m / min to flatten the silk fabric and impregnate the solution; the solution is water and anti-washing damage auxiliary agent, and the concentration of the anti-washing damage auxiliary agent is 5g / L;
[0072] 7) Washing: 25℃ water temperature, wash 3 times;
[0073] 8) Pickling: 25℃ water temperature, acetic acid 1g / L, pickling 3 times;
[0074] 9) Wet setting: Set the wet silk fabric at a setting temperature of 100°C;
[0075] 10) Drying: Use hot air to pat and dry the silk fabric in a relaxed state, with the hot air temperature at 70°C and the time for 2.5 hours;
[0076] 11) Tentering: 120℃ steam spray tentering.
[0077] Example 3
[0078] 1) Wet setting: The wet silk fabric after degumming is set at a setting temperature of 95°C;
[0079] 2) Dyeing: Use reactive dye jig dyeing, dyeing temperature 60℃, dyeing solution pH 11, dyeing time 120 minutes; the dyeing solution includes: water, reactive dye 10 g / L, sodium sulfate 30 g / L, soda ash 4 g / L;
[0080] 3) Wet setting: The wet silk fabric is set at a setting temperature of 105°C
[0081] 4) Sand washing: Use an industrial washing machine to wash, 35°C water temperature, sand wash 4 times continuously, 4 minutes / time, the sand washing solution used is water, 100g / L soda ash and 52g / L softener; the softener is softener 3165 and finishing agent 6820 mixed in a mass ratio of 10:3;
[0082] 5) Tentering: 105℃ steam spraying tentering;
[0083] 6) Rolling and impregnation: Put the silk fabric on the roller dyeing machine, add the solution into the dyeing tank of the roller dyeing machine, the solution temperature is 35℃, and the roller runs for 60 minutes at a speed of 40m / min to flatten the silk fabric and impregnate the solution; the solution is water and anti-washing damage auxiliary agent, and the concentration of the anti-washing damage auxiliary agent is 3g / L;
[0084] 7) Washing: 35℃ water temperature, 2 washes;
[0085] 8) Pickling: 35℃ water temperature, 1g / L acetic acid, pickling 3 times;
[0086] 9) Wet setting: Set the wet silk fabric at a setting temperature of 110°C;
[0087] 10) Drying: Use hot air to pat and dry the silk fabric in a relaxed state, with the hot air temperature at 80°C and the time for 1 hour;
[0088] 11) Tentering: 110℃ steam spray tentering.
[0089] Comparative Example 1
[0090] The preparation method of this comparative example is the same as that of Example 1, except that steps 5) to 9) are not performed.
[0091] Comparative Example 2
[0092] The preparation method of this comparative example is the same as that of Example 1, except that the wet setting of steps 1) and 3) is not performed.
[0093] Comparative Example 3
[0094] The preparation method of this comparative example is the same as that of Example 1, except that the infiltration method in step 6) is different.
[0095] Step 6 of this comparative example): The silk fabric is immersed in a rolling solution with a rolling rate of 80%, a solution temperature of 30°C, a solution of water and an anti-washing injury aid of 4g / L, the solution is placed in a rolling tank, and a lane is taken from the rolling tank at a speed of 40m / min.
[0096] Comparative Example 4
[0097] The preparation method of this comparative example is the same as that of Example 1, except that the solution used in step 6) is only water, and no anti-washing injury aid is used.
[0098] Comparative Example 5
[0099] The preparation method of this comparative example is the same as that of Example 1, except that the solution in step 6) is water and 8 g / L of an anti-washing injury aid.
[0100] Comparative Example 6
[0101] The preparation method of this comparative example is the same as that of Example 1, except that no softener is added in step 4).
[0102] Performance Testing
[0103] Test 1: Detection of crease defects
[0104] Manual inspection was adopted, 20 meters of the silk fabric obtained in each example was randomly sampled and visually observed, the total number of defects on each crease was recorded, and the average value was calculated. The average value of crease defects = total number of crease defects / 2×100% (unit: pieces / 10 meters, with one decimal place reserved).
[0105] Test 2: Washing defects during preparation
[0106] Manual inspection was adopted, 20 meters of the silk fabric obtained in each example was randomly sampled, visually observed, the total number of washing defects was recorded, and the average value was calculated. The average value of washing defects = total number of washing defects / 2×100% (unit: pieces / 10 meters, retain one decimal place).
[0107] Test 3: Number of wash injuries
[0108] In each example, 100 meters of silk fabric were cut, 50 meters of which were kept as a blank control and not washed. The remaining 50 meters were sewed with marks to simulate the daily washing process of consumers and washed repeatedly.
[0109] The process of each washing is as follows: put it into the washing machine, add silk detergent, wash and dehydrate at room temperature, take it out, dry it at 60℃ flat width, and dry it at 100℃ stretched width, compare it with the blank control, and observe whether there is obvious washing damage after this washing. Then repeat the next washing until obvious washing damage appears, and record the number of washing times.
[0110] Standard for obvious washing damage: Compared with the blank control, the silk fabric has a noticeably duller sheen, and the average number of washing damage defects is ≥ 1 per meter.
[0111] Washing machine: Haier Casarte drum-type fully automatic washing machine model C1HD10G3ELU1, maximum speed: 800 rpm, set washing temperature 30℃, washing time 45 minutes. Select washing mode: mixed wash.
[0112] Detergent: Commercially available product Blue Moon Silk and Wool Cleaner, 45 ml per kg of silk fabric.
[0113] Table 1 Performance test results
[0114] .
[0115] Table 2 Performance test results
[0116] .
[0117] From Tables 1 and 2, we can see that:
[0118] In comparative example 1, steps 5) to 9) are not performed, that is, the sand washing is similar to the prior art, and direct drying is adopted after sand washing. No anti-washing damage additive is used, and the creases are not flattened. It can be seen that the method of this comparative example has the most crease defects.
[0119] In Comparative Example 2, steps 1) and 3) were not performed, that is, wet setting was not performed before and after dyeing, and a small amount of crease defects were still present on the obtained fabric.
[0120] In step 6) of comparative example 3, the padding method was used, and the resulting fabric still had creases. In addition, due to the padding method, the fabric stayed in the solution for 2-4 seconds, which was too short, and the anti-washing damage agent could not fully penetrate into the silk fiber bundle, and the number of anti-washing damages was significantly lower than that of example 1.
[0121] In step 6) of comparative example 4, the solution is only water, and no anti-washing injury auxiliary agent is used, so it has no anti-washing injury effect.
[0122] In step 6) of comparative example 5, the concentration of the anti-washing damage auxiliary agent is greater than that of example 1, 8 g / L. The anti-washing damage times of the silk fabric finally obtained are not significantly improved compared with example 1, and the applicant finds that the fabric obtained in comparative example 3 feels slightly hard and not as good as example 1, and loses the glutinous and velvety feel obtained by sand washing finishing.
[0123] In step 4) of comparative example 6, no softener was added, and the silk surface of the obtained silk fabric had fine washing scratches produced during the preparation process.
[0124] The silk fabrics obtained in Examples 1 to 3 feel soft, velvety and smooth. When the silk fabrics are rotated against light, no creases are observed and the silk fabrics have a smooth and soft luster. While ensuring the hand feel, they have a long-term anti-washing injury effect.
[0125] Large-area silk products such as bedding require no defects within at least 3 meters, that is, ≤3 defects / 10 meters. Examples 1 to 3 of the present invention can meet this requirement and are suitable for making large-area high-end silk products such as bedding and curtains. Consumers usually use machine washing for large-area silk products such as bedding. Test 3 proves that the silk fabrics obtained in Examples 1 to 3 of the present invention can withstand more than 40 washes, can maintain gloss for a long time, and have no obvious signs of washing damage.
[0126] The above is only a preferred embodiment of the present invention, and does not limit the present invention in other forms. Any technician familiar with the profession may use the above disclosed technical content to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the technical solution of the present invention still belongs to the protection scope of the technical solution of the present invention.
Claims
1. A method for preventing silk fabric from being damaged by washing and sand washing, characterized in that: The following steps are involved: 1) Wet setting - 2) Dyeing - 3) Wet setting - 4) Sand washing - 5) Tentering - 6) Curling and soaking - 7) Water washing - 8) Acid washing - 9) Wet setting - 10) Air blowing - 11) Tentering; 4) Sand washing: Use industrial washing machine for washing, 25~35℃ water temperature, sand washing 3~4 times, 4~5 minutes / time, the sand washing solution used is water, soda ash 50~100g / L and softener 52~78g / L; 6) Rolling and impregnation: put the silk fabric on the roller dyeing machine, add the solution into the dyeing tank of the roller dyeing machine, the solution temperature is 25~35℃, and the roller runs for 30~60min at a speed of 40~60m / min to flatten the silk fabric and impregnate the solution; the solution is water and anti-washing damage auxiliary agent, and the concentration of the anti-washing damage auxiliary agent is 3~5g / L; Step 10) The specific operation of drying is: use hot air to beat and dry the silk fabric in a relaxed state, with the hot air temperature at 70-80°C and the time for 1-3 hours.
2. A method for preventing silk fabric from being damaged by washing and sand washing according to claim 1, characterized in that: The specific operation of step 1) wet setting is: setting the wet silk fabric after degumming at a setting temperature of 95-100°C; the specific operation of step 3) wet setting is: setting the wet silk fabric at a setting temperature of 100-105°C.
3. A method for preventing silk fabric from being damaged by washing and sand washing according to claim 1, characterized in that: Step 9) The specific operation of wet setting is: setting the wet silk fabric at a setting temperature of 100~110℃.
4. A method for preventing silk fabric from being damaged by washing and sand washing according to claim 1, characterized in that: The specific operation of the tentering in step 5) is: tentering by spraying steam at 100-110°C; the specific operation of the tentering in step 11) is: tentering by spraying steam at 110-120°C.
5. The method for preventing silk fabric from being damaged by washing and sand washing according to claim 1, characterized in that: The dye used in step 2) is a reactive dye.
6. A method for preventing silk fabric from being damaged by washing and sand washing according to claim 1, characterized in that: Step 6) The anti-washing injury aid is the anti-washing injury aid W-08.
7. A method for preventing silk fabric from being damaged by washing and sand washing according to claim 1, characterized in that: Step 4) The softener is a mixture of softener 3165 and finishing agent 6820 in a mass ratio of 10:
3.
8. The method for preventing silk fabric from being damaged by washing and sand washing according to claim 1, characterized in that: The specific operation of step 7) water washing is: 25~35°C water temperature, 2~3 times of water washing; the specific operation of step 8) acid washing is: 25~35°C water temperature, 1g / L acetic acid, 2~3 times of acid washing.