A kind of 2,5-furandicarboxylic acid polyester and preparation method thereof
Through negative pressure transesterification and multi-stage polymerization process, the problems of deep color and poor thermal stability of 2,5-furandicarboxylic acid-based polyester were solved, and polyester with excellent heat resistance and mechanical properties was prepared, simplifying the process and Reduces cost and is suitable for a variety of applications.
Patent Information
- Application Number
- CN202310125456.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-03
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-02-03
AI Technical Summary
In the prior art, 2,5-furandicarboxylic acid-based polyester has a darker color, low molecular weight, and poor thermal stability, which leads to problems such as yellowing of slices during the preparation process, and the conventional polymerization process is complex and costly.
It adopts a multi-stage reaction process of negative pressure transesterification, precondensation polymerization and final polycondensation, and polymerizes through gradient heating and negative pressure conditions. It uses acetate metal salts and antimony or germanium catalysts to control the reaction temperature and pressure to avoid decarboxylation reaction and Increase molecular weight.
The preparation of 2,5-furandicarboxylic acid-based polyester with good color, excellent heat resistance and mechanical properties has been achieved, simplifying the process and reducing production costs, and is suitable for applications such as food packaging and chemical fiber fabrics.
Smart Images

Figure CN116003762B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, and in particular to a 2,5-furandicarboxylic acid-based polyester and a preparation method thereof. Background Art
[0002] 2,5-Furandicarboxylic acid (FDCA) is a stable furan derivative. It has been selected by the U.S. Department of Energy as one of the 12 most promising bio-based platform compounds. It has a wide range of sources and can be obtained from biomass such as fruit shells and straw. The structure of FDCA is similar to that of terephthalic acid (PTA). Both have a cyclic conjugated system and two carboxyl groups. Since 2,5-Furandicarboxylic acid (FDCA) and terephthalic acid (PTA) are similar in structure and chemical properties, it is speculated that the polyester synthesized with FDCA as a dibasic acid is similar in structure and chemical properties to the corresponding polyester with PTA. This polyester synthesized by reacting FDCA as a dibasic acid with a diol or polyol is called 2,5-Furandicarboxylic acid-based polyester. Poly (ethylene 2,5-furandicarboxylate) (PEF) is produced by polymerization of bio-based monomers 2,5-furandicarboxylic acid / 2,5-furandicarboxylic acid dimethyl ester and ethylene glycol. It has a similar molecular structure to polyethylene terephthalate (PET), but has better heat resistance and barrier properties, so it has broad application prospects.
[0003] However, the furan-based polyesters currently prepared by FDCA generally have the problem of dark color. Due to the production technology problems of the monomer FDCA, its purity cannot meet the polymerization requirements; at the same time, the carboxyl group on the furan ring has poor thermal stability, and decarboxylation reaction will occur above 180°C, resulting in low polymer molecular weight and yellowing.
[0004] At present, a large number of patents have disclosed various synthesis methods of 2,5-furandicarboxylic acid polyesters. In all of them, 2,5-furandicarboxylic acid and its esters are directly polymerized with diols, but there is no description and comparison of the characteristics of the two monomers. Conventional polyester polymerization processes are generally used for reaction. After a large number of experimental demonstrations and literature research, it is concluded that there are significant differences in the processes for preparing furan-based polyesters from monomers 2,5-furandicarboxylic acid and 2,5-furandicarboxylic acid dimethyl ester (FDME) with diols, especially for the product purity and high-temperature decomposition of monomer 2,5-furandicarboxylic acid, which are difficult to solve in the short term. Therefore, polyesters prepared from monomers 2,5-furandicarboxylic acid and diols generally have problems such as yellowing of slices. Publication Nos. CN114057998A, CN108129644A, CN108659209A, and CN104144967A all use 2,5-furandicarboxylic acid or its diester as a reaction monomer and aliphatic diol for polymerization reaction, and the esterification / ester exchange temperature is generally higher than 170°C. CN108219121A discloses a bio-based high barrier polyester material and a synthesis method thereof, which is synthesized by esterification reaction, polycondensation reaction, and purification and refining of 2,5-furandicarboxylic acid and diol in three steps. Adding purification and refining after the conventional polymerization process can obtain slices with better color value to a certain extent, but the process is complicated and cumbersome, and the production cost is high.
[0005] In view of this, in view of the above shortcomings of the prior art, the present invention proposes 2,5-furandicarboxylic acid-based polyester and a preparation method thereof, which can realize the preparation of polyester chips with excellent heat resistance and mechanical properties as well as good chromaticity. Summary of the invention
[0006] (1) Technical issues to be solved
[0007] The purpose of the present invention is to provide 2,5-furandicarboxylic acid polyester and a preparation method thereof, so as to solve the technical problems of dark color, low molecular weight and poor thermal stability in the preparation of 2,5-furandicarboxylic acid polyester in the prior art.
[0008] (2) Technical solution
[0009] In order to solve the above problems, the present invention provides a method for preparing 2,5-furandicarboxylic acid polyester, and the specific scheme is as follows:
[0010] Add dimethyl 2,5-furandicarboxylate, diol, catalyst and stabilizer into a reaction kettle;
[0011] A protective gas is introduced into the reactor to expel the air, and the polymerization reaction is carried out by step-by-step temperature increase under stirring conditions;
[0012] The material is discharged and granulated to obtain 2,5-furandicarboxylic acid-based polyester.
[0013] Preferably, the polymerization reaction sequentially undergoes three reaction stages: negative pressure transesterification reaction, pre-polycondensation reaction and final polycondensation reaction;
[0014] The reaction temperature of the negative pressure transesterification reaction is 140°C to 160°C, the reaction time is 1.5h to 3h, and the reaction pressure is ≤-25kpa;
[0015] The reaction temperature of the pre-polycondensation reaction is 200°C to 230°C, the reaction pressure is ≤-0.1Mpa, and the reaction time is 0.5h to 1h;
[0016] The reaction temperature of the final polycondensation reaction is 230° C. to 250° C., the vacuum degree is ≤70 Pa, and the reaction time is 1 h to 3 h.
[0017] Preferably, the discharging is specifically carried out by introducing protective gas into the reaction kettle to normal pressure, standing for 3 minutes to 10 minutes, and introducing protective gas again for granulation to obtain 2,5-furandicarboxylic acid-based polyester.
[0018] Preferably, the viscosity of the product of the final polycondensation reaction at the time of discharge is 0.63 dL / g to 0.85 dL / g.
[0019] Preferably, the molar ratio of dimethyl 2,5-furandicarboxylate to diol is 1:1.8-2.5, the amount of the catalyst added is 0.01%-0.2% of the mass of dimethyl 2,5-furandicarboxylate, and the amount of the stabilizer added is 0.05%-0.5% of the mass of 2,5-furandicarboxylic acid / dimethyl ester.
[0020] Preferably, the diol is at least one of ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,3-cyclohexanediol, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, 2,5-tetrahydrofuran dimethanol, and 2,2,4,4-tetramethyl-1,3-cyclobutanediol.
[0021] Preferably, the catalyst is a composite system of metal acetate salts and antimony series, or a composite system of metal acetate salts and germanium series.
[0022] Preferably, the metal acetate is at least one of cadmium acetate, zinc acetate, calcium acetate, manganese acetate and cobalt acetate, and the metal acetate accounts for 30wt% to 70wt% of the total amount of the catalyst.
[0023] Preferably, the stabilizer is at least one of phosphoric acid, phosphorous acid, hypophosphorous acid, triphenyl phosphate, diphenyl phosphate, triphenyl phosphite, diphenyl phosphorus, ammonium phosphite, and diammonium phosphate.
[0024] Another aspect of the present invention provides 2,5-furandicarboxylic acid-based polyester prepared by the preparation method described in the above scheme.
[0025] (3) Beneficial effects
[0026] The above technical solution of the present invention has the following advantages:
[0027] Firstly, the present invention uses 2,5-furandicarboxylic acid dimethyl ester, diol, catalyst and stabilizer as raw materials to carry out polymerization reaction to prepare 2,5-furandicarboxylic acid-based polyester, and the polymerization process involves the steps of transesterification, pre-polycondensation and final polycondensation; wherein the transesterification stage adopts a negative pressure process, and the reaction temperature is below 160°C to avoid the decarboxylation reaction of 2,5-furandicarboxylic acid dimethyl ester, and at the same time, a relatively low reaction temperature can satisfy the transesterification reaction of 2,5-furandicarboxylic acid dimethyl ester; after the distillate reaches the theoretical value, the reaction temperature is increased in the pre-polycondensation process, and at the same time, the 2,5-furandicarboxylic acid-based esterification product is polycondensed under the action of negative pressure, and a large amount of diol is removed to generate oligomers; during the final polycondensation, the pressure in the kettle is gradually reduced, a large amount of oligomers are polycondensed to form macromolecular chains, the molecular weight of the polymer is gradually increased, and the melt viscosity is increased, and at this time, the rotation speed of the stirring motor is reduced to prevent the melt from climbing the rod, and at the same time, the exothermic effect in the polycondensation reaction process is suppressed to avoid overheating and decomposition of the polymer.
[0028] Secondly, the melting point of 2,5-furandicarboxylic acid dimethyl ester is about 117°C. When it reacts with diols, 2,5-furandicarboxylic acid dimethyl ester can melt at a relatively low temperature, increasing the reaction volume with diols, improving the transesterification reaction rate, and avoiding the thermal degradation of 2,5-furandicarboxylic acid dimethyl ester. At the same time, the negative pressure transesterification process in the present invention can reduce the reaction temperature to 160°C. In addition, the 2,5-furandicarboxylic acid-based polyester obtained by the preparation method of the present invention can be processed to prepare films, containers and chemical fiber fabrics for food packaging, and can be widely used in production, life and other related industries.
[0029] In summary, the 2,5-furandicarboxylic acid-based polyester prepared by the special process of negative pressure ester exchange + synergistic catalyst has excellent heat resistance, mechanical properties and chromaticity. At the same time, the preparation method is simple and efficient, the product quality is high, it can effectively meet the application needs, and has broad market prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is a physical picture of the polyethylene 2,5-furandicarboxylate slice prepared in Example 1 of the present invention.
[0031] Figure 2 This is a physical picture of the processed polyethylene 2,5-furandicarboxylate wafer prepared in Example 1 of the present invention.
[0032] Figure 3 This is a physical picture of the tensile test specimen of polyethylene 2,5-furandicarboxylate prepared in Example 1 of the present invention
[0033] Figure 4 It is a schematic diagram of the stress-strain curve of polyethylene 2,5-furandicarboxylate prepared in Example 1 of the present invention.
[0034] Figure 5 It is a schematic diagram of the DSC test curve of polyethylene 2,5-furandicarboxylate prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0035] In order to more clearly understand the above-mentioned objectives, features and advantages of the present invention, the scheme of the present invention will be further described below. It should be noted that the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.
[0036] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein; it is obvious that the embodiments in the specification are only part of the embodiments of the present invention, rather than all of the embodiments.
[0037] The following detailed description of the embodiments of the present invention is provided in conjunction with the accompanying drawings and examples. The following detailed description of the embodiments and the accompanying drawings are used to illustrate the principles of the present invention, but cannot be used to limit the scope of the present invention, that is, the present invention is not limited to the described embodiments.
[0038] A method for preparing 2,5-furandicarboxylic acid-based polyester, the specific scheme is as follows:
[0039] Dimethyl 2,5-furandicarboxylate, diol, catalyst and stabilizer are added into a reactor, protective gas is introduced to discharge the air in the reactor, and then a polymerization reaction is carried out under gradient heating and stirring conditions. After the polymerization reaction is completed, the material is discharged and granulated to obtain 2,5-furandicarboxylic acid-based polyester chips.
[0040] It should be noted that the protective gas introduced into the reactor for evacuation is an inert gas or nitrogen. Considering the comprehensive production cost, the present invention preferably uses nitrogen as the protective gas. Preferably, when evacuating, high-purity nitrogen is introduced into the reactor until the gauge pressure reaches 0.08Mpa to 0.1Mpa, and then the pressure is slowly released, which is repeated 1 to 3 times.
[0041] The above-mentioned polymerization reaction is completed in three stages: negative pressure ester exchange reaction, pre-polycondensation reaction and final polycondensation reaction. Gradient temperature increase means that different reaction temperatures are set in the three stages of the polymerization reaction, and the reaction temperature is gradually increased from the first stage to the third stage.
[0042] The first stage is a negative pressure transesterification reaction, wherein the reaction temperature of the negative pressure transesterification reaction is 140°C to 160°C, the reaction time is 1.5h to 3h, and the reaction pressure is ≤-25kpa;
[0043] The second stage is a pre-polycondensation reaction, wherein the reaction temperature of the pre-polycondensation reaction is 200°C to 230°C, the reaction pressure is ≤-0.1Mpa, and the reaction time is 0.5h to 1h;
[0044] The third stage is the final polycondensation reaction, wherein the reaction temperature of the final polycondensation reaction is 230° C. to 250° C., the vacuum degree is ≤70 Pa, and the reaction time is 1 h to 3 h.
[0045] It should be noted that in order to ensure the completeness of the negative pressure transesterification reaction in the first stage, the temperature should be raised to enter the second stage pre-polycondensation reaction when the distillate reaches more than 95% of the theoretical value.
[0046] It should be noted that in the negative pressure transesterification reaction stage, dimethyl 2,5-furandicarboxylate undergoes an esterification reaction with a diol to remove methanol, and the methanol is recovered and measured; the pressure in the kettle is ensured to be ≤-25kpa through intermittent operation of the vacuum pump and adjustment of the esterification valve.
[0047] When the melt viscosity in the final polycondensation reaction stage reaches the required level, stirring is stopped, nitrogen is continuously introduced into the reactor to normal pressure, the reactor is allowed to stand for 3 to 10 minutes, and nitrogen is introduced again to discharge the product to obtain an antibacterial, heat-resistant, high-barrier copolyester containing furan rings. Preferably, the melt viscosity is 0.63 dL / g to 0.85 dL / g, and the chip color preferably has a b value of ≤5.
[0048] Preferably, the gradient temperature rise adopts heat medium heating, and the stirring device is a magnetic stirring motor. Preferably, the speed of the stirring motor is 80r / min to 120r / min in the negative pressure ester exchange and pre-polycondensation stages, and 40r / min to 60r / min in the final polycondensation stage.
[0049] Preferably, the molar ratio of dimethyl 2,5-furandicarboxylate to diol is 1:1.8-2.5, the amount of the catalyst added is 0.01%-0.2% of the mass of dimethyl 2,5-furandicarboxylate, and the amount of the stabilizer added is 0.05%-0.5% of the mass of 2,5-furandicarboxylic acid / dimethyl ester.
[0050] Preferably, the diol is at least one of ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,3-cyclohexanediol, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, 2,5-tetrahydrofuran dimethanol, and 2,2,4,4-tetramethyl-1,3-cyclobutanediol.
[0051] Preferably, the catalyst is a composite system of metal acetate salts and antimony series, or a composite system of metal acetate salts and germanium series.
[0052] More preferably, the metal acetate is at least one of cadmium acetate, zinc acetate, calcium acetate, manganese acetate, and cobalt acetate, and the metal acetate accounts for 30wt% to 70wt% of the total amount of the catalyst. The antimony-based catalyst is preferably antimony oxide or ethylene glycol antimony, and the germanium-based catalyst is preferably germanium oxide.
[0053] Preferably, the stabilizer is at least one of phosphoric acid, phosphorous acid, hypophosphorous acid, triphenyl phosphate, diphenyl phosphate, triphenyl phosphite, diphenyl phosphorus, ammonium phosphite, and diammonium phosphate.
[0054] Example 1
[0055] 700g of dimethyl 2,5-furandicarboxylate, 472g of ethylene glycol, 0.6g of zinc acetate, 0.4g of antimony glycol and 1.0g of triphenyl phosphite are added to a polymerization kettle; after the feeding is completed, the kettle is sealed and nitrogen is passed to replace the air in the kettle, and the process is repeated 1-3 times; the circulating heat medium is turned on to start heating and stirring is started at the same time; the ester exchange reaction is carried out at a temperature of 150°C, a time of 2h, and a pressure in the kettle of ≤-25kpa; when the distillate reaches 95% of the theoretical value, the ester exchange reaction is completed; then a preliminary polycondensation reaction is carried out at a reaction temperature of 230°C, a reaction time of 1h, and a pressure in the kettle of ≤-0.1Mpa, and finally a final polycondensation reaction is carried out at a reaction temperature of 240°C; a time of 3h, and a vacuum degree of ≤70Pa; when the melt reaches the viscosity requirement, stirring is stopped, nitrogen is passed to normal pressure, the mixture is allowed to stand for 5min, and nitrogen is passed again to discharge and granulate the mixture to obtain polyethylene 2,5-furandicarboxylate.
[0056] Example 2
[0057] 700g of dimethyl 2,5-furandicarboxylate, 578g of 1,3-propylene glycol, 0.6g of zinc acetate, 0.4g of antimony glycol and 1.0g of triphenyl phosphite are added to a polymerization kettle; after the feeding is completed, the kettle is sealed and nitrogen is passed to replace the air in the kettle, and the process is repeated 1-3 times; the circulating heat medium is turned on to start heating and stirring is started at the same time; the ester exchange reaction is carried out at a temperature of 150°C, a time of 2h, and a pressure in the kettle of ≤-25kpa; when the distillate reaches 95% of the theoretical value, the ester exchange reaction is completed; then a preliminary polycondensation reaction is carried out at a reaction temperature of 230°C, a reaction time of 1h, and a pressure in the kettle of ≤-0.1Mpa, and finally a final polycondensation reaction is carried out at a reaction temperature of 240°C; a time of 3h, and a vacuum degree of ≤70Pa; after the melt reaches the viscosity requirement, stirring is stopped, nitrogen is passed to normal pressure, the mixture is allowed to stand for 5min, and nitrogen is passed again to discharge and granulate to obtain poly(propylene 2,5-furandicarboxylate).
[0058] Example 3
[0059] 700g of dimethyl 2,5-furandicarboxylate, 378g of ethylene glycol, 219g of 1,4-cyclohexanedimethanol, 0.6g zinc acetate, 0.4g antimony glycol and 1.0g triphenyl phosphite are added to a polymerization kettle; after the feeding is completed, the kettle is sealed and nitrogen is passed to replace the air in the kettle, and the process is repeated 1-3 times; the circulating heat medium is turned on to start heating and stirring is started at the same time; the ester exchange reaction is carried out at a temperature of 150°C, a time of 2h, and a pressure in the kettle of ≤-25kpa; when the distillate reaches 95% of the theoretical value, the ester exchange reaction is completed; then a pre-polycondensation reaction is carried out at a reaction temperature of 230°C, a reaction time of 1h, and a pressure in the kettle of ≤-0.1Mpa, and finally a final polycondensation is carried out at a reaction temperature of 240°C; the time is 3h, and the vacuum degree is ≤70Pa; when the melt reaches the viscosity requirement, stirring is stopped, nitrogen is passed to normal pressure, the mixture is allowed to stand for 5min, and nitrogen is passed again to discharge and granulate the mixture to obtain polyethylene 2,5-furandicarboxylic acid glycol copolyester.
[0060] Example 4
[0061] 700g of dimethyl 2,5-furandicarboxylate, 472g of ethylene glycol, 0.4g of zinc acetate, 0.6g of antimony glycol and 1.0g of triphenyl phosphite are added to a polymerization kettle; after the feeding is completed, the kettle is sealed and nitrogen is passed to replace the air in the kettle, and the process is repeated 1-3 times; the circulating heat medium is turned on to start heating and stirring is started at the same time; the ester exchange reaction is carried out at a temperature of 150°C, a time of 2h, and a pressure in the kettle of ≤-25kpa; when the distillate reaches 95% of the theoretical value, the ester exchange reaction is completed; then a preliminary polycondensation reaction is carried out at a reaction temperature of 230°C, a reaction time of 1h, and a pressure in the kettle of ≤-0.1Mpa, and finally a final polycondensation reaction is carried out at a reaction temperature of 240°C; a time of 3h, and a vacuum degree of ≤70Pa; when the melt reaches the viscosity requirement, stirring is stopped, nitrogen is passed to normal pressure, the mixture is allowed to stand for 5min, and nitrogen is passed again to discharge and granulate the mixture to obtain polyethylene 2,5-furandicarboxylate.
[0062] Example 5
[0063] 700g of dimethyl 2,5-furandicarboxylate, 472g of ethylene glycol, 0.7g of zinc acetate, 0.3g of antimony glycol and 1.0g of triphenyl phosphite are added to a polymerization kettle; after the feeding is completed, the kettle is sealed and nitrogen is passed to replace the air in the kettle, and the process is repeated 1-3 times; the circulating heat medium is turned on to start heating and stirring is started at the same time; the ester exchange reaction is carried out at a temperature of 150°C, a time of 2h, and a pressure in the kettle of ≤-25kpa; when the distillate reaches 95% of the theoretical value, the ester exchange reaction is completed; then a preliminary polycondensation reaction is carried out at a reaction temperature of 230°C, a reaction time of 1h, and a pressure in the kettle of ≤-0.1Mpa, and finally a final polycondensation reaction is carried out at a reaction temperature of 240°C; a time of 3h, and a vacuum degree of ≤70Pa; when the melt reaches the viscosity requirement, stirring is stopped, nitrogen is passed to normal pressure, the mixture is allowed to stand for 5min, and nitrogen is passed again to discharge and granulate the mixture to obtain polyethylene 2,5-furandicarboxylate.
[0064] Example 6
[0065] 700g of dimethyl 2,5-furandicarboxylate, 472g of ethylene glycol, 0.6g of calcium acetate, 0.4g of antimony glycol and 1.0g of triphenyl phosphite are added to a polymerization kettle; after the feeding is completed, the kettle is sealed and nitrogen is passed to replace the air in the kettle, and the process is repeated 1-3 times; the circulating heat medium is turned on to start heating and stirring is started at the same time; the ester exchange reaction is carried out at a temperature of 150°C, a time of 2h, and a pressure in the kettle of ≤-25kpa; when the distillate reaches 95% of the theoretical value, the ester exchange reaction is completed; then a preliminary polycondensation reaction is carried out at a reaction temperature of 230°C, a reaction time of 1h, and a pressure in the kettle of ≤-0.1Mpa, and finally a final polycondensation reaction is carried out at a reaction temperature of 240°C; a time of 3h, and a vacuum degree of ≤70Pa; when the melt reaches the viscosity requirement, stirring is stopped, nitrogen is passed to normal pressure, the mixture is allowed to stand for 5min, and nitrogen is passed again to discharge and granulate the mixture to obtain polyethylene 2,5-furandicarboxylate.
[0066] Example 7
[0067] 700g of dimethyl 2,5-furandicarboxylate, 472g of ethylene glycol, 0.6g of zinc acetate, 0.4g of germanium oxide and 1.0g of triphenyl phosphite are added to a polymerization kettle; after the feeding is completed, the kettle is sealed and nitrogen is passed to replace the air in the kettle, and the process is repeated 1-3 times; the circulating heat medium is turned on to start heating and stirring is started at the same time; the ester exchange reaction is carried out at a temperature of 150°C, a time of 2h, and a pressure in the kettle of ≤-25kpa; when the distillate reaches 95% of the theoretical value, the ester exchange reaction is completed; then a preliminary polycondensation reaction is carried out at a reaction temperature of 230°C, a reaction time of 1h, and a pressure in the kettle of ≤-0.1Mpa, and finally a final polycondensation reaction is carried out at a reaction temperature of 240°C; a time of 3h, and a vacuum degree of ≤70Pa; when the melt reaches the viscosity requirement, stirring is stopped, nitrogen is passed to normal pressure, the mixture is allowed to stand for 5min, and nitrogen is passed again to discharge and granulate the mixture to obtain polyethylene 2,5-furandicarboxylate.
[0068] Example 8
[0069] 700g of dimethyl 2,5-furandicarboxylate, 472g of ethylene glycol, 0.6g of zinc acetate, 0.4g of antimony glycol and 1.0g of phosphoric acid are added to a polymerization kettle; after the feeding is completed, the kettle is sealed and nitrogen is passed to replace the air in the kettle, and the process is repeated 1-3 times; the circulating heat medium is turned on to start heating and stirring is started at the same time; the ester exchange reaction is carried out at a temperature of 150°C, a time of 2h, and a pressure in the kettle of ≤-25kpa; when the distillate reaches 95% of the theoretical value, the ester exchange reaction is completed; then a preliminary polycondensation reaction is carried out at a reaction temperature of 230°C, a reaction time of 1h, and a pressure in the kettle of ≤-0.1Mpa, and finally a final polycondensation reaction is carried out at a reaction temperature of 240°C; a time of 3h, and a vacuum degree of ≤70Pa; when the melt reaches the viscosity requirement, stirring is stopped, nitrogen is passed to normal pressure, the mixture is allowed to stand for 5min, and nitrogen is passed again to discharge and granulate the mixture to obtain polyethylene 2,5-furandicarboxylate.
[0070] Example 9
[0071] 700g of dimethyl 2,5-furandicarboxylate, 472g of ethylene glycol, 0.6g of zinc acetate, 0.4g of antimony glycol and 1.0g of triphenyl phosphite are added to a polymerization kettle; after the feeding is completed, the kettle is sealed and nitrogen is passed to replace the air in the kettle, and the process is repeated 1-3 times; the circulating heat medium is turned on to start heating and stirring is started at the same time; the ester exchange reaction is carried out at a temperature of 160°C, a time of 1.5h, and a pressure in the kettle of ≤-25kpa; when the distillate reaches 95% of the theoretical value, the ester exchange reaction is completed; then a preliminary polycondensation reaction is carried out at a reaction temperature of 230°C, a reaction time of 1h, and a pressure in the kettle of ≤-0.1Mpa, and finally a final polycondensation reaction is carried out at a reaction temperature of 240°C; a time of 3h, and a vacuum degree of ≤70Pa; when the melt reaches the viscosity requirement, stirring is stopped, nitrogen is passed to normal pressure, the mixture is allowed to stand for 5min, and nitrogen is passed again to discharge and granulate the mixture to obtain polyethylene 2,5-furandicarboxylate.
[0072] Example 10
[0073] 700g of dimethyl 2,5-furandicarboxylate, 472g of ethylene glycol, 0.6g of zinc acetate, 0.4g of antimony glycol and 1.0g of triphenyl phosphite are added to a polymerization kettle; after the feeding is completed, the kettle is sealed and nitrogen is passed to replace the air in the kettle, and the process is repeated 1-3 times; the circulating heat medium is turned on to start heating and stirring is started at the same time; the ester exchange reaction is carried out at a temperature of 140°C, a time of 3h, and a pressure in the kettle of ≤-25kpa; when the distillate reaches 95% of the theoretical value, the ester exchange reaction is completed; then a preliminary polycondensation reaction is carried out at a reaction temperature of 230°C, a reaction time of 1h, and a pressure in the kettle of ≤-0.1Mpa, and finally a final polycondensation reaction is carried out at a reaction temperature of 240°C; a time of 3h, and a vacuum degree of ≤70Pa; when the melt reaches the viscosity requirement, stirring is stopped, nitrogen is passed to normal pressure, the mixture is allowed to stand for 5min, and nitrogen is passed again to discharge and granulate the mixture to obtain polyethylene 2,5-furandicarboxylate.
[0074] Comparative Example 1
[0075] 700g 2,5-furandicarboxylic acid, 556g ethylene glycol, 0.6g zinc acetate, 0.4g antimony glycol and 1.0g triphenyl phosphite are added to a polymerization kettle; after the feeding is completed, the kettle is sealed and nitrogen is passed to replace the air in the kettle, and the process is repeated 1-3 times, and then nitrogen is filled as a protective gas at a pressure of 30kpa; the circulating heat medium is turned on to start heating, and stirring is started at the same time, and the esterification reaction is performed at a temperature of 180°C and a time of 2.5h; when the distillate reaches 95% of the theoretical value, the esterification reaction is completed; then a preliminary polycondensation reaction is performed at a reaction temperature of 230°C, a reaction time of 1h, and a pressure in the kettle of ≤-0.1Mpa, and finally a final polycondensation reaction is performed at a reaction temperature of 240°C; the time is 4h, and the vacuum degree is ≤70Pa; after the melt reaches the viscosity requirement, stirring is stopped, nitrogen is passed to normal pressure, and the mixture is allowed to stand for 5min, and nitrogen is passed again to discharge and granulate to obtain polyethylene 2,5-furandicarboxylate.
[0076] Comparative Example 2
[0077] 700g of dimethyl 2,5-furandicarboxylate, 472g of ethylene glycol, 0.7g of tetrabutyl titanate and 1.0g of triphenyl phosphite are added to a polymerization kettle; after the feeding is completed, the kettle is sealed and nitrogen is passed through to replace the air in the kettle, and the process is repeated 1-3 times, and then nitrogen is filled in as a protective gas at a pressure of 30kpa; the circulating heat medium is turned on to start heating, and stirring is started at the same time, and the esterification reaction is carried out at a temperature of 180°C and a time of 2.5h; when the distillate reaches 95% of the theoretical value, the esterification reaction is completed; then a preliminary polycondensation reaction is carried out at a reaction temperature of 230°C, a reaction time of 1h, and a pressure in the kettle of ≤-0.1Mpa, and finally a final polycondensation is carried out at a reaction temperature of 240°C; a time of 4h, and a vacuum degree of ≤70Pa; after the melt reaches the viscosity requirement, stirring is stopped, nitrogen is passed through to normal pressure, and the mixture is allowed to stand for 5min, and nitrogen is passed through again to discharge and granulate to obtain polyethylene 2,5-furandicarboxylate.
[0078] Comparative Example 3
[0079] 700g of dimethyl 2,5-furandicarboxylate, 472g of ethylene glycol, 0.6g of zinc acetate, 0.4g of antimony glycol and 1.0g of triphenyl phosphite are added to a polymerization kettle; after the feeding is completed, the kettle is sealed and nitrogen is passed through to replace the air in the kettle, and the process is repeated 1-3 times, and then nitrogen is filled in as a protective gas at a pressure of 30kpa; the circulating heat medium is turned on to start heating, and stirring is started at the same time; ester exchange reaction is carried out at a temperature of 180°C, a time of 2.5h, and a positive pressure in the kettle; when the distillate reaches 95% of the theoretical value, the ester exchange reaction is completed; then a preliminary polycondensation reaction is carried out at a reaction temperature of 230°C, a reaction time of 1h, and a pressure in the kettle of ≤-0.1Mpa, and finally a final polycondensation is carried out at a reaction temperature of 240°C; a time of 3h, and a vacuum degree of ≤70Pa; when the melt reaches the viscosity requirement, stirring is stopped, nitrogen is passed through to normal pressure, and the mixture is allowed to stand for 5min, and nitrogen is passed through again to discharge and granulate to obtain polyethylene 2,5-furandicarboxylate.
[0080] The 2,5-furandicarboxylic acid-based polyester prepared in the above examples and comparative examples was tested for performance. The intrinsic viscosity test standard refers to GB / T 14190 2017; the tensile mechanical property test standard refers to GB / T 1040.1-2018; the glass transition temperature is measured by differential scanning calorimetry (DSC), and the test conditions are: nitrogen atmosphere, gas flow rate 20ml / min; the sample temperature is increased from 30°C to 250°C, and the heating rate is 10°C / min. The test results are shown in Table 1.
[0081] Table 1 Performance test results of 2,5-furandicarboxylic acid-based polyesters prepared in Examples and Comparative Examples
[0082]
[0083] In Example 1 and Comparative Example 1, polyethylene 2,5-furandicarboxylate (PEF) was prepared from dimethyl 2,5-furandicarboxylate (FDME) and 2,5-furandicarboxylic acid (FDCA), respectively. From the test results, it can be seen that the PEF prepared in Example 1 has a higher intrinsic viscosity and a greater tensile strength; at the same time, the slice appearance color is lighter, and the chromaticity b value is much lower than that of the PEF prepared in Comparative Example 1. The test results show that the decarboxylation reaction of 2,5-furandicarboxylic acid is avoided by using FDME as a monomer to participate in the polymerization reaction, thereby ensuring the physical properties of PEF to a large extent. Figure 1 This is a physical picture of the polyethylene 2,5-furandicarboxylate slice prepared in Example 1. Figure 2 This is a physical picture of the polyethylene 2,5-furandicarboxylate processed disc prepared in Example 1. Figure 3 This is a physical picture of the tensile test specimen of polyethylene 2,5-furandicarboxylate prepared in Example 1. Figure 4 Schematic diagram of the stress-strain curve of polyethylene 2,5-furandicarboxylate prepared in Example 1, Figure 5 This is a schematic diagram of the DSC test curve of polyethylene 2,5-furandicarboxylate prepared in Example 1.
[0084] In Comparative Example 2, tetrabutyl titanate was used as the catalyst, and the b value of the PEF slice was 8.55. In Comparative Example 3, the b value of the PEF slice was 5.87 through the conventional high-pressure transesterification process, while the b value (2.23) of the PEF slice in Example 1 was significantly lower than that of Comparative Example 1 and Comparative Example 2. It can be seen that different catalysts and transesterification processes have a greater impact on the chromaticity of PEF. The synergistic catalyst and negative pressure transesterification process provided by the present invention can greatly improve the physical properties and chromaticity of PEF.
[0085] In Examples 2 to 3, poly (propylene 2,5-furandicarboxylate) (PTF) and poly (ethylene 2,5-furandicarboxylate-cyclohexanedimethanol) (PEFM) were prepared by reacting FDME with bio-based 1,3-propylene glycol and ethylene glycol plus 1,4-cyclohexanedimethanol, respectively. Both polyester chips have good appearance, high elongation at break, and excellent comprehensive performance.
[0086] In Examples 4 to 7, the ratio of the synergistic catalyst was adjusted, and the overall effect was weaker than the specific formula in Example 1.
[0087] In Example 8, when the stabilizer is phosphoric acid, its effect on improving the chromaticity of the slices is limited.
[0088] In Examples 9 to 10, the temperature of the negative pressure ester exchange was adjusted. The results showed that when the temperature was too high, the chromaticity b value of the slices increased. When the temperature was too low, the ester exchange rate was slow, which was not conducive to the growth of the PEF molecular weight. Therefore, the ester exchange temperature had a certain influence on the chromaticity and intrinsic viscosity of the slices.
[0089] It can be seen from the above examples that the 2,5-furandicarboxylic acid-based polyester prepared by FDME via negative pressure transesterification process with a synergistic catalyst has good comprehensive physical properties, a chromaticity b value of <5, and no obvious yellowing phenomenon.
[0090] It should be clear that the present invention is not limited to the specific steps and structures described above. In addition, for the sake of brevity, detailed descriptions of known methods and technologies are omitted here.
[0091] The above is only an embodiment of the present application and is not limited to the present application. For those skilled in the art, the present application may have various changes and variations without departing from the scope of the present invention. Any modification, equivalent substitution, improvement, etc. made within the spirit and principle of the present application should be included in the scope of the claims of the present application.
Claims
1. A method for preparing 2,5-furandicarboxylic acid polyester, characterized in that: Adding dimethyl 2,5-furandicarboxylate, diol, catalyst and stabilizer into a reaction kettle; introducing protective gas into the reaction kettle to discharge air, and performing polymerization reaction by step-by-step temperature increase under stirring conditions; discharging and granulating to obtain 2,5-furandicarboxylic acid-based polyester; The polymerization reaction sequentially undergoes three reaction stages: negative pressure transesterification reaction, pre-polycondensation reaction and final polycondensation reaction; The reaction temperature of the negative pressure transesterification reaction is 140°C to 160°C, the reaction time is 1.5h to 3h, and the reaction pressure is ≤-25kpa; The reaction temperature of the pre-polycondensation reaction is 200°C to 230°C, the reaction pressure is ≤-0.1Mpa, and the reaction time is 0.5h to 1h; The reaction temperature of the final polycondensation reaction is 230°C to 250°C, the vacuum degree is ≤70Pa, and the reaction time is 1h to 3h; The catalyst is a composite system of acetate metal salts and antimony.
2. The method for preparing 2,5-furandicarboxylic acid-based polyester according to claim 1, characterized in that: The discharging is specifically carried out by introducing protective gas into the reaction kettle to normal pressure, standing for 3 minutes to 10 minutes, and introducing protective gas again for granulation to obtain 2,5-furandicarboxylic acid-based polyester.
3. The preparation method according to claim 1, characterized in that: The viscosity of the product of the final polycondensation reaction is 0.63 dL / g to 0.85 dL / g.
4. The method for preparing 2,5-furandicarboxylic acid-based polyester according to claim 1, characterized in that: The molar ratio of dimethyl 2,5-furandicarboxylate to diol is 1:1.8-2.5, the added amount of the catalyst is 0.01%-0.2% of the mass of dimethyl 2,5-furandicarboxylate, and the added amount of the stabilizer is 0.05%-0.5% of the mass of dimethyl 2,5-furandicarboxylate.
5. The method for preparing 2,5-furandicarboxylic acid-based polyester according to claim 1, characterized in that: The diol is at least one of ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,3-cyclohexanediol, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, 2,5-tetrahydrofuran dimethanol, and 2,2,4,4-tetramethyl-1,3-cyclobutanediol.
6. The method for preparing 2,5-furandicarboxylic acid-based polyester according to claim 1, characterized in that: The metal acetate salt is at least one of cadmium acetate, zinc acetate, calcium acetate, manganese acetate, and cobalt acetate, and the metal acetate salt accounts for 30wt% to 70wt% of the total amount of the catalyst.
7. The method for preparing 2,5-furandicarboxylic acid-based polyester according to claim 1, characterized in that: The stabilizer is at least one of phosphoric acid, phosphorous acid, hypophosphorous acid, triphenyl phosphate, diphenyl phosphate, triphenyl phosphite, diphenyl phosphorus, ammonium phosphite, and diammonium phosphate.
8. A 2,5-furandicarboxylic acid-based polyester, characterized in that: The invention is prepared by the preparation method according to any one of claims 1 to 7.
Citation Information
Patent Citations
Process for the production of poly (ethylene 2,5- furandicarboxylate) from 2,5-furandicarboxylic acid and use thereof, polyester compound and blends thereof
CN104144967A
Furan dicarboxylic acid copolyester and preparation method and application thereof
CN108129644A
Bio-based high-barrier-property polyester material and synthesis method thereof
CN108219121A
2,5-Furandicarboxylic acid copolyester and preparation method and application thereof
CN108659209A
2,5-furandicarboxylic acid copolyester and preparation method thereof
CN114057998A