Preparation method of sol-gel film opening agent
Through the surface modification technology of sol-gel method and silane coupling agent, the problem of dispersion and transparency of opening agents in polyethylene terephthalate plastic films has been solved, and efficient film processing performance has been achieved.
Patent Information
- Application Number
- CN202211488469.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-25
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-11-25
AI Technical Summary
The existing technology feedbacks a heavy packing density in polyethylene terephthalate plastic film, and there is a gap between the physical and chemical indicators and application performance of Grace E300, and the dispersion performance and transparency of the silica opening agent are insufficient.
The silica film opening agent is prepared by the sol-gel method, and the silica gel is formed by high-pressure convection of high-purity water glass and sulfuric acid. It is combined with the surface modification of silane coupling agents A and B, and is washed and dispersed to ensure the uniformity and uniformity of the particles. stability.
It achieves good transparency and processing performance in polyethylene terephthalate plastic film, improves the dispersion and transparency of the opening agent, and improves the physical and chemical indicators and application performance of the film.
Smart Images

Figure BDA0003963771590000051 
Figure BDA0003963771590000061 
Figure BDA0003963771590000062
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer material processing, and in particular relates to a method for preparing a film opening agent using a sol-gel method. Background Art
[0002] In production and life, during the production and storage of plastics, the film layers are prone to adhesion due to heat pressure or material pressure. The adhesion between the films will affect the unwinding speed of the plastics, such as during winding, slitting, and packaging. In severe cases, the plastics cannot be unfolded and used. The main reasons for film adhesion are: 1. After the film is closed, a vacuum closed state is formed between the films, which is not easy to separate; 2. After the film is formed, there are a large number of exposed molecular chains on its surface. After the two films are closed, the macromolecular chains are entangled and adhered to each other, making it impossible to open. The adhesion of plastic films brings difficulties to the application of automated packaging. In order to solve this problem, an opening agent is usually added during the plastic production process to improve its opening.
[0003] The earliest anti-blocking agents used were inorganic talcum powder, diatomaceous earth, etc. Diatomaceous earth and talcum powder were abandoned mainly because of their low pore volume, poor anti-blocking properties and poor transparency of the produced films. In the middle stage, they developed into organic oleic acid phthalamide, erucic acid phthalamide EBS derivatives, etc. The disadvantage is that organic anti-blocking agents have a large amount of precipitates on the surface of the film, which affects the printability, heat sealing and color of the film, and thus affects the use of the film. Silicon dioxide has high chemical purity, is non-toxic, harmless, and pollution-free. Its refractive index is close to that of plastic materials such as PE, PP, PET, and PA, and has little effect on optical properties. It is a high-quality anti-blocking agent that is widely used in the plastic industry and is currently widely used in various plastic film fields.
[0004] Chinese patent CN109705402A discloses a method for preparing an aerogel film opening agent, wherein sulfuric acid is added to form gel and glue, the temperature is raised to 70-90°C, sulfuric acid and water glass solution are added at the same time to maintain the pH value of 8-10, and after the co-flow is completed, the temperature is adjusted to 85-95°C, and then a silane coupling agent is added, and the aging is performed for 2-4 hours, and the pH value is adjusted to 2-4, and then the aging is performed, and then the 1-3% dilute sulfuric acid is used for washing, and then the filter cake is washed with ammonium salt solution, and then washed with water, and finally dispersed by a disperser and an emulsifier, spray dried, and crushed to obtain a particle size of 3.3-3.5um. The product has been successfully used in a polypropylene plastic film system, but the feedback in the polyethylene terephthalate plastic film is that the bulk density is heavy, and there is a gap with the physical and chemical indicators and application performance of Grace E300. Chinese patent CN110229380A discloses a method for preparing an efficient and highly transparent silicon dioxide plastic film opening agent, which comprises the following steps: heating the bottom water, adding ammonium bicarbonate and water glass solution to obtain a first reaction liquid; reacting and flowing to a second reaction liquid with a pH value of 3.0 to 5.0, and then aging for 30 minutes to obtain a reaction slurry; washing the reaction slurry with water, grinding, atomizing and drying, and crushing to obtain an efficient and highly transparent silicon dioxide plastic film opening agent. The silicon dioxide synthesized by the method has not been surface treated, and the affinity of the silicon dioxide particles to the organic polymer is greatly reduced, which affects the opening performance and dispersion performance of the opening agent. Summary of the invention
[0005] In view of the problems existing in the prior art, the present invention provides a method for preparing a film opening agent by a sol-gel method. The film opening agent particles prepared by the present invention are uniform and easy to disperse, and have good transparency and processing performance in the production of polyethylene terephthalate plastic film.
[0006] The primary purpose of the present invention is to provide a method for preparing a sol-gel film opening agent.
[0007] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0008] A method for preparing a sol-gel film opening agent comprises the following steps:
[0009] S1, forming silica sol by pressurized convection of water glass solution and sulfuric acid;
[0010] S2, heating the silica sol obtained in step S1, adjusting the pH to be alkaline, then adding silane coupling agent A and silane coupling agent B to modify the surface of silica, and after aging, adjusting the pH to be acidic, and then aging to form silica gel;
[0011] S3, washing the silica gel obtained in step S2, and dispersing the silica gel uniformly after washing;
[0012] S4, drying the slurry dispersed in step S3, and then crushing it to obtain;
[0013] In step S2, the silane coupling agent A is one of KH520 (γ-aminopropylmethyldiethoxysilane), KH530 (γ-aminopropylmethyldimethoxysilane), KH540 (γ-aminopropyltrimethoxysilane), KH550 (γ-aminopropyltriethoxysilane), KH560 (γ-glycidyloxypropyl), and KH570 (γ-(methacryloyloxy)propyltrimethoxysilane), and the silane coupling agent B is one of KH580 (3-mercaptopropyltrimethoxysilane) and KH590 (3-mercaptopropyltriethoxysilane).
[0014] The pressurized convection method of the present invention is to equip the water glass and sulfuric acid flow pipes with a booster pump to increase the flow rate when the prepared water glass and sulfuric acid solution are injected into the reaction container at the same time. The pressurized convection accelerates the rapid formation of silica primary particles, thereby enabling the rapid formation of the silica network structure. The richness of the silica network structure also increases, thereby improving the porosity of the silica.
[0015] Preferably, the silicon dioxide modulus of the water glass solution in step S1 is 3.20-3.40, the concentration is 10wt%-20wt%, and the concentration of sulfuric acid is 30wt%-50wt%.
[0016] Preferably, in the water glass solution in step S1, the Fe content is ≤15ppm, the Al content is ≤1ppm, the Ca content is ≤1ppm, the Mg content is ≤1ppm, and the solubility of solid water glass is ≥99.5%.
[0017] Preferably, after the pressurization in step S1, the flow pipe pressure of the water glass and sulfuric acid is maintained at 0.5Mpa to 1Mpa, the flow rate of the water glass solution is 180L / h to 230L / h, and the flow rate of the sulfuric acid is 30L / h to 50L / h.
[0018] Preferably, the total amount of the silane coupling agent added in step S2 is 0.50wt% to 0.80wt% on a dry basis, wherein the mass ratio of silane coupling agent A to silane coupling agent B is 4:1.
[0019] Preferably, in step S2, the pH is adjusted to be alkaline to a value of 8 to 10, and the pH is adjusted to be acidic to a value of 2 to 4.
[0020] Preferably, the washing in step S3 refers to washing with pure water, sulfuric acid solution, ammonium salt aqueous solution and pure water in the washing order with time intervals of 1:5:3:1 respectively, until the conductivity of the silica gel is less than 50 us / cm.
[0021] More preferably, the conductivity of the pure water is lower than 5 us / cm, the temperature is 50°C to 80°C, the concentration of the sulfuric acid solution is 30% to 60% solution, the ammonium salt is one of ammonium sulfate, ammonium bisulfate, ammonium carbonate and ammonium bicarbonate, and the weight ratio of ammonium salt to water in the ammonium salt aqueous solution is 0.05 to 0.10:1.
[0022] Preferably, the dispersion in step S3 is carried out under the joint action of a disperser and an emulsifier, the speed of the disperser is 1500-2500 rpm, the speed of the emulsifier is 3000-5000 rpm, and the joint action time is 30 minutes to 60 minutes, more preferably 45 minutes.
[0023] Under the joint action of the disperser and the emulsifier, the aerogel particles of the filter cake of the present application are uniform and fine, so that the aerogel film opening agent has good dispersibility and filterability.
[0024] Another object of the present invention is to provide a film opening agent prepared by the above method.
[0025] The present invention also provides the use of the film opening agent in preparing polyethylene terephthalate film to improve the film performance.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] (1) The present application adopts high-purity water glass as the raw material for preparing silicon dioxide by the sol-gel method, wherein the Fe element content of the high-purity water glass is ≤15ppm, the Al element content is ≤1ppm, the Ca element content is ≤1ppm, the Mg element content is ≤1ppm, the solubility of solid water glass is ≥99.5%, the iron content and the content of other miscellaneous elements are small, and the solubility of fixed water glass is high, which can ensure that the appearance of the synthesized anti-blocking agent masterbatch is white, the color is lighter, and the transparency is higher.
[0028] (2) The present application adopts high-purity water glass and sulfuric acid high-pressure convection method to react, which can ensure that the generated silica gel has a uniform structure, high stability, and is easy to disperse in the opening agent synthesis process.
[0029] (3) The present application adopts pure water washing to reduce the sulfate ion of silica, and ammonium salt solution washing, in which the ammonium ions and sodium ions are exchanged with each other to increase the washing speed, saving the amount of water washing, and can also expand the pores of silica particles to a certain extent. Sulfuric acid solution washing can reduce the iron elements in sulfuric acid and water glass and the iron elements and other impurities in the production process to a certain extent, thereby ensuring the appearance and color of the anti-blocking agent masterbatch.
[0030] (4) The present application uses silane coupling agents A and B to simultaneously treat silicone gel, wherein silane coupling agent A can increase the affinity between silica particles and organic polymers, improve their antistatic, lubricating and moisture-proof properties, and reduce the friction coefficient and bonding resistance, while silane coupling agent B can increase the hardness of the silica structure, thereby making the silica better dispersed in the opening agent system. The two work together to achieve better opening and dispersion effects. DETAILED DESCRIPTION
[0031] The technical scheme of the present invention will be clearly and completely described below in combination with the embodiments of the present invention and the comparative examples. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods; the materials and reagents used are reagents and materials that can be obtained from commercial channels unless otherwise specified.
[0033] Example 1
[0034] At a temperature of 30°C, the pressure of the water glass and sulfuric acid pump flow tubes was 1 MPa, and 16 L of high-purity water glass with a flow rate of 200 L / h, a silica concentration of 15 wt%, and a modulus of 3.25, and 4 L of sulfuric acid solution with a flow rate of 50 L / h and a concentration of 30 wt% were simultaneously injected into a 50 L stirred reaction vessel for 6 min to form a silica sol. After the silica sol was formed, caustic soda was added to adjust the pH to 9.0, the temperature was raised to 95°C, and KH540 (γ-aminopropyltrimethoxysilane) with a silica content of 0.40 wt% and KH580 (3-mercaptopropyltrimethoxysilane) with a silica content of 0.10 wt% were added. Methoxysilane), and stirred and aged for 3 hours under this condition. After aging, sulfuric acid was added to adjust the pH value to 3, and aged for 1 hour to form silica gel. After the gel was completed, the temperature was cooled to 60°C, and the filter press frame was drawn into the water washing. The silica gel was washed according to 60°C pure water, 50% sulfuric acid solution, ammonium bicarbonate: water solution of 0.05:1, and 60°C pure water. The washing sequence time intervals were 1:5:3:1, and the water washing time was 5 hours. The water washing was carried out until the conductivity was below 50us / cm. After washing, it was dispersed for 45 minutes with a disperser and an emulsifier at the same time. The speed of the disperser was 2500 rpm and the speed of the emulsifier was 3000 rpm. The slurry obtained after dispersion was spray dried and pulverized by air flow to obtain a product with a particle size of 3.00-5.00um.
[0035] Testing methods and standards for the physical and chemical properties of products:
[0036] (1) Porosity test: fully automatic surface area and porosity analyzer Mike: TriStar II 3020;
[0037] (2) Average particle size: Laser particle size analyzer: Malvern 3000;
[0038] (3) Oil absorption value: Knife picking method: the amount of dibutyl phthalate absorbed by 1g of silica; refer to industry standard HG / T3072-2008;
[0039] (4) Iron content test: o-phenanthroline spectrophotometry;
[0040] (5) Conductivity test: Leici DDS-11A;
[0041] (6) Bulk density test: Bulk density refers to the density obtained by dividing the mass of the powder by the volume V of the container occupied by the powder, also known as bulk density;
[0042] The physicochemical properties of the seven parallel products are shown in Table 1.
[0043] Table 1
[0044]
[0045]
[0046] Example 2
[0047] At a temperature of 40°C, the pressure of the water glass and sulfuric acid pump flow tubes was 0.5 MPa, and 18 L of high-purity water glass with a flow rate of 230 L / h, a silica concentration of 10 wt%, and a modulus of 3.25, and 5 L of sulfuric acid solution with a flow rate of 50 L / h and a concentration of 30 wt% were simultaneously injected into a 50 L stirred reaction vessel for 5 min to form a silica sol. After the silica sol was formed, caustic soda was added to adjust the pH to 10.0, the temperature was raised to 80°C, and KH550 (γ-glycidyloxypropyl) with a silica content of 0.64 wt% and KH580 (3-mercaptopropyltrimethoxysilane) with a silica content of 0.16 wt% were added. Methoxysilane), and stirred and aged for 2 hours under this condition. After aging, sulfuric acid was added to adjust the pH value to 4, and aged for 0.5 hours to form silica gel. After the gel was completed, the temperature was cooled to 70°C, and the filter press frame was drawn into the water washing. The silica gel was washed according to 60°C pure water, 50% sulfuric acid solution, ammonium bicarbonate: water solution of 0.05:1, and 60°C pure water. The washing sequence time intervals were 1:5:3:1, and the water washing time was 5 hours. The conductivity was washed below 50us / cm. After washing, it was dispersed for 45 minutes with a disperser and an emulsifier at the same time. The speed of the disperser was 2500 rpm and the speed of the emulsifier was 5000 rpm. The slurry obtained after dispersion was spray dried and pulverized by air flow to obtain a product with a particle size of 3.00~5.00um.
[0048] The testing methods and standards for the physicochemical properties of the products are the same as those in Example 1. The physicochemical properties of seven parallel products are shown in Table 2.
[0049] Table 2
[0050]
[0051]
[0052] Example 3
[0053] At a temperature of 20°C, the pressure of the water glass and sulfuric acid pump flow tubes was 1 MPa, and 14 L of high-purity water glass with a flow rate of 180 L / h, a silica concentration of 20 wt%, and a modulus of 3.25, and 3 L of sulfuric acid solution with a flow rate of 30 L / h and a concentration of 30 wt% were simultaneously injected into a 50 L stirred reaction vessel for 8 min to form a silica sol. After the silica sol was formed, caustic soda was added to adjust the pH to 8.0, the temperature was raised to 95°C, and KH560 (γ-aminopropyltriethoxysilane) with a silica content of 0.56 wt% and KH590 (3-mercaptopropyltriethoxysilane) with a silica content of 0.14 wt% were added. triethoxysilane), and stirred and aged for 5 hours under this condition. After aging, sulfuric acid was added to adjust the pH value to 2, and aged for 1.5 hours to form silica gel. After the gel was completed, the temperature was cooled to 50°C, and the filter press frame was drawn into the water washing. The silica gel was washed according to 80°C pure water, 30% sulfuric acid solution, ammonium bicarbonate: water solution of 0.10:1, and 80°C pure water. The washing sequence time intervals were 1:5:3:1, and the water washing time was 3 hours. The water washing was carried out until the conductivity was below 50us / cm. After washing, it was dispersed for 45 minutes with a disperser and an emulsifier at the same time. The speed of the disperser was 1500 rpm and the speed of the emulsifier was 5000 rpm. The slurry obtained after dispersion was spray dried and pulverized by air flow to obtain a product with a particle size of 3.00~5.00um.
[0054] The testing methods and standards for the physicochemical properties of the products are the same as those in Example 1. The physicochemical properties of seven parallel products are shown in Table 3.
[0055] Table 3
[0056]
[0057]
[0058] Example 4
[0059] At a temperature of 25°C, the pressure of the water glass and sulfuric acid pump flow tubes was 0.9 MPa. 16 L of high-purity water glass with a flow rate of 200 L / h, a silica concentration of 15 wt%, and a modulus of 3.20, and 4 L of sulfuric acid solution with a flow rate of 40 L / h and a concentration of 40 wt% were simultaneously injected into a 50 L stirred reaction vessel for 5 min to form silica sol. After the silica sol was formed, caustic soda was added to adjust the pH to 9.5, the temperature was raised to 90°C, and KH530 (γ-(methacryloyloxy)propyltrimethoxysilane) with a silica content of 0.48 wt% and KH590 ( 3-mercaptopropyl triethoxysilane), and stirred and aged for 3 hours under this condition. After aging, sulfuric acid was added to adjust the pH value to 4, and aged for 1.0 hour to form silica gel. After the gel was completed, the temperature was cooled to 70°C, and the filter press frame was drawn into the water washing. The silica gel was washed according to 70°C pure water, 60% sulfuric acid solution, ammonium bicarbonate: water solution of 0.08:1, and 70°C pure water. The washing sequence time intervals were 1:5:3:1, and the water washing time was 4 hours. The conductivity was washed to less than 50us / cm. After washing, it was dispersed for 45 minutes with a disperser and an emulsifier at the same time. The speed of the disperser was 2000 rpm and the speed of the emulsifier was 3000 rpm. The slurry obtained after dispersion was spray dried and pulverized by air flow to obtain a product with a particle size of 3.00~5.00um.
[0060] The testing methods and standards for the physicochemical properties of the products are the same as those in Example 1. The physicochemical properties of seven parallel products are shown in Table 4.
[0061] Table 4
[0062]
[0063]
[0064] Example 5
[0065] At a temperature of 29°C, the pressure of the water glass and sulfuric acid pump flow tubes was 0.7 MPa, and 15 L of high-purity water glass with a flow rate of 190 L / h, a silica concentration of 18 wt%, and a modulus of 3.30, and 3.8 L of sulfuric acid solution with a flow rate of 45 L / h and a concentration of 40 wt% were simultaneously injected into a 50 L stirred reaction vessel for 6 min to form a silica sol. After the silica sol was formed, caustic soda was added to adjust the pH to 9.5, the temperature was raised to 95°C, and KH570 (γ-(methacryloyloxy)propyltrimethoxysilane) with a silica content of 0.64 wt% and KH580 with a silica content of 0.16 wt% were added. (3-mercaptopropyltrimethoxysilane), and stirred and aged for 5 hours under this condition. After aging, sulfuric acid was added to adjust the pH value to 3, and aged for 1.0 hour to form silica gel. After the gel was completed, the temperature was cooled to 60°C, and the filter press frame was drawn into the water washing. The silica gel was washed according to 50°C pure water, 30% sulfuric acid solution, ammonium bicarbonate: water solution of 0.05:1, and 50°C pure water. The washing sequence time intervals were 1:5:3:1, and the water washing time was 5 hours. The conductivity was washed below 50us / cm. After washing, it was dispersed for 45 minutes with a disperser and an emulsifier at the same time. The speed of the disperser was 2000 rpm and the speed of the emulsifier was 5000 rpm. The slurry obtained after dispersion was spray dried and pulverized by air flow to obtain a product with a particle size of 3.00~5.00um.
[0066] The testing methods and standards for the physicochemical properties of the products are the same as those in Example 1. The physicochemical properties of seven parallel products are shown in Table 5.
[0067] Table 5
[0068]
[0069] Example 6
[0070] At a temperature of 30°C, the pressure of the water glass and sulfuric acid pump flow tubes was 0.8 MPa. 15 L of high-purity water glass with a flow rate of 210 L / h, a silica concentration of 15 wt%, and a modulus of 3.40, and 5 L of sulfuric acid solution with a flow rate of 40 L / h and a concentration of 30 wt% were simultaneously injected into a 50 L stirred reaction vessel for 7 min to form a silica sol. After the silica sol was formed, caustic soda was added to adjust the pH to 9.0, the temperature was raised to 90°C, and KH520 (γ-glycidyloxypropyl) with a silica content of 0.40 wt% and KH580 (3-mercaptopropyl) with a silica content of 0.10 wt% were added. 1-trimethoxysilane), and stirred and aged for 4 hours under this condition. After aging, sulfuric acid was added to adjust the pH value to 4, and aged for 1.0 hour to form silica gel. After gelling, the temperature was cooled to 65°C, and the filter press frame was drawn into the water washing. The silica gel was washed according to 55°C pure water, 60% sulfuric acid solution, ammonium bicarbonate: water solution of 0.10:1, and 55°C pure water. The washing sequence time intervals were 1:5:3:1, and the water washing time was 5 hours. The conductivity was washed to less than 50us / cm. After washing, it was dispersed for 45 minutes with a disperser and an emulsifier at the same time. The speed of the disperser was 2500 rpm and the speed of the emulsifier was 4000 rpm. The slurry obtained after dispersion was spray dried and pulverized by air flow to obtain a product with a particle size of 3.00-5.00um.
[0071] The testing methods and standards for the physicochemical properties of the products are the same as those in Example 1. The physicochemical properties of seven parallel products are shown in Table 6.
[0072] Table 6
[0073]
[0074] Comparative Example 1
[0075] The difference compared with Example 1 is that high-purity water glass is not used, but ordinary water glass is used. The element analysis of ordinary water glass shows that the Fe content is equal to 35 ppm, the Al content is equal to 5.3 ppm, the Ca content is equal to 4.7 ppm, the Mg content is equal to 4.9 ppm, and the solubility of solid water glass is equal to 95.5%. Other operations are the same as in Example 1.
[0076] The testing methods and standards for the physicochemical properties of the products are the same as those in Example 1. The physicochemical properties of seven parallel products are shown in Table 7.
[0077] Table 7
[0078]
[0079]
[0080] Comparative Example 2
[0081] The difference compared with Example 1 is that, instead of using pressurized water glass and sulfuric acid flow meters, ordinary flow tubes are used instead, wherein the water glass flow rate is 200 L / h, and the sulfuric acid flow rate is 50 L / h, and other operations are the same as in Example 1.
[0082] The testing methods and standards for the physicochemical properties of the products are the same as those in Example 1. The physicochemical properties of seven parallel products are shown in Table 8.
[0083] Table 8
[0084]
[0085] Comparative Example 3
[0086] The difference compared with Example 1 is that 80°C pure water is used instead of 60°C pure water in Example 1, 50% sulfuric acid solution, a solution with a weight ratio of ammonium bicarbonate: water of 0.05:1, and 60°C pure water are used to wash the silica gel, and the washing sequence time intervals are 1:5:3:1 steps respectively, and the silica gel is directly washed for 5 hours. Other operations are the same as Example 1.
[0087] The testing methods and standards for the physicochemical properties of the products are the same as those in Example 1. The physicochemical properties of seven parallel products are shown in Table 9.
[0088] Table 9
[0089]
[0090] Comparative Example 4
[0091] The difference compared with Example 1 is that KH540 (γ-aminopropyltrimethoxysilane) with a silicon dioxide content of 0.50 wt% is added instead of KH580 (3-mercaptopropyltrimethoxysilane). Other operations are the same as Example 1.
[0092] The testing methods and standards for the physicochemical properties of the products are the same as those in Example 1. The physicochemical properties of seven parallel products are shown in Table 10.
[0093] Table 10
[0094]
[0095]
[0096] Comparative Example 5
[0097] The difference compared with Example 1 is that KH580 (3-mercaptopropyltrimethoxysilane) with a silicon dioxide content of 0.50 wt % is added instead of KH540 (γ-aminopropyltrimethoxysilane). Other operations are the same as in Example 1.
[0098] The testing methods and standards for the physicochemical properties of the products are the same as those in Example 1. The physicochemical properties of seven parallel products are shown in Table 11.
[0099] Table 11
[0100]
[0101] Comparative Example 6
[0102] The difference compared with Example 1 is that, instead of adding KH540 (γ-aminopropyltrimethoxysilane) with a silica content of 0.40wt% and KH580 (3-mercaptopropyltrimethoxysilane) with a silica content of 0.10wt%, KH540 (γ-aminopropyltrimethoxysilane) with a silica content of 0.40wt% and A171 (vinyltrimethoxysilane) with a silica content of 0.10wt% are added, and the other operations are the same as in Example 1.
[0103] The testing methods and standards for the physicochemical properties of the products are the same as those in Example 1. The physicochemical properties of seven parallel products are shown in Table 12.
[0104] Table 12
[0105]
[0106] Comparative Example 7
[0107] The difference compared with Example 1 is that A171 (vinyltrimethoxysilane) with a silica content of 0.40wt% and KH580 (3-mercaptopropyltrimethoxysilane) with a silica content of 0.10wt% are added instead of KH540 (γ-aminopropyltrimethoxysilane) with a silica content of 0.40wt% and KH580 (3-mercaptopropyltrimethoxysilane) with a silica content of 0.10wt%. The other operations are the same as in Example 1.
[0108] The testing methods and standards for the physicochemical properties of the products are the same as those in Example 1. The physicochemical properties of seven parallel products are shown in Table 13.
[0109] Table 13
[0110]
[0111] Results Analysis
[0112] It can be seen from the test data of the above six embodiments of the present invention that the physical indicators of the products produced according to the technical solution of the present invention are basically similar, indicating that the production of this technical solution is stable.
[0113] From Comparative Example 1, it can be seen that the oil absorption and porosity of the product produced by using ordinary water glass instead of high-purity water glass are significantly reduced, while the bulk density, electrical conductivity and iron content are significantly increased, and the particle size does not change much. This is mainly because the increase of impurity elements in ordinary water glass causes a chelating reaction between the primary silica particles and the impurity elements, which reduces the degree of the silica sol network structure, thereby resulting in a decrease in oil absorption and porosity.
[0114] In addition, by using conventional ordinary flow tubes to replace the pressurized water glass and sulfuric acid flow meters in Comparative Example 2, the oil absorption and porosity of the product will be significantly reduced, while the bulk density, electrical conductivity and iron content will be significantly increased. This is mainly because the high-pressure convection accelerates the rapid formation of silica primary particles, thereby allowing the rapid formation of the silica network structure. The richness of the silica network structure also increases, thereby improving the porosity of the silica.
[0115] In Comparative Example 3, ordinary pure water is directly used to replace sulfuric acid solution, ammonium bicarbonate solution and the three solutions to wash the silica gel. The oil absorption and porosity of the product are significantly reduced, while the bulk density, electrical conductivity and iron content are significantly increased. The sulfuric acid solution can reduce the content of iron. The main reason is that the sulfuric acid solution can react with the iron element to a certain extent, thereby reducing the iron content in the silica structure; ammonium ions can expand the pores and improve the washing efficiency to a certain extent. The main reason is that ammonium ions can exchange ions with hydrogen ions, thereby making the porosity of the silica richer and larger, thereby expanding the pores with ammonium bicarbonate, and the exchange of ammonium ions with hydrogen ions can improve the washing efficiency to a certain extent.
[0116] In Comparative Examples 4 and 5, the oil absorption and porosity of the products synthesized by directly using a silane coupling agent A or B will be significantly reduced, while the bulk density, electrical conductivity and iron content will not change much. However, the application effect of the two silane coupling agents cannot be achieved. This is mainly because the silane coupling agent type A (γ silane coupling agent, etc.) and type B (3-mercaptosilane coupling agent) can react with the silanol groups of silica. The type A coupling agent can increase the affinity of the silica particles with the organic polymer, improve its antistatic, lubricating and moisture-proof properties, and reduce the friction coefficient and bonding resistance. The silane coupling agent B can increase the hardness of the silica structure, thereby making the silica better dispersed in the opening agent system. The combination of the two makes the oil absorption and porosity of the product larger, and is better used in plastic film opening agents. Comparative Examples 6 and 7 better prove that the silane coupling agents A and B used together in the present invention have a synergistic effect, while in Comparative Examples 6 and 7, another silane coupling agent A-171 (vinyl triethoxysilane) or A-172 (vinyl tri(β-methoxyethoxy) silane) coupling agent is selected to replace the silane coupling agent type A (γ silane coupling agent, etc.) or type B (3-mercaptosilane coupling agent) to synthesize the opening agent. The oil absorption and pore volume cannot reach the expected value. It can be seen that the combined use of coupling agents A and B needs to be screened and scientifically and reasonably matched to achieve the technical effect of the present invention.
[0117] Application performance testing
[0118] The three silica sol-gel example products 1-5, 3-5, 5-5 and comparative examples 1-5, 3-5, 5-5 prepared by the present invention were used to compare the performance of plastic film opening agents with Fuji SY340 and Grace E300. Polyethylene terephthalate: silica opening agent: dispersant (ethylene glycol): antioxidant (commercially available antioxidant 1010): antistatic agent (sold by Dinghai Plastic Chemical Co., Ltd.) were melt-mixed in a ratio of 93.5:0.5:3:2:1 to form an opening masterbatch, which was then melt-mixed by a twin-screw extruder and then subjected to longitudinal stretching, transverse stretching, and heat setting treatment to obtain a polyethylene terephthalate film. The film application performance was tested, and the physical and chemical indicators and application test results are shown in Table 14.
[0119] Table 14
[0120]
[0121] By comparing the three samples of Examples 1-5, 3-5, and 5-5, the three samples of Comparative Examples 1-5, 3-5, and 5-5 with the Fuji SY340 and Grace E300 anti-blocking agent products, the anti-blocking agent synthesized by the method of the present invention is close to or even better than the physical and chemical indicators and application performance of the foreign anti-blocking agent, and has good transparency, low haze and good transparency, and the anti-blocking performance is close to that of the anti-blocking agent product.
[0122] Obviously, the above embodiments of the present invention are only examples for clearly illustrating the technical solution of the present invention, and are not intended to limit the specific implementation methods of the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the claims of the present invention shall be included in the protection scope of the claims of the present invention.
Claims
1. A method for preparing a sol-gel film opening agent, characterized in that: The steps include: S1, forming silica sol by pressurized convection of water glass solution and sulfuric acid; S2, heating the silica sol obtained in step S1, adjusting the pH to be alkaline, then adding silane coupling agent A and silane coupling agent B for modification, adjusting the pH to be acidic after aging, and then aging to form silica gel; S3, washing the silica gel obtained in step S2, and dispersing the silica gel uniformly after washing; S4, drying and crushing the slurry dispersed in step S3 to obtain; The silane coupling agent A is one of γ-aminopropylmethyldiethoxysilane, γ-aminopropylmethyldimethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-glycidyloxypropyl, and γ-(methacryloyloxy)propyltrimethoxysilane; the silane coupling agent B is one of 3-mercaptopropyltrimethoxysilane and 3-mercaptopropyltriethoxysilane; In step S1, the Fe content of the water glass solution is ≤15ppm, the Al content is ≤1ppm, the Ca content is ≤1ppm, the Mg content is ≤1ppm, and the solubility of solid water glass is ≥99.5%; The washing in step S3 refers to washing with pure water, sulfuric acid solution, ammonium salt aqueous solution, and pure water in a washing order with a washing time ratio of 1:5:3:1 respectively, and the total washing time is 3h, 4h or 5h, until the conductivity of the silica gel is below 50us / cm.
2. The method for preparing a sol-gel film opening agent according to claim 1, characterized in that: The silicon dioxide modulus of the water glass solution in step S1 is 3.20-3.40, the concentration is 10wt%-20wt%, and the concentration of sulfuric acid is 30wt%-50wt%.
3. The method for preparing a sol-gel film opening agent according to claim 1, characterized in that: After the pressurization in step S1, the flow pipeline pressure of the water glass and sulfuric acid is maintained at 0.5Mpa~1Mpa, the flow rate of the water glass solution is 180L / h~230L / h, and the flow rate of the sulfuric acid is 30L / h~50L / h.
4. The method for preparing a sol-gel film opening agent according to claim 1, characterized in that: The total amount of the silane coupling agent added in step S2 is 0.50wt%~0.80wt% of the dry base material, wherein the mass ratio of silane coupling agent A to silane coupling agent B is 4:
1.
5. The method for preparing a sol-gel film opening agent according to claim 1, characterized in that: The conductivity of the pure water is lower than 5us / cm, the temperature is 50°C~80°C, the concentration of the sulfuric acid solution is 30%~60%, the ammonium salt is one of ammonium sulfate, ammonium bisulfate, ammonium carbonate and ammonium bicarbonate, and the weight ratio of ammonium salt to water in the ammonium salt aqueous solution is 0.05~0.10:
1.
6. The method for preparing a sol-gel film opening agent according to claim 1, characterized in that: The dispersion in step S3 is carried out under the joint action of a disperser and an emulsifier, the speed of the disperser is 1500-2500 rpm, the speed of the emulsifier is 3000-5000 rpm, and the joint action time is 30 minutes to 60 minutes.
7. A sol-gel film opening agent, characterized in that: Prepared by the method according to any one of claims 1 to 6, the film opening agent has a particle size of 3.00-5.00 μm.
8. Use of the film opening agent according to claim 7 in improving the performance of preparing polyethylene terephthalate film.