A fracturing fluid concentrate and preparation method thereof, and a fracturing fluid

The fracturing fluid stock solution prepared through the inverse emulsion polymerization method solves the problems of complex operation and high cost of existing fracturing fluids, enables online adjustment of concentration and good performance of fracturing fluid, and is suitable for mixed water fracturing technology.

CN116041615BActive Publication Date: 2024-10-11CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111266179.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-28
Publication Date
2024-10-11
Estimated Expiration
2041-10-28

AI Technical Summary

Technical Problem

There are many types of fracturing fluid additives used for mixed water fracturing, with numerous construction procedures and complex operations. It is impossible to achieve online continuous fluid mixing, which increases the cost.

Method used

The fracturing fluid stock solution is prepared using the inverse emulsion polymerization method, using a water phase composed of acrylamide, sodium 2-acrylamide-2-methylpropanesulfonate and an oil phase composed of white oil and emulsifier. By controlling the pH value and the ratio of molecular weight regulator to form a fracturing fluid stock solution with good tackiness, tackification, resistance reduction and salt resistance properties, and the concentration and use can be adjusted online.

Benefits of technology

It achieves simple operation, rapid dissolution, good sand suspension performance and low friction of the fracturing fluid. It is suitable for various complex water qualities, reduces construction costs, and improves the stability and efficiency of the fracturing fluid.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116041615B_ABST
    Figure CN116041615B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of oil and gas field fracturing transformation, and specifically relates to a fracturing fluid stock solution and a preparation method thereof and a fracturing fluid. The fracturing fluid stock solution of the present invention is mainly obtained by reverse emulsion polymerization of an aqueous phase and an oil phase; the aqueous phase is mainly composed of a molecular weight regulator, a metal ion removal agent, a pH regulator, acrylamide, 2-acrylamide-2-methylpropanesulfonate sodium and water; the pH value of the aqueous phase is 6.8-7.0. The fracturing fluid stock solution of the present invention has good viscosity and viscosity-increasing properties in different water qualities, and exhibits good salt resistance, is suitable for various complex water qualities, and has good resistance reduction performance and temperature resistance and shear resistance. When the fracturing fluid emulsion stock solution of the present invention is used to prepare the fracturing fluid, there is no need to prepare the liquid in advance, and the use concentration can be adjusted online at any time, with the advantages of fast dissolution rate, good sand suspension performance and low friction resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of oil and gas field fracturing transformation, and specifically relates to a fracturing fluid stock solution and a preparation method thereof, and a fracturing fluid. Background Art

[0002] Hydraulic fracturing is the main measure for the effective development of low permeability oil and gas fields. In recent years, due to the successful application of the volume fracturing concept, in-depth research has been carried out at home and abroad, and a series of technological advances have been made. Among them, mixed water fracturing technology is one of them. This technology has gone through four major development stages: (1) In the 1980s, tap water fracturing was the main method; (2) In the 1990s, it transitioned to slick water fracturing; (3) At the beginning of this century, it developed into mixed water fracturing; (4) Currently, the main method used is horizontal well multi-stage + mixed water fracturing technology. Among them, mixed water fracturing technology is mainly used for tight reservoirs with developed natural fractures and high rock brittleness index. By adopting "large liquid volume, large sand volume, large displacement, high sand ratio" and low viscosity and high viscosity sand-carrying fluid, the fracture conductivity is improved, the natural fractures are opened and effectively supported, and a network of fractures is formed, thereby forming sand-filled fractures with certain geometric dimensions and high conductivity in the formation near the bottom of the well, so that the well can achieve the purpose of increasing production and injection.

[0003] Chinese patent document CN104212436A discloses a fracturing fluid for mixed water fracturing, which is composed of 0.05-0.50% thickener, 0.02-0.15% sand suspension capacity enhancer, 0.05-0.20% drag reducer, 0.30-1.00% clay stabilizer, 0.30-1.00% drainage aid, 0.05-0.20% bactericide and 0.01-0.10% breaker. There are many kinds of additives in the above fracturing fluid, and the construction procedures are numerous and the operation is complicated. It cannot be mixed online and must be prepared in advance, which invisibly increases its cost. In addition, slippery water and sand-carrying fluid belong to two different types of systems, both of which need to be prepared in advance. At present, it is impossible to achieve online continuous preparation. Summary of the invention

[0004] The purpose of the present invention is to provide a fracturing fluid concentrate to solve the problems that the fracturing fluid currently used for mixed water fracturing has many types of additives, numerous construction procedures and complicated operations.

[0005] The second object of the present invention is to provide a method for preparing a fracturing fluid concentrate.

[0006] The third object of the present invention is to provide a fracturing fluid.

[0007] In order to achieve the above-mentioned purpose, the technical solution adopted by the fracturing fluid stock solution of the present invention is:

[0008] A fracturing fluid stock solution is mainly obtained by inverse emulsion polymerization of a water phase and an oil phase; the water phase is mainly composed of a molecular weight regulator, a metal ion removing agent, a pH regulator, acrylamide, sodium 2-acrylamide-2-methylpropane sulfonate and water; based on 100 parts by total mass of acrylamide, sodium 2-acrylamide-2-methylpropane sulfonate and water, the mass portion of acrylamide is 35-40 parts, and the mass portion of sodium 2-acrylamide-2-methylpropane sulfonate is 10-15 parts; the pH value of the water phase is 6.8-7.0.

[0009] The fracturing fluid stock solution of the present invention uses acrylamide and sodium 2-acrylamide-2-methylpropane sulfonate as polymerization monomers, and the fracturing fluid stock solution obtained by reverse emulsion polymerization has good viscosity and viscosity-increasing performance in different water qualities, and shows good salt resistance, is suitable for various complex water qualities, and has good resistance reduction performance and temperature resistance and shear resistance. When the fracturing fluid stock solution of the present invention is used to prepare the fracturing fluid, there is no need to prepare the liquid in advance, and the use concentration can be adjusted online at any time, and it has the advantages of fast dissolution speed, good sand suspension performance and low friction resistance.

[0010] Preferably, based on 100 parts by total weight of acrylamide, sodium 2-acrylamide-2-methylpropane sulfonate and water, the weight of acrylamide is 37.5 parts, and the weight of sodium 2-acrylamide-2-methylpropane sulfonate is 12.75 parts.

[0011] Preferably, the method for preparing the aqueous phase comprises the following steps: firstly dissolving sodium 2-acrylamide-2-methylpropane sulfonate in part of water to obtain a sodium 2-acrylamide-2-methylpropane sulfonate aqueous solution with a mass fraction of 45-50%, then uniformly mixing acrylamide, a sodium 2-acrylamide-2-methylpropane sulfonate aqueous solution with a mass fraction of 45-50, and the remaining amount of water to obtain a solution A, then adding a molecular weight regulator and a metal ion removing agent to the solution A, mixing uniformly, to obtain a solution B, and finally adding a pH regulator to the solution B, mixing uniformly, to obtain the solution.

[0012] Preferably, the molecular weight regulator is a composite molecular weight regulator and / or sodium hypophosphite monohydrate. Preferably, the composite molecular weight regulator is composed of sodium formate and urea. Preferably, the mass ratio of sodium formate to urea is 2:1. Preferably, the mass fraction of the molecular weight regulator in the aqueous phase is 60 to 80 ppm. Experiments have shown that when the mass fraction of the molecular weight regulator in the aqueous phase is less than 60 ppm, the polymer molecular chain is severely branched during the chain transfer process, resulting in more insoluble colloids in the finished product, which seriously affects the production and preparation, and the stock solution has poor solubility and slow viscosity; when the mass fraction of the molecular weight regulator in the aqueous phase is greater than 80 ppm, the obtained polymer fraction is small, which affects the drag reduction performance and temperature and shear resistance of the fracturing fluid prepared from the fracturing fluid stock solution.

[0013] Preferably, the pH regulator is acrylic acid. Using acrylic acid as a pH regulator can adjust the pH value of the reaction system, and acrylic acid can also participate in the polymerization reaction, thereby avoiding the introduction of free corrosive ions and reducing the corrosion of the prepared fracturing fluid to the equipment during construction.

[0014] Preferably, the oil phase is mainly composed of white oil and emulsifier. Preferably, the white oil is No. 7 white oil. Preferably, the HLB value of the emulsifier is 4 to 8. When the HLB value of the emulsifier is less than 4, the solubility of the obtained fracturing fluid stock solution is poor, and the finished product itself is relatively viscous, which affects the dispersion effect of the stock solution in water. When the HLB value of the emulsifier is greater than 8, the stability of the obtained fracturing fluid stock solution is poor and stratification occurs in a short time.

[0015] Preferably, the emulsifier is a nonionic surfactant. Preferably, the nonionic surfactant is Span or a compound nonionic surfactant; the nonionic surfactant is composed of Span and Tween. Preferably, the nonionic surfactant is Span 80. Preferably, the oil phase is composed of No. 7 white oil and Span 80. Preferably, the mass ratio of No. 7 white oil to Span 80 is 10:1. When white oil and Span 80 are used as the oil phase, the stability of the prepared fracturing fluid stock solution can be improved.

[0016] Preferably, the mass ratio of the water phase to the oil phase is 6.8:3.2. When the mass ratio of the water phase to the oil phase is 6.8:3.2, not only can the reaction system be guaranteed to have good stability, but also the prepared fracturing fluid stock solution can be guaranteed to have a high solid content.

[0017] Preferably, the metal ion removal agent is a metal chelating agent. Preferably, the metal chelating agent is diethylenetriamine pentaacetic acid sodium salt and / or ethylenediaminetetraacetic acid sodium salt. Preferably, the diethylenetriamine pentaacetic acid sodium salt is diethylenetriamine pentaacetic acid pentasodium. Preferably, the ethylenediaminetetraacetic acid sodium salt is ethylenediaminetetraacetic acid disodium. Preferably, the mass fraction of the metal ion removal agent in the aqueous phase is 150 to 200 ppm.

[0018] The technical solution adopted by the method for preparing the fracturing fluid stock solution of the present invention is:

[0019] A method for preparing the above-mentioned fracturing fluid stock solution comprises the following steps: firstly, mixing and emulsifying the water phase and the oil phase to obtain a mixed phase, then adding an initiator to the mixed phase under an inert atmosphere, and then performing inverse emulsion polymerization.

[0020] The preparation method of the fracturing fluid stock solution of the present invention is simple and easy to operate.

[0021] Preferably, the viscosity of the mixed phase is 600-800 mPa·s. When the viscosity of the mixed phase is 600-800 mPa·s, the prepared fracturing fluid can be guaranteed to have good stability. Further preferably, the viscosity of the mixed phase is 680-800 mPa·s.

[0022] Preferably, the temperature of the inverse emulsion polymerization does not exceed 60°C. The temperature of the inverse emulsion polymerization does not exceed 60°C. When the reaction temperature is too high, the number of free radicals is large, the chain transfer is violent, and chain termination is likely to occur, making it difficult to prepare a high molecular weight polymer. At the same time, when the temperature is too high, the emulsion itself is unstable and is prone to risks such as demulsification. When the temperature is too low, the number of free radicals is small, the chain transfer is weak, and chain termination is likely to occur prematurely, resulting in a low polymer quality. Therefore, by controlling a reasonable temperature range, under the action of a molecular weight regulator, a polymer with a larger molecular weight can be prepared, which can effectively ensure that the molecular weight is controlled within a narrow range, that is, between 15 million and 18 million.

[0023] Preferably, the initiator is composed of persulfate and bisulfite. Preferably, the initiator is composed of ammonium persulfate and sodium bisulfite. Preferably, the mass ratio of ammonium persulfate and sodium bisulfite is (1-2): (5-3). Preferably, the amount of ammonium persulfate added is 5-10ppm of the mass of the aqueous phase. Preferably, the amount of sodium bisulfite added is 15-25ppm of the mass of the aqueous phase. When there is too much initiator, the reaction will be violent, the heat will be released rapidly, and the heat will not be easily released, resulting in excessive temperature, uncontrolled heat release, explosion, and polymerization failure; when the initiator is less, the monomer polymerization reaction is slow, the reaction time is long, the efficiency is low, the polymer molecular weight distribution range is wide, and the monomer conversion rate is low. At the same time, when the amount of oxidant persulfate is too low, the reaction activity of the system is low, the monomer is difficult to generate free radicals, and thus it is difficult to be induced to cause chain transfer; if the concentration of the oxidant persulfate is too high, the monomer is easily initiated, the reaction is violent, and the polymer molecular weight is too low. Only when the persulfate and sulfite are used in a certain amount and within a certain ratio range, can a higher molecular weight polymer be obtained, the polymerization process can be well controlled, and the cost can be saved.

[0024] The technical solution adopted by the fracturing fluid of the present invention is:

[0025] A fracturing fluid is mainly obtained by mixing the above-mentioned fracturing fluid stock solution and water.

[0026] The fracturing fluid of the present invention has a good drag reduction effect, the drag reduction rate changes little with viscosity, and has a good dynamic sand suspension property. The fracturing fluid stock solution of the present invention can be used for the preparation of slick water, the preparation of linear glue, and the preparation of sand suspension liquid, and can be used to prepare a variety of fracturing fluids.

[0027] When preparing fracturing fluid, you can use tap water, highly mineralized brine, and various types of flowback fluids used on site.

[0028] Preferably, the mass ratio of the fracturing fluid stock solution to water is (0.4-0.6):(99.4-99.6). When the mass ratio of the fracturing fluid stock solution to water is (0.4-0.6):(99.4-99.6), the obtained fracturing fluid is a low-viscosity fracturing fluid.

[0029] Preferably, the mass ratio of the fracturing fluid stock solution to water is (0.8-1.2):(98.8-99.2). When the mass ratio of the fracturing fluid stock solution to water is (0.8-1.2):(98.8-99.2), the obtained fracturing fluid is a high-viscosity fracturing fluid. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 is the rheological curve of the high-viscosity fracturing fluid of Example 7, wherein A represents the temperature curve, B represents the shear rate curve, and C represents the viscosity curve;

[0031] Figure 2 This is a test curve of the drag reduction rate of the low-viscosity fracturing fluid in Example 8;

[0032] Figure 3 The suspended sand test results of the high viscosity fracturing fluid in Example 9;

[0033] Figure 4 The construction fracturing curve obtained when the fracturing fluid stock prepared in Example 6 was used for the construction of J30xx well in a gas field, wherein D represents the real-time construction displacement, E represents the real-time wellhead pressure, F represents the real-time sand concentration (sand ratio), and G represents the real-time casing pressure; wherein, low viscosity fluid represents low viscosity fracturing fluid, and high viscosity sand-carrying fluid represents high viscosity fracturing fluid. DETAILED DESCRIPTION

[0034] The technical solution of the present invention is further described below in conjunction with specific implementation methods.

[0035] 1. The specific embodiments of the fracturing fluid stock solution of the present invention are as follows:

[0036] Example 1

[0037] The fracturing fluid stock solution of this embodiment is obtained by inverse emulsion polymerization of an aqueous phase and an oil phase; the aqueous phase is composed of a molecular weight regulator, a metal ion removing agent, a pH regulator, acrylamide, sodium 2-acrylamide-2-methylpropane sulfonate and water; based on the total mass of acrylamide, sodium 2-acrylamide-2-methylpropane sulfonate and water as 100 parts, the mass of acrylamide is 37.5 parts, and the mass of sodium 2-acrylamide-2-methylpropane sulfonate is 12.75 parts; the pH value of the aqueous phase is 6.8; The molecular weight regulator is composed of sodium formate and urea, the mass ratio of sodium formate to urea is 2:1, the mass fraction of the molecular weight regulator in the water phase is 60ppm, the pH regulator is acrylic acid, the oil phase is mainly composed of white oil and an emulsifier, the white oil is No. 7 white oil, the emulsifier is Span 80, the mass ratio of the water phase to the oil phase is 6.8:3.2, and the metal ion removal agent is disodium ethylenediaminetetraacetic acid, and the mass fraction of the metal ion removal agent in the water phase is 150ppm.

[0038] Example 2

[0039] The fracturing fluid stock solution of this embodiment is obtained by inverse emulsion polymerization of water phase and oil phase; the water phase is composed of a molecular weight regulator, a metal ion removing agent, a pH regulator, acrylamide, sodium 2-acrylamide-2-methylpropane sulfonate and water; based on the total mass of acrylamide, sodium 2-acrylamide-2-methylpropane sulfonate and water as 100 parts, the mass of acrylamide is 40 parts, and the mass of sodium 2-acrylamide-2-methylpropane sulfonate is 10 parts; the pH value of the water phase is 6.9; The molecular weight regulator is composed of sodium formate and urea, the mass ratio of sodium formate to urea is 2:1, the mass fraction of the molecular weight regulator in the water phase is 70ppm, the pH regulator is acrylic acid, the oil phase is mainly composed of white oil and an emulsifier, the white oil is No. 7 white oil, the emulsifier is Span 80, the mass ratio of the water phase to the oil phase is 6.8:3.2, and the metal ion removal agent is disodium ethylenediaminetetraacetic acid, and the mass fraction of the metal ion removal agent in the water phase is 180ppm.

[0040] Example 3

[0041] The fracturing fluid stock solution of this embodiment is obtained by inverse emulsion polymerization of water phase and oil phase; the water phase is composed of a molecular weight regulator, a metal ion removal agent, a pH regulator, acrylamide, sodium 2-acrylamide-2-methylpropane sulfonate and water; based on the total mass of acrylamide, sodium 2-acrylamide-2-methylpropane sulfonate and water as 100 parts, the mass of acrylamide is 35 parts, and the mass of sodium 2-acrylamide-2-methylpropane sulfonate is 15 parts; the pH value of the water phase is 7.0; The molecular weight regulator is composed of sodium formate and urea, the mass ratio of the sodium formate and urea is 2:1, the mass fraction of the molecular weight regulator in the water phase is 80ppm, the pH regulator is acrylic acid, the oil phase is mainly composed of white oil and an emulsifier, the white oil is No. 7 white oil, the emulsifier is Span 80, the mass ratio of the water phase to the oil phase is 6.8:3.2, and the metal ion removal agent is disodium ethylenediaminetetraacetic acid, and the mass fraction of the metal ion removal agent in the water phase is 200ppm.

[0042] 2. The specific embodiment of the method for preparing the fracturing fluid stock solution of the present invention is as follows:

[0043] Example 4

[0044] The method for preparing the fracturing fluid stock solution of this embodiment is the method for preparing the fracturing fluid stock solution of embodiment 1, comprising the following steps:

[0045] (1) First, acrylamide, a 50% by mass aqueous solution of sodium 2-acrylamide-2-methylpropane sulfonate and water are uniformly mixed to obtain solution A, then a molecular weight regulator and a metal ion removal agent are added to solution A, mixed uniformly to obtain solution B, and finally a pH regulator is added to solution B to adjust the pH value of solution B to be weakly acidic (pH=6.8) to obtain an aqueous phase; the mass fraction of acrylamide in the solution A is 37.5%, and the mass fraction of sodium 2-acrylamide-2-methylpropane sulfonate is 12.75%; the pH regulator is acrylic acid, the metal ion removal agent is disodium ethylenediaminetetraacetic acid, the mass fraction of the molecular weight regulator in the aqueous phase is 60 ppm, and the mass fraction of the metal ion removal agent in the aqueous phase is 150 ppm.

[0046] (2) Under nitrogen protection, the water phase and the oil phase are mixed and stirred at room temperature to emulsify until the viscosity of the mixed phase composed of the water phase and the oil phase is 680 mPa·s, and then the mixed phase is cooled to 20±3°C, and an initiator is added to the mixed phase (the initiator is composed of ammonium persulfate and sodium bisulfite, and the amount of ammonium persulfate and sodium bisulfite added is 5 ppm and 25 ppm of the mass of the water phase, respectively). Then, an inverse emulsion polymerization reaction is initiated at 20±3°C, and the temperature of the reaction system is controlled not to exceed 60°C. When the temperature of the reaction system no longer rises, excess sulfurous acid is added to the reaction system. The mixture is added with sodium bisulfite (the amount of sodium bisulfite added is 10ppm of the mass of the water phase) to react to remove a small amount of residual monomers, and then the system after the reaction is cooled to room temperature to obtain a fracturing fluid stock solution; the oil phase is composed of No. 7 white oil and Span 80, the mass ratio of No. 7 white oil to Span 80 is 10:1, and the mass ratio of the oil phase to the water phase is 3.2:6.8; the molecular weight of the polymer in the fracturing fluid stock solution prepared in this embodiment is measured according to the method of "GBT12005.10-1992 Polyacrylamide Molecular Weight Determination Viscosity Method", and the viscosity-average molecular weight is measured to be 17.5 million.

[0047] Example 5

[0048] The method for preparing the fracturing fluid stock solution of this embodiment is the method for preparing the fracturing fluid stock solution of embodiment 2, comprising the following steps:

[0049] (1) First, acrylamide, a 50% by mass aqueous solution of sodium 2-acrylamide-2-methylpropane sulfonate and water are uniformly mixed to obtain solution A, then a molecular weight regulator and a metal ion removal agent are added to solution A, mixed uniformly to obtain solution B, and finally a pH regulator is added to solution B to adjust the pH value of solution B to be weakly acidic (pH=6.9) to obtain an aqueous phase; the mass fraction of acrylamide in the solution A is 40%, and the mass fraction of sodium 2-acrylamide-2-methylpropane sulfonate is 10%; the pH regulator is acrylic acid, the metal ion removal agent is disodium ethylenediaminetetraacetate, the mass fraction of the molecular weight regulator in the aqueous phase is 70 ppm, and the mass fraction of the metal ion removal agent in the aqueous phase is 180 ppm.

[0050] (2) Under nitrogen protection, the water phase and the oil phase are mixed and stirred at room temperature to emulsify until the viscosity of the mixed phase composed of the water phase and the oil phase is 750 mPa·s, and then the mixed phase is cooled to 20±3°C, and an initiator is added to the mixed phase (the initiator is composed of ammonium persulfate and sodium bisulfite, and the amount of ammonium persulfate and sodium bisulfite added is 10 ppm and 15 ppm of the mass of the water phase, respectively). Then, an inverse emulsion polymerization reaction is initiated at 20±3°C, and the temperature of the reaction system is controlled not to exceed 60°C. When the temperature of the reaction system no longer rises, an excess of sodium bisulfite is added to the reaction system. The mixture is reacted with sodium bisulfite (the amount of sodium bisulfite added is 10ppm of the mass of the water phase) to remove a small amount of residual monomers, and then the system after the reaction is cooled to room temperature to obtain a fracturing fluid stock solution; the oil phase is composed of No. 7 white oil and Span 80, the mass ratio of No. 7 white oil to Span 80 is 10:1, and the mass ratio of the oil phase to the water phase is 3.2:6.8; the molecular weight of the polymer in the fracturing fluid stock solution prepared in this embodiment is determined according to the method of "GBT12005.10-1992 Polyacrylamide Molecular Weight Determination Viscosity Method", and the viscosity-average molecular weight is measured to be 16.2 million.

[0051] Example 6

[0052] The method for preparing the fracturing fluid stock solution of this embodiment is the method for preparing the fracturing fluid stock solution of embodiment 3, comprising the following steps:

[0053] (1) First, acrylamide, a 50% by mass aqueous solution of sodium 2-acrylamide-2-methylpropane sulfonate and water are uniformly mixed to obtain solution A, then a molecular weight regulator and a metal ion removal agent are added to solution A, mixed uniformly to obtain solution B, and finally a pH regulator is added to solution B to adjust the pH value of solution B to be weakly acidic (pH=7.0) to obtain an aqueous phase; the mass fraction of acrylamide in the solution A is 35%, and the mass fraction of sodium 2-acrylamide-2-methylpropane sulfonate is 15%; the pH regulator is acrylic acid, the metal ion removal agent is disodium ethylenediaminetetraacetate, the mass fraction of the molecular weight regulator in the aqueous phase is 80 ppm, and the mass fraction of the metal ion removal agent in the aqueous phase is 200 ppm.

[0054] (2) Under nitrogen protection, the water phase and the oil phase are mixed and stirred at room temperature to emulsify until the viscosity of the mixed phase composed of the water phase and the oil phase is 800 mPa·s, and then the mixed phase is cooled to 20±3°C, and an initiator is added to the mixed phase (the initiator is composed of ammonium persulfate and sodium bisulfite, and the amount of ammonium persulfate and sodium bisulfite added is 8 ppm and 20 ppm of the mass of the water phase, respectively). Then, an inverse emulsion polymerization reaction is initiated at 20±3°C, and the temperature of the reaction system is controlled not to exceed 60°C. When the temperature of the reaction system no longer rises, excess sulfurous acid is added to the reaction system. The mixture is added with sodium bisulfite (the amount of sodium bisulfite added is 10ppm of the mass of the water phase) to react to remove a small amount of residual monomers, and then the system after the reaction is cooled to room temperature to obtain a fracturing fluid stock solution; the oil phase is composed of No. 7 white oil and Span 80, the mass ratio of No. 7 white oil to Span 80 is 10:1, and the mass ratio of the oil phase to the water phase is 3.2:6.8; the molecular weight of the polymer in the fracturing fluid stock solution prepared in this embodiment is measured according to the method of "GBT12005.10-1992 Polyacrylamide Molecular Weight Determination Viscosity Method", and the viscosity-average molecular weight is measured to be 17.9 million.

[0055] Comparative Example 1

[0056] The preparation method of the fracturing fluid stock solution of this comparative example is different from that of Example 5 only in that the polymerizable monomers in the solution A are composed of acrylamide and acrylic acid, the mass fraction of acrylamide in the solution A is 40%, the mass fraction of acrylic acid is 10%, the pH regulator used in the preparation process is sodium hydroxide, and the viscosity-average molecular weight of the polymer in the prepared fracturing fluid stock solution is 8.5 million.

[0057] Comparative Example 2

[0058] The preparation method of the fracturing fluid stock solution of this comparative example is different from that of Example 5 only in that the polymerizable monomers in the solution A are composed of acrylamide, sodium 2-acrylamide-2-methylpropane sulfonate and acrylic acid, the mass fraction of acrylamide in the solution A is 25%, the mass fraction of sodium 2-acrylamide-2-methylpropane sulfonate is 12.5%, and the mass fraction of acrylic acid is 12.5%. The pH regulator used in the preparation process is sodium hydroxide, and the viscosity-average molecular weight of the polymer in the prepared fracturing fluid stock solution is 11.8 million.

[0059] 3. Specific embodiments of the fracturing fluid of the present invention are as follows:

[0060] Example 7

[0061] The fracturing fluid of this embodiment is obtained by mixing the fracturing fluid stock solution prepared in Example 4 with tap water; the mass ratio of the fracturing fluid stock solution to tap water is 1:99, the viscosity of the high-viscosity fracturing fluid of this embodiment is 96.0 mPa·s, and the fracturing fluid of this embodiment is a high-viscosity fracturing fluid.

[0062] Example 8

[0063] The fracturing fluid of this embodiment is obtained by mixing the fracturing fluid stock solution prepared in Example 5 with tap water; the mass ratio of the fracturing fluid stock solution to tap water is 0.4:99.6. The fracturing fluid of this embodiment is a low-viscosity fracturing fluid.

[0064] Example 9

[0065] The fracturing fluid of this embodiment is obtained by mixing the fracturing fluid stock solution prepared in Example 6 with tap water; the mass ratio of the fracturing fluid stock solution to tap water is 0.9:99.1, and the fracturing fluid of this embodiment is a high-viscosity fracturing fluid.

[0066] Example 10

[0067] The fracturing fluid of this embodiment is obtained by mixing the fracturing fluid stock solution prepared in Example 6 with tap water; the mass ratio of the fracturing fluid stock solution to tap water is 1:99, and the fracturing fluid of this embodiment is a high-viscosity fracturing fluid.

[0068] Embodiment 11

[0069] The fracturing fluid of this embodiment is obtained by mixing the fracturing fluid stock solution prepared in Example 6 with tap water; the mass ratio of the fracturing fluid stock solution to tap water is 0.4:99.6. The fracturing fluid of this embodiment is a low-viscosity fracturing fluid.

[0070] Experimental example

[0071] 1. Temperature resistance

[0072] The high viscosity fracturing fluid of Example 7 was heated at 110°C and a rotation speed of 170s -1 Under the condition of shearing for 60 minutes, the rheological data were obtained. Figure 1 The results show that the viscosity of the prepared high-viscosity fracturing fluid is 62 mPa·s after 60 minutes of shearing, showing good temperature and shear resistance.

[0073] 2. Drag reduction rate

[0074] The drag reduction rate of the low-viscosity fracturing fluid of Example 8 was measured under the conditions of a pipe diameter of 8 mm and a flow rate of 10 m / s. The test results are as follows: Figure 2 The results show that the drag reduction rate of the prepared low-viscosity fracturing fluid after shearing for 300s is still greater than 70%, indicating that the low-viscosity fracturing fluid of Example 8 has good drag reduction performance and heat and shear resistance.

[0075] 3. Suspended sand

[0076] Add ceramsite with a particle size of 20-40 mesh (sand ratio of 30%) to the high-viscosity fracturing fluid of Example 9, stir evenly to obtain a suspended sand solution, and then transfer the suspended sand solution to a measuring cylinder and let it stand to observe the sedimentation of the ceramsite in the suspended sand solution. The results are as follows: Figure 3 The results show that after the suspended sand liquid was left to stand for 9 minutes, the ceramsite in the suspended sand liquid hardly sank, indicating that the high-viscosity fracturing fluid of Example 9 has good sand suspension performance.

[0077] 4. Dynamic suspended sand

[0078] The fracturing fluid prepared in Example 6 was used in the construction of a J30xx well in a gas field, and the construction fracturing curve obtained was as follows: Figure 4 As shown; Figure 4 In the figure, D represents the real-time operation displacement, E represents the real-time wellhead pressure, F represents the real-time sand concentration, and G represents the real-time casing pressure.

[0079] The construction parameters designed for the J30xx well are as follows: 300 m3 of low-viscosity fracturing fluid with a viscosity of 6 to 12 mPa·s 3 and high viscosity fracturing fluid 800m 3 , 20~40 mesh proppant 90m 3 The well depth is about 3600m, the number of perforations is 48, and the designed construction displacement is 8m 3 / min, the mineralization of the on-site water is 150-2500ppm.

[0080] It can be seen from the on-site real-time construction curve that the actual construction displacement on site is 8m 3 / min, the maximum wellhead pressure during construction was 50mPa·s, the maximum sand ratio of stage sand addition was 25%, and during the entire construction process, the low-viscosity fracturing fluid and high-viscosity fracturing fluid used were mixed with the fracturing fluid stock solution prepared in Example 6 and on-site water, and the construction displacement was always stable at 8m 3 / min, the construction pressure is stable, and the construction pressure has almost no obvious fluctuation when switching from low-viscosity fracturing fluid to high-viscosity fracturing fluid. The low-viscosity fracturing fluid and high-viscosity fracturing fluid prepared on the surface have good drag reduction effect, and the drag reduction rate changes little with viscosity; with the increase of sand concentration, it can be seen from the construction pressure curve E that the construction pressure has almost no fluctuation and is maintained at about 40mPa·s as a whole, indicating that the high-viscosity fracturing fluid prepared from the fracturing fluid stock solution prepared in Example 6 has good dynamic sand suspension; it can be seen from the entire construction curve that the low-viscosity fracturing fluid with a viscosity of 6 to 12mPa·s is used in the early stage of the construction to create fractures in the formation, forming The relatively complex formation cracks with a certain width provide a good channel for the later high-viscosity fracturing fluid to add sand, which effectively ensures that the maximum amount of sand can be added under the condition of lower fluid usage. Changing the proportion of the fracturing fluid stock at any time during the construction process can not only save the dosage and reduce the cost, but also help to extend the extension of the formation cracks and increase the width of the cracks, maximize the formation transformation, form a complex network, and create a favorable channel for oil and gas outflow; therefore, the fracturing fluid stock prepared in Example 6 has excellent variable viscosity performance, can well meet the construction requirements, and can change the liquid properties in real time without the need for advance liquid preparation.

[0081] 5. Salt tolerance

[0082] The fracturing fluid stock solution prepared in Example 5 was added to different water qualities in different proportions, and the apparent viscosity at different dissolution times was tested according to "SY-T 5107-2005 Water-based Fracturing Fluid Performance Evaluation Method", and the experimental results are shown in Table 1. The results show that the fracturing fluid stock solution prepared in Example 5 has good viscosity and viscosity-increasing properties in different water qualities, and exhibits good salt resistance, and is suitable for various complex water qualities.

[0083] Table 1. Viscosity and viscosity enhancement properties of the fracturing fluid prepared in Example 5 in different water qualities

[0084]

[0085] The fracturing fluid stock solution prepared in Example 4 was added to different water qualities in different proportions to obtain fracturing fluid, and then the viscosity of the fracturing fluid stock solution was measured when it was dissolved for 5 minutes according to the method of "SY-T 5107-2005 Water-based fracturing fluid performance evaluation method", and then the drag reduction rate of the low-viscosity fracturing fluid (concentration not more than 0.15%) under the conditions of 8mm pipe diameter and 10m / s flow rate was measured according to "NBT14003.2-2016 Drag reduction agent performance index and test method", and the test results are shown in Table 2. The results show that under different concentrations and different water qualities, the low-viscosity fracturing fluid (concentration not more than 0.15%) prepared by the fracturing fluid stock solution prepared in Example 4 has a good drag reduction rate, and when the concentration of the fracturing fluid stock solution prepared in Example 4 in 40,000 high-mineralization salt water is 0.1%, the obtained fracturing fluid still has a good drag reduction performance and exhibits a good salt resistance.

[0086] Table 2 Viscosity and drag reduction rate of fracturing fluid prepared by mixing the fracturing fluid stock solution prepared in Example 4 with different water qualities

[0087]

[0088]

[0089] The fracturing fluid stock solution prepared in Example 5 was added to different water qualities in different proportions to obtain fracturing fluids, and then the viscosity of the fracturing fluid stock solution after dissolution for 5 minutes was determined according to the method of "SY-T 5107-2005 Water-based fracturing fluid performance evaluation method", and then the drag reduction rate of low-viscosity fracturing fluid (concentration not more than 0.15%) under the conditions of 8 mm pipe diameter and 10 m / s flow rate was determined according to "NBT14003.2-2016 Drag Reducing Agent Performance Index and Test Method". The test results are shown in Table 3. The results show that under different concentrations and different water quality conditions, the low-viscosity fracturing fluid (concentration not greater than 0.15%) prepared from the fracturing fluid stock solution prepared in Example 5 has a good drag reduction rate; when the concentration of the fracturing fluid stock solution prepared in Example 5 in tap water is 0.05%, the drag reduction rate of the obtained fracturing fluid is greater than 70%, and when the concentration is 0.1%, the drag reduction rate of the obtained fracturing fluid is as high as 74%; when the concentration of the fracturing fluid stock solution prepared in Example 5 in 40,000 high-mineralization salt water is 0.1%, the drag reduction rate of the obtained fracturing fluid is greater than 70%. Therefore, whether the fracturing fluid stock solution prepared in Example 5 is in tap water or high-mineralization salt water, the obtained low-viscosity fracturing fluid has good drag reduction performance and exhibits good salt resistance.

[0090] Table 3 Viscosity and drag reduction rate of fracturing fluids prepared by mixing the fracturing fluid stock solution prepared in Example 5 with different water qualities

[0091]

[0092]

[0093] The fracturing fluid stock solution prepared in Example 6 was added to different water qualities in different proportions to obtain fracturing fluid, and then the viscosity of the fracturing fluid stock solution was measured when it was dissolved for 5 minutes according to the method of "SY-T 5107-2005 Water-based fracturing fluid performance evaluation method", and then the drag reduction rate of the fracturing fluid under the conditions of 8mm pipe diameter and 10m / s flow rate was measured according to "NBT14003.2-2016 Drag reduction agent performance index and test method", and the test results are shown in Table 4. The results show that when the concentration of the fracturing fluid stock solution prepared in Example 6 in tap water is 0.4%, the drag reduction rate of the obtained fracturing fluid is greater than 70%, indicating that the fracturing fluid with a viscosity of 12 to 30mPa·s still has good drag reduction performance, when the concentration is greater than 0.8%, the obtained fracturing fluid still has a good drag reduction rate, and when the viscosity of the fracturing fluid is greater than 51mPa·s, the drag reduction rate is still above 60%, showing good drag reduction performance. Under different concentrations and different water qualities, the fracturing fluid prepared from the fracturing fluid stock solution prepared in Example 6 has a very good drag reduction rate and exhibits very good salt resistance.

[0094] Table 4 Viscosity and drag reduction rate of fracturing fluid prepared by mixing the fracturing fluid stock solution prepared in Example 6 with different water qualities

[0095]

[0096] The fracturing fluid stock solutions of Comparative Example 1 and Comparative Example 2 were added to different water qualities in different proportions to obtain fracturing fluids, and then the viscosity of the fracturing fluid stock solution when dissolved for 5 minutes was determined according to the method of "SY-T 5107-2005 Water-based fracturing fluid performance evaluation method", and then the drag reduction rate of the fracturing fluid under the conditions of 8 mm pipe diameter and 10 m / s flow rate was determined according to "NBT14003.2-2016 Drag reduction agent performance indicators and test methods". The test results are shown in Tables 5 and 6. The results show that the fracturing fluid stock solution of Comparative Example 1 cannot dissolve in high-mineralization brine and cannot become sticky, and the viscosity-average molecular weight of the polymer in the fracturing fluid stock solution of Comparative Example 1 is much smaller than the viscosity-average molecular weight of the polymer in the fracturing fluid stock solution prepared by the embodiment of the present invention, indicating that the fracturing fluid stock solution prepared by the embodiment has good salt resistance, stickiness and high molecular weight; although the fracturing fluid stock solution of Comparative Example 2 can become sticky and dissolved in brine, compared with the fracturing fluid stock solution prepared by Example 5, under the conditions of the same water quality and the same concentration, the viscosity and drag reduction rate of the fracturing fluid prepared by the fracturing fluid stock solution of Comparative Example 2 are lower, indicating that the fracturing fluid stock solution prepared by the embodiment has excellent performance.

[0097] Table 5 Viscosity and drag reduction rate of fracturing fluids prepared by mixing the fracturing fluid stock solution of Comparative Example 1 with different water qualities

[0098]

[0099] Table 6 Viscosity and drag reduction rate of fracturing fluids prepared by mixing the fracturing fluid stock solution of Comparative Example 2 with different water qualities

[0100]

[0101]

Claims

1. A fracturing fluid concentrate, characterized in that: The invention is mainly obtained by reverse emulsion polymerization of water phase and oil phase; the water phase is mainly composed of molecular weight regulator, metal ion remover, pH regulator, acrylamide, sodium 2-acrylamide-2-methylpropane sulfonate and water; based on the total mass of acrylamide, sodium 2-acrylamide-2-methylpropane sulfonate and water as 100 parts, the mass of acrylamide is 35-40 parts, and the mass of sodium 2-acrylamide-2-methylpropane sulfonate is 10-15 parts; the pH value of the water phase is 6.8-7.0; the viscosity average molecular weight of the polymer in the fracturing fluid stock solution is 15 million-18 million; the pH regulator is acrylic acid.

2. The fracturing fluid stock solution according to claim 1, characterized in that: The molecular weight regulator is a composite molecular weight regulator and / or sodium hypophosphite monohydrate; the composite molecular weight regulator is composed of sodium formate and urea; the mass ratio of sodium formate to urea is 2:1; the mass fraction of the molecular weight regulator in the aqueous phase is 60-80 ppm.

3. The fracturing fluid stock solution according to claim 1, characterized in that: The metal ion removing agent is a metal chelating agent; the metal chelating agent is diethylenetriaminepentaacetic acid sodium salt and / or ethylenediaminetetraacetic acid sodium salt.

4. The fracturing fluid stock solution according to claim 1, characterized in that: The mass fraction of the metal ion removal agent in the water phase is 150-200 ppm.

5. The fracturing fluid stock solution according to claim 1, characterized in that: The oil phase is mainly composed of white oil and emulsifier; the HLB value of the emulsifier is 4-8.

6. The fracturing fluid stock solution according to any one of claims 1 to 5, characterized in that: The mass ratio of the water phase to the oil phase is 6.8:3.

2.

7. The method for preparing a fracturing fluid stock solution according to any one of claims 1 to 6, characterized in that: The following steps are involved: Firstly, the water phase and the oil phase are mixed and emulsified to obtain a mixed phase, and then an initiator is added to the mixed phase under an inert atmosphere, and then an inverse emulsion polymerization is carried out.

8. The method for preparing a fracturing fluid stock solution according to claim 7, characterized in that: The viscosity of the mixed phase is 600-800 mPa·s.

9. A fracturing fluid, characterized in that: The fracturing fluid is mainly obtained by mixing the fracturing fluid stock solution according to any one of claims 1 to 6 and water.