Magnesium-based composite material, preparation method thereof, and electronic device
By adding Zn, Ca and other elements and reinforcements to the magnesium alloy matrix, combined with stir casting and hot extrusion processes, magnesium-based composite materials with high thermal conductivity, high strength and toughness, and high modulus are prepared, which solves the problem of insufficient performance of magnesium alloys. , achieving low-cost and high-quality preparation and meeting the application needs of the 3C industry.
Patent Information
- Application Number
- CN202111267083.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-28
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-10-28
AI Technical Summary
Due to insufficient stiffness, strength and thermal conductivity of existing magnesium alloys in 3C industry applications, it is difficult to meet the needs of large-screen, thinner, integrated and high-power battery products. Moreover, the preparation process of traditional magnesium-based composite materials is high in cost and quality. Low and difficult to achieve large-scale application.
Zn, Ca and other elements are added to the magnesium alloy matrix formula, combined with reinforcements such as SiC particles and carbon fibers, and magnesium-based composite materials are prepared through stirring casting and hot extrusion processes to optimize the interface combination between the matrix and reinforcements and improve the thermal conductivity and toughness and modulus properties, and control process conditions to achieve low-cost, high-quality preparation.
It achieves the comprehensive properties of high thermal conductivity, high strength, toughness and high modulus of magnesium-based composite materials, reduces preparation costs, meets the application needs of end products, and provides better molding processing performance and weight reduction effects.
Smart Images

Figure CN116043085B_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the present application relate to the technical field of composite material preparation, and in particular to a magnesium-based composite material, a preparation method thereof, and an electronic device. Background Art
[0002] Magnesium alloy is the lightest metal structural material, and has broad application prospects in the 3C industry and the automotive industry. At present, with the development of 5G communication technology, higher structural and functional integration requirements are put forward for lightweight structural materials, but traditional magnesium alloys have low strength (modulus is only 43GPa), low strength (yield strength is generally less than 200MPa), and insufficient thermal conductivity (thermal conductivity is less than 70W / mK), which limits their application in new 3C products with large screens, thin and light, integrated, and high-power batteries.
[0003] Alloying and composite are effective ways to improve the comprehensive performance of magnesium alloys. By adding high modulus and high thermal conductivity reinforcements to the magnesium alloy matrix, a beneficial strengthening effect can be produced to obtain magnesium-based composite materials with ideal performance. However, traditional magnesium-based composite materials generally use traditional alloy matrices such as pure Mg and AZ91, and the modulus, thermal conductivity and ductility are mismatched, and the coordination of reinforcements and preparation processes is generally unable to achieve large-scale application. Therefore, it is urgent to develop new magnesium-based composite materials that can meet the requirements of high thermal conductivity, high toughness and high modulus performance, while having a low-cost and high-quality preparation process. Summary of the invention
[0004] In view of this, an embodiment of the present application provides a magnesium-based composite material, a preparation method thereof, and an electronic device. The magnesium-based composite material has excellent comprehensive properties of high thermal conductivity, high strength and high modulus, and can be prepared at low cost.
[0005] Specifically, a first aspect of an embodiment of the present application provides a magnesium-based composite material, which includes a magnesium alloy matrix and a reinforcement distributed in the magnesium alloy matrix. Based on 100% by weight of the magnesium alloy matrix, the magnesium alloy matrix includes the following components in percentage by weight: Zn 4%-7%, Ca 0.05%-0.8%, Al 0-4%, Zr 0-1%, Ce0-0.8%, La 0-0.8%, Y 0-0.8%, Nd 0-0.8%, Si 0-0.8%, Mn 0-1.5%, Sr 0-0.5%, Sn0-1%, Sc 0-0.5%, Gd 0-0.8%, and the balance is Mg and unavoidable impurity elements.
[0006] The magnesium-based composite material provided in the present application can have the comprehensive properties of high thermal conductivity, high strength and high modulus by adopting the above-mentioned specific formula, and can be prepared at low cost, with high process feasibility, and can meet the application requirements of terminal products. Specifically, it can be used to process and form terminal product structural parts, such as middle frame, back cover, etc. Among them, the magnesium-based composite material in the embodiment of the present application takes Mg-Zn as the main system, and by controlling the appropriate Zn content, the Mg-Zn system can have a wider semi-solid process window range, ensuring that it can be prepared by a stirring casting process with a short processing flow and low cost, and can maintain better thermal conductivity and elongation performance; and the introduction of an appropriate amount of Ca can improve the interface bonding ability between the magnesium alloy matrix and the external reinforcement, thereby improving the toughness, ductility and other mechanical properties of the magnesium-based composite material.
[0007] In the implementation manner of the present application, the weight percentage of Zn in the magnesium alloy matrix is 4.5%-6%.
[0008] In the implementation manner of the present application, the weight percentage of Ca in the magnesium alloy matrix is 0.1%-0.5%.
[0009] In the implementation manner of the present application, the weight percentage of Ca in the magnesium alloy matrix is 0.2%-0.4%.
[0010] In the implementation manner of the present application, the weight percentage of Al in the magnesium alloy matrix is 0.2%-2%.
[0011] In the implementation manner of the present application, the weight percentage of Zr in the magnesium alloy matrix is 0.2%-0.4%.
[0012] In the implementation manner of the present application, the weight percentage of Ce in the magnesium alloy matrix is 0.1%-0.4%.
[0013] In the implementation manner of the present application, the weight percentage of La in the magnesium alloy matrix is 0.1%-0.4%.
[0014] In the implementation manner of the present application, the weight percentage of Y in the magnesium alloy matrix is 0.05%-0.4%.
[0015] In an embodiment of the present application, in the magnesium alloy matrix, the total weight percentage of Ca, Zr, Ce, La, Y, Nd, Si, Mn, Sr, Sn, Sc, and Gd is less than or equal to 2%.
[0016] In an embodiment of the present application, in the magnesium alloy matrix, the total weight percentage of Ca, Zr, Ce, La, Y, Nd, Si, Mn, Sr, Sn, Sc, and Gd is greater than or equal to 0.15% and less than or equal to 2%.
[0017] In the embodiment of the present application, the weight percentage of the inevitable impurity elements in the magnesium alloy matrix does not exceed 0.1%. The less the inevitable impurity content, the more conducive it is to obtain a magnesium-based composite material with the desired performance.
[0018] In the embodiment of the present application, in the magnesium-based composite material, the volume percentage of the reinforcement is 1%-20%. The addition of a high modulus and high thermal conductivity reinforcement in the magnesium-based composite material can produce a beneficial strengthening effect and improve the performance of the magnesium-based composite material. Controlling the volume percentage of the reinforcement within the above range can obtain better molding and processing performance and better avoid the generation of material cracks.
[0019] In the embodiment of the present application, the reinforcement includes reinforcement particles and / or reinforcement fibers.
[0020] In the embodiment of the present application, the reinforcing particles include SiC, B 4 C. SiO 2 、ZrO 2 、Si 3 N 4 、AlN、BN、Al 2 O 3 、TiC、TiB 2 , diamond, graphite, graphene, one or more of carbon nanotubes; the reinforcing fiber includes carbon fiber.
[0021] In the embodiment of the present application, the size of the reinforcing particles is less than or equal to 50 μm; the reinforcing fibers are chopped fibers, and the chopped length is less than or equal to 2 mm. Controlling the size of the reinforcement within the above-mentioned suitable range can obtain better molding and processing performance, which is conducive to ensuring that the magnesium-based composite material has both good strengthening effect and good extrusion processability.
[0022] In the embodiment of the present application, the reinforcement further comprises an additional layer disposed on the surface of the reinforcement particles and / or reinforcement fibers, and the additional layer comprises one or more of magnesium oxide, silicon dioxide, titanium dioxide, titanium and its alloys, copper and its alloys, zirconium and its alloys, titanium nitride, and silicon carbide. The additional layer can further enhance the bonding force between the reinforcement and the magnesium alloy matrix, thereby enhancing the mechanical properties of the magnesium-based composite material.
[0023] In the implementation manner of the present application, the thermal conductivity of the magnesium-based composite material is 90W / mK-130W / mK, the yield strength is ≥200Mpa, the tensile strength is ≥250MPa, the elongation is ≥3%, and the elastic modulus is 45Gpa-70Gpa.
[0024] A second aspect of the embodiment of the present application provides a method for preparing a magnesium-based composite material, comprising the following steps:
[0025] Obtaining a magnesium alloy matrix melt by smelting, and adjusting the temperature of the magnesium alloy matrix melt to a semi-solid temperature range to obtain a semi-solid melt;
[0026] The semi-solid melt is subjected to vortex stirring, a preheated reinforcement is added to the center of the vortex, the mixture is continuously stirred and heated to a temperature above the liquidus temperature, and then cast to obtain a magnesium-based composite material ingot;
[0027] The magnesium-based composite material ingot is hot extruded or rolled into shape, and then subjected to heat treatment to obtain the magnesium-based composite material.
[0028] A third aspect of an embodiment of the present application provides a structural component, wherein the structural component is prepared by using the magnesium-based composite material described in the first aspect of the present application.
[0029] A fourth aspect of an embodiment of the present application provides a shell, wherein the shell is prepared by using the magnesium-based composite material described in the first aspect of the present application.
[0030] An embodiment of the present application provides an electronic device, comprising a housing and a mainboard located inside the housing, wherein the housing is wholly or partially the shell as described in the fourth aspect of the embodiment of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 A schematic diagram of the structure of a housing provided in an embodiment of the present application;
[0032] Figure 2 A schematic diagram of the structure of an electronic device provided in an embodiment of the present application;
[0033] Figure 3 A schematic diagram of the structure of the front cover, middle frame and back cover of a mobile phone provided in an embodiment of the present application;
[0034] Figure 4 This is a scanning electron microscope (SEM) image of the magnesium-based composite material of Example 1 of the present application;
[0035] Figure 5 This is an XCT (X-ray computed tomography) image of the magnesium-based composite material of Example 1 of the present application;
[0036] Figure 6 This is a scanning electron microscope image of the magnesium-based composite material of Example 2 of the present application;
[0037] Figure 7 This is a scanning electron microscope image of the magnesium-based composite material of Example 3 of the present application;
[0038] Figure 8This is a transmission electron microscope (TEM) image of the magnesium-based composite material of Example 3 of the present application;
[0039] Fig. 9 This is the metallographic structure diagram of the magnesium-based composite material plate obtained in Example 4;
[0040] Fig.10 This is the metallographic structure diagram of the magnesium-based composite material plate obtained in Example 5;
[0041] Fig.11 This is the metallographic structure diagram of the magnesium-based composite material plate obtained in Example 6;
[0042] Fig.12 This is the metallographic structure diagram of the magnesium-based composite material plate obtained in Example 7;
[0043] Fig.13 This is the metallographic structure diagram of the magnesium-based composite material plate obtained in Example 8. DETAILED DESCRIPTION
[0044] The embodiments of the present application will be described below in conjunction with the drawings in the embodiments of the present application.
[0045] At present, it is difficult for existing magnesium-based composite materials to have the comprehensive properties of high thermal conductivity, high toughness and high modulus, and it is impossible to achieve low-cost, high-quality and continuous preparation, which limits its wide application in electronic devices. In order to obtain magnesium-based composite materials with excellent comprehensive performance and achieve low-cost and high-quality preparation, the inventors of this application have conducted design research from multiple angles such as magnesium alloy matrix formula, reinforcement phase formula, preparation process, interface bonding, etc., and provided a magnesium-based composite material.
[0046] The magnesium-based composite material provided in the embodiment of the present application includes a magnesium alloy matrix and a reinforcement distributed in the magnesium alloy matrix. Based on 100% weight of the magnesium alloy matrix, the magnesium alloy matrix includes the following components in weight percentage: Zn 4%-7%, Ca 0.05%-0.8%, Al 0-4%, Zr 0-1%, Ce 0-0.8%, La 0-0.8%, Y 0-0.8%, Nd 0-0.8%, Si 0-0.8%, Mn 0-1.5%, Sr 0-0.5%, Sn 0-1%, Sc 0-0.5%, Gd 0-0.8%, and the balance is Mg and unavoidable impurity elements. The sum of the weight percentages of the components of the magnesium alloy matrix is 100%.
[0047] The magnesium-based composite material provided in the present application can have the comprehensive properties of high thermal conductivity, high strength and high modulus by adopting the above-mentioned specific formula, and can be prepared at low cost, with high process feasibility, and can meet the application requirements of terminal products. Specifically, it can be used to process and form terminal product structural parts, such as middle frame, back cover, etc. Among them, the magnesium-based composite material in the embodiment of the present application takes Mg-Zn as the main system, and by controlling the appropriate Zn content, the Mg-Zn system can have a wider semi-solid process window range, ensuring that it can be prepared by a stirring casting process with a short processing flow and low cost, and can maintain better thermal conductivity and elongation performance; and the introduction of an appropriate amount of Ca can improve the interface bonding ability between the magnesium alloy matrix and the external reinforcement, thereby improving the toughness, ductility and other mechanical properties of the magnesium-based composite material.
[0048] In order to obtain a magnesium-based composite material with a short processing flow and low cost, the preparation process selected in this application is a stirring casting scheme. In order to achieve the best processing and dispersion effect, the addition and stirring of the reinforcement body is selected in the semi-solid state of the magnesium alloy matrix, which requires the magnesium alloy matrix to have a wide semi-solid process temperature window range. The inventor has explored and determined the Mg-Al and Mg-Zn systems through a large amount of experimental data. Table 1 is a comparison of the semi-solid intervals of magnesium alloys with Mg-xAl and Mg-xZn (x is the weight percentage) formulas calculated by material thermodynamics software for the solidification path of Mg-Al and Mg-Zn alloy formulas from liquid solidification to solid phase.
[0049] Table 1 Semi-solid range of magnesium alloys with Mg-xAl and Mg-xZn formulas
[0050]
[0051]
[0052] It can be seen from Table 1 that when the Al and Zn contents are too low (≤3%), the semi-solid processing window is too small, which is not conducive to the realization of the stirring casting process. In order to better realize the stirring casting process, Mg-xAl, Mg-xZn (x≥4%) systems can be selected as alternatives.
[0053] Since the external reinforcement is a hard and brittle phase, in order to ensure the high ductility and high thermal conductivity of the magnesium alloy matrix and the external reinforcement after composite, a series of comprehensive evaluations of mechanical properties and thermal conductivity of the alloying elements in the magnesium alloy formula are carried out. Table 2 shows the mechanical properties and thermal conductivity results of magnesium alloys with Mg-xAl and Mg-xZn formulas.
[0054] Table 2 Mechanical properties and thermal conductivity results of magnesium alloys with Mg-xAl and Mg-xZn formulas
[0055] Main alloy element formula Thermal conductivity W / (m·K) Yield strength MPa Elongation % Mg-4%Al 68 124 14.3 Mg-5%Al 60 141 12 Mg-4%Zn 121 135 16.2 Mg-6%Zn 113 150 15 Mg-7%Zn 110 156 13.6 Mg-8%Zn 102 160 9.5
[0056] It can be seen from Table 2 that selecting Mg-xZn (4%≤x≤7%) as the main component element of the magnesium alloy matrix can ensure that excellent thermal conductivity and mechanical properties are obtained while obtaining a wider semi-solid process window.
[0057] Since the interface bonding between the magnesium alloy matrix and the external reinforcement will also affect the performance of the final magnesium-based composite material, in order to promote the interface bonding, the Ca element is introduced into the magnesium-based composite material of the embodiment of the present application, and the adhesion work of the Ca element and the external reinforcement is calculated by software simulation using the first principle, and the adhesion work of the Ca element is obtained to be 0.7461 J·m -2 , relative to the interfacial adhesion work of Mg element and external reinforcement 0.2216 J·m -2 , and the interfacial adhesion work between Zn element and external reinforcement is 0.2490 J·m -2 The introduction of Ca element can greatly improve the bonding of composite interface, which is beneficial to improve the mechanical properties of composite materials. In addition, Ca and Zn elements tend to co-segregate at the grain boundary of magnesium alloy. This co-segregation leads to a weaker extrusion texture. During the deformation process, it can promote the plastic deformation of grain boundary, making the alloy have good deformation ability, thus ensuring the strength and toughness of the composite material.
[0058] In the embodiment of the present application, the weight percentage of Zn in the magnesium alloy matrix can be, but is not limited to, 4%, 4.2%, 4.5%, 4.8%, 5%, 5.2%, 5.5%, 5.8%, 6%, 6.2%, 6.5%, 6.8%, 7%. In some embodiments, the weight percentage of Zn can be 4.5%-6%.
[0059] In the implementation manner of the present application, the weight percentage of Ca in the magnesium alloy matrix can be, but is not limited to, 0.05%, 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.45%, 0.5%, 0.55%, 0.6%, 0.65%, 0.7%, 0.75%, 0.8%. In some embodiments, the weight percentage of Ca can be 0.1%-0.5%. In other embodiments, the weight percentage of Ca can be 0.2%-0.4%.
[0060] In the embodiments of the present application, in the magnesium alloy matrix, the weight percentage of Al, Zr, Ce, La, Y, Nd, Si, Mn, Sr, Sn, Sc, and Gd can all be 0. In some embodiments of the present application, the magnesium alloy matrix includes Zn 4%-7%, Ca 0.05%-0.8%, and the balance is Mg and inevitable impurity elements; that is, in this embodiment, the total weight percentage of Mg, Zn, Ca and inevitable impurity elements is 100%.
[0061] In some embodiments of the present application, in order to further enhance the comprehensive performance of magnesium-based composite materials, a small amount of Al, Zr, Ce, La, Y, Nd, Si, Mn, Sr, Sn, Sc, Gd and other elements may be further added. These elements can refine the grains, remove oxygen and impurities, improve the melt quality, enhance the interface bonding between the magnesium alloy matrix phase and the reinforcement phase, and enhance the mechanical properties of the material. For example, through simulation calculation, the interface adhesion work of Al element and the added reinforcement is 0.2537 J·m -2 The interface adhesion work between Mn element and external reinforcement is 0.6953 J·m -2 The interfacial adhesion work between La element and external reinforcement is 0.8031 J·m -2 The interface adhesion work between Ce element and external reinforcement is 1.5108 J·m -2 In addition, Zr and Sr elements have the effect of effectively refining the grains of magnesium alloys. Zr can form Mg 3 Zr phase produces heterogeneous nucleation, which plays a role in grain refinement; while Sr element is enriched at the solidification growth front, inhibiting the growth of grains, thus also providing a good grain refinement effect for magnesium alloys. Sn and Si elements can form Mg in magnesium 2 Sn and Mg 2 The second phase of Si has a strengthening effect on the magnesium alloy matrix. Rare earth elements such as Y, Nd, Sc, and Gd have a large solid solubility in magnesium alloys and have a good micro-alloying solid solution strengthening effect. The trace composite addition of the above elements can better ensure the high strength and toughness of the magnesium alloy matrix.
[0062] In some embodiments of the present application, the weight percentage of Al in the magnesium alloy matrix may be, but is not limited to, 0.1%, 0.2%, 0.5%, 1.0%, 1.5%, 2.0%, 2.5%, 3.0%, 3.5%, 4.0%. In some embodiments, the weight percentage of Al may be 0.2%-2%.
[0063] In some embodiments of the present application, the weight percentage of Zr in the magnesium alloy matrix may be, but is not limited to, 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%. In some embodiments, the weight percentage of Ca may be 0.2%-0.4%.
[0064] In some embodiments of the present application, the weight percentage of Ce in the magnesium alloy matrix may be, but is not limited to, 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%. In some embodiments, the weight percentage of Ce may be 0.1%-0.4%.
[0065] In some embodiments of the present application, the weight percentage of La in the magnesium alloy matrix may be, but is not limited to, 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%. In some embodiments, the weight percentage of La may be 0.1%-0.4%.
[0066] In some embodiments of the present application, the weight percentage of Y in the magnesium alloy matrix may be, but is not limited to, 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%. In some embodiments, the weight percentage of Y may be 0.05%-0.4%.
[0067] In some embodiments of the present application, the weight percentage of Nd in the magnesium alloy matrix can be specifically 0.2%-0.4%. In some embodiments of the present application, the weight percentage of Si in the magnesium alloy matrix can be specifically 0.2%-0.4%. In some embodiments of the present application, the weight percentage of Mn in the magnesium alloy matrix can be specifically 0.2%-1.0%. In some embodiments of the present application, the weight percentage of Sr in the magnesium alloy matrix can be specifically 0.1%-0.3%. In some embodiments of the present application, the weight percentage of Sn in the magnesium alloy matrix can be specifically 0.2%-0.5%. In some embodiments of the present application, the weight percentage of Sc in the magnesium alloy matrix can be specifically 0.1%-0.3%. In some embodiments of the present application, the weight percentage of Gd in the magnesium alloy matrix can be specifically 0.2%-0.4%.
[0068] In the embodiments of the present application, in the magnesium alloy matrix, the total weight percentage of Ca, Zr, Ce, La, Y, Nd, Si, Mn, Sr, Sn, Sc, and Gd may be less than or equal to 2%. In some embodiments of the present application, the total weight percentage of Ca, Zr, Ce, La, Y, Nd, Si, Mn, Sr, Sn, Sc, and Gd may be greater than or equal to 0.15% and less than or equal to 2%. Among them, controlling the total content of the above elements to ≥0.15% can better ensure the alloying degree of the matrix alloy, improve the basic strength of the alloy, and the interface bonding effect with the added reinforcement phase. Controlling the total content of the above elements to ≤2% can better avoid the mismatch between the strength and thermal conductivity of the magnesium-based composite material, while avoiding unnecessary cost increases in the alloy formula.
[0069] In the embodiment of the present application, in order to ensure the performance of the magnesium-based composite material, the weight percentage of the inevitable impurity elements in the magnesium alloy matrix can be controlled to be no more than 0.1%. In some embodiments, the weight percentage of the inevitable impurity elements can be controlled to be no more than 0.05%. The less the inevitable impurity content, the more conducive it is to obtain a magnesium-based composite material with the desired performance.
[0070] In the embodiment of the present application, the addition of a high modulus and high thermal conductivity reinforcement in the magnesium-based composite material can produce a beneficial strengthening effect and improve the performance of the magnesium-based composite material. In the embodiment of the present application, in the magnesium-based composite material, the volume percentage of the reinforcement can be 1%-20%. Specifically, the volume percentage of the reinforcement can be but is not limited to 1%, 3%, 5%, 7%, 8%, 10%, 12%, 13%, 15%, 18%, 20%. The addition amount of the reinforcement is controlled within the above range, which can better play the high modulus transfer effect of the reinforcement phase and improve the final elastic modulus of the magnesium-based composite material; at the same time, due to the brittleness of the reinforcement itself, it may cause a significant decrease in the elongation of the magnesium-based composite material, thereby causing cracks in the corresponding structural shell during processing, or brittle fracture failure during the use of the whole machine. Controlling the volume percentage of the reinforcement to ≤20% is conducive to the magnesium-based composite material to obtain a higher elongation.
[0071] In the embodiment of the present application, the reinforcement may include reinforcement particles and / or reinforcement fibers. The reinforcement particles include SiC, B 4 C. SiO 2 、ZrO 2 、Si 3 N 4 、AlN、BN、Al 2 O 3 、TiC、TiB 2, diamond, graphite, graphene, carbon nanotubes. The reinforcing fiber may include carbon fiber. In some embodiments of the present application, the reinforcement may include only reinforcing particles; in some embodiments, the reinforcement may include only reinforcing fibers; in some embodiments, the reinforcement may also include both reinforcing particles and reinforcing fibers. Among them, the specific shape of the reinforcing particles is not limited, and may be powder, spherical, quasi-spherical, tubular, flake, irregular, etc. In the embodiment of the present application, the size of the reinforcing particles may be less than or equal to 50μm. In some embodiments, the size of the reinforcing particles may be 1μm-30μm. Specifically, in some embodiments, the size of the reinforcing particles may be, for example, 1μm, 5μm, 10μm, 15μm, 20μm, 25μm, 30μm, 35μm, 40μm, 50μm. In the embodiment of the present application, the reinforcing fibers are chopped fibers, and the chopped length is less than or equal to 2mm. Specifically, in some embodiments, the length of the chopped fibers may be, for example, 0.5mm, 1mm, 1.5mm, 2mm.
[0072] In the process of preparing magnesium-based composite materials, the presence of reinforcements generally increases friction, thereby exacerbating the unevenness of alloy flow and easily leading to periodic cracks in the material. In order to obtain better forming and processing performance, the embodiment of the present application controls the size of the reinforcement to a reinforcement particle size of less than or equal to 50 μm, a reinforcement fiber length of less than or equal to 2 mm, and a volume content of no more than 20%, which is conducive to ensuring that the magnesium-based composite material has both good strengthening effect and good extrusion processability.
[0073] In order to better improve the bonding force between the reinforcement and the magnesium alloy matrix, and thus improve the mechanical properties of the magnesium-based composite material, in some embodiments of the present application, the reinforcement may also include an additional layer disposed on the surface of the reinforcement particles and / or reinforcement fibers, and the additional layer may include one or more of magnesium oxide, silicon dioxide, titanium dioxide, titanium and its alloys, copper and its alloys, zirconium and its alloys, titanium nitride, and silicon carbide. The additional layer may be prepared by coating or by plating, that is, the additional layer may be a coating or plating formed by the above materials.
[0074] In the implementation mode of the present application, the thermal conductivity of the magnesium-based composite material is 90W / mK-130W / mK, the yield strength is ≥200Mpa, the tensile strength is ≥250MPa, the elongation is ≥3%, and the elastic modulus is 45Gpa-70Gpa. In some embodiments, the thermal conductivity of the magnesium-based composite material can be, for example, 90W / mK, 95W / mK, 100W / mK, 105W / mK, 110W / mK, 115W / mK, 120W / mK, 125W / mK, 130W / mK, etc. In some embodiments, the yield strength of the magnesium-based composite material can be, for example, 200Mpa, 210Mpa, 220Mpa, 230Mpa, 250Mpa, 280Mpa, 300Mpa, etc. In some embodiments, the yield strength of the magnesium-based composite material is ≥220Mpa. In some embodiments, the tensile strength of the magnesium-based composite material can be, for example, 250Mpa, 260Mpa, 270Mpa, 280Mpa, 290Mpa, 300Mpa, 310Mpa, etc. In some embodiments, the elongation of the magnesium-based composite material can be, for example, 3%, 4%, 4.5%, 5%, 6%. In some embodiments, the elongation of the magnesium-based composite material is 3%-6%. In some embodiments, the elastic modulus of the magnesium-based composite material can be, for example, 45Gpa, 48Gpa, 50Gpa, 52Gpa, 55Gpa, 58Gpa, 60Gpa, 65Gpa, 66Gpa, 68Gpa, 70Gpa. In the embodiment of the present application, the density of the magnesium-based composite material is 1.8g / cm 3 -2.0g / cm 3 The magnesium-based composite material provided in the embodiment of the present application has excellent comprehensive performance. The plate made of the magnesium-based composite material can be used as the raw material of the terminal shell, and can be processed into a middle frame or back cover of a specified structural size (such as a mobile phone middle frame, an ACD shell of a laptop computer, a middle frame or back cover of a tablet computer, a watch case, etc.) by CNC (Computerized Nμmerical Control). Compared with the currently used aluminum alloy or general magnesium alloy, magnesium-aluminum alloy solutions, the terminal shell prepared by the magnesium-based composite material of the embodiment of the present application has higher structural rigidity and can also achieve a weight reduction effect.
[0075] The present invention also provides a method for preparing a magnesium-based composite material, comprising the following steps:
[0076] Step S101, obtaining a magnesium alloy matrix melt by smelting, and adjusting the temperature of the magnesium alloy matrix melt to a semi-solid temperature range to obtain a semi-solid melt;
[0077] Specifically, raw materials may be prepared according to the designed ratio of the magnesium alloy matrix and smelted to obtain a magnesium alloy matrix melt, and liquid stirring is performed at above 740°C to promote full melting; after full melting, the temperature is lowered to a semi-solid temperature range, and the temperature is kept constant for a period of time to obtain a semi-solid melt. The magnesium alloy matrix formula designed in the embodiment of the present application has a wide semi-solid temperature range, which is conducive to the subsequent uniform dispersion of the reinforcement through stirring.
[0078] Step S102, vortex stirring the semi-solid melt, adding the preheated reinforcement at the center of the vortex, stirring continuously and heating to a temperature above the liquidus temperature, and then casting to obtain a magnesium-based composite material ingot;
[0079] The embodiments of the present application can achieve low-cost preparation with few processes by adopting stirring casting, wherein the casting can be gravity casting or semi-continuous casting. The present application selects a semi-solid temperature range for reinforcement dispersion, which can achieve better dispersion of the reinforcement in the magnesium alloy matrix. The present application can achieve highly uniform dispersion of the reinforcement in the semi-solid melt by adding preheated reinforcements to the center of the vortex, which is beneficial to improving the performance of magnesium-based composite materials. The speed of vortex stirring can be 300-800r / min. In some embodiments, the speed of vortex stirring can specifically be 300r / min, 500r / min, 600r / min, and 800r / min. The preheating temperature can be 400℃-600℃.
[0080] Step S103, hot extrusion or rolling forming the magnesium-based composite material ingot, and heat treatment to obtain a magnesium-based composite material. In the embodiment of the present application, the hot extrusion process temperature can be 300°C-350°C, and hot extrusion in this temperature range can enable the material to obtain better extrusion processability. In some embodiments, the hot extrusion process temperature can be 300°C, 320°C, and 350°C. During the hot extrusion or rolling deformation process, the reinforcement dispersion can be further strengthened. The heat treatment can be an under-aging heat treatment or a peak aging heat treatment. The heat treatment temperature can be 150°C-300°C, and the time can be 4-12 hours. Specifically, the heat treatment temperature can be, for example, 150°C, 160°C, 175°C, 180°C, 200°C, 220°C, 250°C, 280°C, 300°C, etc., and the heat treatment time can be 4 hours, 6 hours, 8 hours, 10 hours, 12 hours, etc. The composite material of the present application adopts appropriate heat treatment to promote the precipitation of dispersed second phase at the interface dislocation, give full play to the joint strengthening effect of aging precipitation phase and external reinforcement, thereby ensuring that the composite material better takes into account high strength and high toughness.
[0081] The method for preparing the magnesium-based composite material in the embodiment of the present application adopts a semi-solid stirring casting combined with a hot extrusion or rolling process, has good processability, can achieve a good dispersion effect of the reinforcement, and ultimately can achieve low-cost continuous preparation of the magnesium-based composite material.
[0082] The embodiment of the present application also provides a structural part, which is prepared by using the magnesium-based composite material mentioned above in the present application. The structural part can be various structural parts with high thermal conductivity, high toughness and high modulus requirements, such as electronic equipment housing.
[0083] See also Figure 1 The embodiment of the present application provides a housing 100, which is made of the magnesium-based composite material mentioned above, that is, the housing 100 is a magnesium-based composite material housing. The housing 100 may be an electronic device housing.
[0084] See also Figure 2 The embodiment of the present application provides an electronic device 200, which includes a housing 21 and components such as a mainboard and a battery located inside the housing 21 (not shown in the figure). The housing 21 is the housing 100 described above in the embodiment of the present application in its entirety or in part, that is, the housing 21 is made of the magnesium-based composite material described above in the embodiment of the present application in its entirety or in part. The electronic device 200 may include a mobile phone, a tablet computer, a laptop computer, a wearable device, a portable machine, a super mobile personal computer (ΜMPC), a handheld computer, a walkie-talkie, a netbook, a POS machine, a personal digital assistant (PDA), a driving recorder, a virtual reality device, a wireless USB flash drive, a Bluetooth speaker / headphone, or a mobile terminal or a fixed terminal with a frame or a housing, such as a car front-end.
[0085] Taking the electronic device 200 as a mobile phone as an example, Figure 3 This is a schematic diagram of the structure of the front cover, middle frame and back cover of the mobile phone in the embodiment of the present application. Figure 3As shown, the mobile phone housing 21 may specifically include a front cover 211 assembled on the front side of the mobile phone (i.e., the display screen side), and may also include a back cover 213 assembled on the back side. In some embodiments, the housing 21 may also include a middle frame 212 located between the front cover 211 and the back cover 213, and the middle frame 212 is used to carry components such as a motherboard and a battery. In an embodiment of the present invention, the front cover 211, the back cover 213 and / or the middle frame 212 are the magnesium-based composite material shell provided in the embodiment of the present application as a whole, or the front cover 211, the back cover 213 and / or the middle frame 212 are a part of the magnesium-based composite material shell provided in the embodiment of the present application, for example, a part of the back cover 213 or a part of the front cover 211 and the middle frame 212 are the magnesium-based composite material shell provided in the embodiment of the present application. In some embodiments of the present application, the back cover 213 and the middle frame 212 may be an integral structure; in other embodiments of the present application, the back cover 213 and the middle frame 212 may also be a split structure. Among them, the mobile phone also includes a display screen. In a full-screen mobile phone, the housing 21 generally does not include a front cover, and the middle frame is located between the display screen and the back cover. Alternatively, in some full-screen mobile phones, the housing 21 may not include a middle frame exposed to the outside.
[0086] The magnesium-based composite material of the embodiment of the present application is used to prepare the housing of an electronic device, which can improve the thermal conductivity, impact resistance, and drop resistance of the electronic device, while also having good weight reduction benefits, which can improve product competitiveness in many aspects and enhance user experience.
[0087] In the present application, “-” indicates a range, including two endpoint values. For example, “Zn 4%-7%” includes two endpoint values of 4% and 7%, as well as any value between the two endpoint values; for another example, “Al 0-4%” includes two endpoint values of 0 and 4%, as well as any value between the two endpoint values.
[0088] The embodiments of the present application are further described below with reference to a plurality of embodiments.
[0089] Example 1
[0090] The present embodiment provides a magnesium-based composite material, including a magnesium alloy matrix and a reinforcement, wherein the magnesium alloy matrix includes the following elements by weight percentage: Zn 6wt%, Al 0.5wt%, Ca 0.2wt%, Zr 0.2wt%, Ce0.1wt%, La 0.1wt%, Y 0.05wt%, Nd 0.05wt%, Si 0.05wt%, Mn 0.05wt%, Sr0.05wt%, Sn 0.05wt%, and the remainder is Mg and unavoidable impurity elements, wherein the weight percentage of the impurity elements does not exceed 0.1%. The reinforcement is SiC particles, the particle size of the SiC particles is 10μm, and the volume fraction is 7%.
[0091] The magnesium alloy matrix is melted according to the above formula, and is fully stirred in liquid state at above 740°C, then cooled to a semi-solid temperature of 50% liquid phase ratio, and the semi-solid melt is subjected to high-speed vortex stirring at a rotation speed of 500r / min, and reinforcement particles are added at the same time. Then, the temperature is raised to 680°C, and semi-continuous casting is performed to obtain a magnesium-based composite material ingot; subsequently, it is hot extruded at 300°C and heat treated at 175°C for 12h to obtain a magnesium-based composite material plate with a cross-sectional size of 90mm×6mm.
[0092] The microstructure and composition distribution of the magnesium-based composite material plate prepared in this embodiment were calibrated using a scanning electron microscope (SEM). The results are as follows: Figure 4 As shown by Figure 4 It can be seen that in the magnesium-based composite material, the reinforcement particles 12 are evenly distributed in the magnesium alloy matrix 11 without agglomeration.
[0093] The magnesium-based composite material plate prepared in this embodiment was processed into a sample with a size of 1 mm×2 mm×3 mm, and the distribution of the internal reinforcement was measured using XCT (X-ray computed tomography) technology. The results are as follows: Figure 5 As shown by Figure 5 It can be seen that the enhancement body ( Figure 5 The bright white part in the middle is evenly distributed in three dimensions without agglomeration.
[0094] Example 2
[0095] The present embodiment provides a magnesium-based composite material, comprising a magnesium alloy matrix and a reinforcement, wherein the magnesium alloy matrix comprises the following elements by weight percentage: Zn 6wt%, Al 0.5wt%, Ca 0.2wt%, Zr 0.2wt%, Ce0.1wt%, La 0.1wt%, Y 0.05wt%, Nd 0.05wt%, Si 0.05wt%, Mn 0.05wt%, Sr0.05wt%, Sn 0.05wt%, and the remainder is Mg and unavoidable impurity elements, wherein the weight percentage of the impurity elements does not exceed 0.1%. The reinforcement is SiC particles, the particle size of the SiC particles is 5μm, and the volume fraction is 13%.
[0096] The magnesium alloy matrix is melted according to the above formula, and is fully stirred in liquid state at above 740°C, then cooled to a semi-solid temperature of 50% liquid phase ratio, and the semi-solid melt is subjected to high-speed vortex stirring at a rotation speed of 500r / min, and reinforcement particles are added at the same time. Then, the temperature is raised to 680°C, and semi-continuous casting is performed to obtain a magnesium-based composite material ingot; subsequently, it is hot extruded at 350°C and heat treated at 175°C for 12h to obtain a magnesium-based composite material plate with a cross-sectional size of 90mm×6mm.
[0097] The microstructure and composition distribution of the magnesium-based composite material plate prepared in this embodiment were calibrated using a scanning electron microscope. The results are as follows: Figure 6 As shown by Figure 6 It can be seen that in the magnesium-based composite material, the reinforcement particles 12 are evenly distributed in the magnesium alloy matrix 11 without agglomeration and the interface bonding is good.
[0098] Compared with Example 1, Example 2 uses a reinforcement with a finer particle size, which can achieve a better strengthening effect.
[0099] Example 3
[0100] The present embodiment provides a magnesium-based composite material, including a magnesium alloy matrix and a reinforcement, wherein the magnesium alloy matrix includes the following elements by weight percentage: Zn 6wt%, Al 0.5wt%, Ca 0.2wt%, Zr 0.2wt%, Ce0.1wt%, La0.1wt%, Y 0.05wt%, Nd 0.05wt%, Si 0.05wt%, Mn 0.05wt%, Sr 0.05wt%, Sn 0.05wt%, and the remainder is Mg and unavoidable impurity elements, wherein the weight percentage of the impurity elements does not exceed 0.1%. The reinforcement is chopped carbon fiber, the length of the chopped carbon fiber is 2mm, and the volume fraction is 20%.
[0101] The magnesium alloy matrix is melted according to the above formula, and is fully stirred in liquid state at above 740°C, then cooled to a semi-solid temperature of 50% liquid phase ratio, and the semi-solid melt is subjected to high-speed vortex stirring at a rotation speed of 500r / min, and reinforcement fibers are added at the same time. Then, the temperature is raised to 680°C, and semi-continuous casting is performed to obtain a magnesium-based composite material ingot; subsequently, it is hot extruded at 350°C and heat treated at 175°C for 12h to obtain a magnesium-based composite material plate with a cross-sectional size of 90mm×6mm.
[0102] The magnesium-based composite material plate prepared in this embodiment was calibrated for its microstructure morphology and component distribution using scanning electron microscopy and transmission electron microscopy. The scanning electron microscopy results are as follows: Figure 7 As shown by Figure 7 It can be seen that in the magnesium-based composite material, the reinforcement fibers 12 are evenly distributed in the magnesium alloy matrix 11, without agglomeration, and the interface is complete; the transmission electron microscopy results are as follows Figure 8 As shown by Figure 8 It can be seen that in magnesium-based composites, the additional layer (TiO 2 ) and the magnesium alloy matrix has a complete and clear interface, and a good interface bonding is maintained between the additional layer and the magnesium alloy matrix.
[0103] Example 4
[0104] This embodiment provides a magnesium-based composite material, including a magnesium alloy matrix and a reinforcement, wherein the magnesium alloy matrix includes the following elements by weight percentage: Zn 6wt%, Ca 0.2wt%, and the remainder is Mg and unavoidable impurity elements, wherein the weight percentage of the impurity elements does not exceed 0.1%. The reinforcement is SiC particles, the particle size of the SiC particles is 10μm, and the volume fraction is 7%.
[0105] The magnesium alloy matrix is melted according to the above formula, and is fully stirred in liquid state at above 740°C, then cooled to a semi-solid temperature of 50% liquid phase ratio, and the semi-solid melt is subjected to high-speed vortex stirring at a rotation speed of 500r / min, and reinforcement particles are added at the same time. Then, the temperature is raised to 680°C, and semi-continuous casting is performed to obtain a magnesium-based composite material ingot; subsequently, it is hot extruded at 300°C and heat treated at 175°C for 12h to obtain a magnesium-based composite material plate with a cross-sectional size of 90mm×6mm.
[0106] Fig. 9 This is the metallographic structure diagram of the magnesium-based composite material plate obtained in Example 4. In the metallographic structure diagram, the grayish white part is the magnesium alloy matrix, and the black part is the reinforcement. Fig. 9 It can be seen that in the magnesium-based composite material, the reinforcement is evenly distributed in the magnesium alloy matrix without agglomeration, and the interface is clear and complete.
[0107] Example 5
[0108] The present embodiment provides a magnesium-based composite material, comprising a magnesium alloy matrix and a reinforcement, wherein the magnesium alloy matrix comprises the following elements by weight percentage: Zn 4.5wt%, Al 0.5wt%, Ca 0.2wt%, Zr 0.2wt%, Ce0.1wt%, La 0.1wt%, Y 0.05wt%, Nd 0.05wt%, Si 0.05wt%, Mn 0.05wt%, Sr0.05wt%, Sn 0.05wt%, and the remainder is Mg and unavoidable impurity elements, wherein the weight percentage of the impurity elements does not exceed 0.1%. The reinforcement is SiC particles, the particle size of the SiC particles is 10μm, and the volume fraction is 5%.
[0109] The magnesium alloy matrix is melted according to the above formula, and is fully stirred in liquid state at above 740°C, then cooled to a semi-solid temperature of 50% liquid phase ratio, and the semi-solid melt is subjected to high-speed vortex stirring at a rotation speed of 500r / min, and reinforcement particles are added at the same time. Then, the temperature is raised to 680°C, and semi-continuous casting is performed to obtain a magnesium-based composite material ingot; subsequently, it is hot extruded at 300°C and heat treated at 175°C for 12h to obtain a magnesium-based composite material plate with a cross-sectional size of 90mm×6mm.
[0110] Fig.10This is the metallographic structure diagram of the magnesium-based composite material plate obtained in Example 5. In the metallographic structure diagram, the grayish white part is the magnesium alloy matrix, and the black part is the reinforcement. Fig.10 It can be seen that in the magnesium-based composite material, the reinforcement is evenly distributed in the magnesium alloy matrix without agglomeration, and the interface is clear and complete.
[0111] Example 6
[0112] This embodiment provides a magnesium-based composite material, including a magnesium alloy matrix and a reinforcement, wherein the magnesium alloy matrix includes the following elements by weight percentage: Zn 6wt%, Ca 0.8wt%, and the remainder is Mg and unavoidable impurity elements, wherein the weight percentage of the impurity elements does not exceed 0.1%. The reinforcement is SiC particles, the particle size of the SiC particles is 10μm, and the volume fraction is 7%.
[0113] The magnesium alloy matrix is melted according to the above formula, and is fully stirred in liquid state at above 740°C, then cooled to a semi-solid temperature of 50% liquid phase ratio, and the semi-solid melt is subjected to high-speed vortex stirring at a rotation speed of 500r / min, and reinforcement particles are added at the same time. Then, the temperature is raised to 680°C, and semi-continuous casting is performed to obtain a magnesium-based composite material ingot; subsequently, it is hot extruded at 300°C and heat treated at 175°C for 12h to obtain a magnesium-based composite material plate with a cross-sectional size of 90mm×6mm.
[0114] Fig.11 This is the metallographic structure diagram of the magnesium-based composite material plate obtained in Example 6. In the metallographic structure diagram, the grayish white part is the magnesium alloy matrix, and the black part is the reinforcement. Fig.11 It can be seen that in the magnesium-based composite material, the reinforcement is evenly distributed in the magnesium alloy matrix without agglomeration, and the interface is clear and complete.
[0115] Example 7
[0116] The present embodiment provides a magnesium-based composite material, including a magnesium alloy matrix and a reinforcement, wherein the magnesium alloy matrix includes the following elements by weight percentage: Zn 6wt%, Ca 0.05wt%, Ce 0.15wt%, La 0.15wt%, Y0.1wt%, Nd 0.1wt%, and the remainder is Mg and unavoidable impurity elements, wherein the weight percentage of the impurity elements does not exceed 0.1%. The reinforcement is SiC particles, the particle size of the SiC particles is 5μm, and the volume fraction is 8%.
[0117] The magnesium alloy matrix is melted according to the above formula, and is fully stirred in liquid state at above 740°C, then cooled to a semi-solid temperature of 50% liquid phase ratio, and the semi-solid melt is subjected to high-speed vortex stirring at a rotation speed of 500r / min, and reinforcement particles are added at the same time. Then, the temperature is raised to 680°C, and semi-continuous casting is performed to obtain a magnesium-based composite material ingot; subsequently, it is hot extruded at 300°C and heat treated at 175°C for 12h to obtain a magnesium-based composite material plate with a cross-sectional size of 90mm×6mm.
[0118] Fig.12 This is the metallographic structure diagram of the magnesium-based composite material plate obtained in Example 7. In the metallographic structure diagram, the grayish white part is the magnesium alloy matrix, and the black part is the reinforcement. Fig.12 It can be seen that in the magnesium-based composite material, the reinforcement is evenly distributed in the magnesium alloy matrix without agglomeration, and the interface is clear and complete.
[0119] Example 8
[0120] The present embodiment provides a magnesium-based composite material, including a magnesium alloy matrix and a reinforcement, wherein the magnesium alloy matrix includes the following elements by weight percentage: Zn 6wt%, Ca 0.05wt%, Zr 0.5wt%, Si 0.1wt%, Mn 0.1wt%, Sr 0.05wt%, Sn 0.1wt%, and the remainder is Mg and unavoidable impurity elements, wherein the weight percentage of the impurity elements does not exceed 0.1%. The reinforcement is SiC particles, the particle size of the SiC particles is 5μm, and the volume fraction is 15%.
[0121] The magnesium alloy matrix is melted according to the above formula, and is fully stirred in liquid state at above 740°C, then cooled to a semi-solid temperature of 50% liquid phase ratio, and the semi-solid melt is subjected to high-speed vortex stirring at a rotation speed of 500r / min, and reinforcement particles are added at the same time. Then, the temperature is raised to 680°C, and semi-continuous casting is performed to obtain a magnesium-based composite material ingot; subsequently, it is hot extruded at 300°C and heat treated at 175°C for 12h to obtain a magnesium-based composite material plate with a cross-sectional size of 90mm×6mm.
[0122] Fig.13 This is the metallographic structure diagram of the magnesium-based composite material plate obtained in Example 8. In the metallographic structure diagram, the grayish white part is the magnesium alloy matrix, and the black part is the reinforcement. Fig.13 It can be seen that in the magnesium-based composite material, the reinforcement is evenly distributed in the magnesium alloy matrix without agglomeration, and the interface is clear and complete.
[0123] In order to demonstrate the beneficial effects of the embodiments of the present application, the magnesium-based composite materials of embodiments 1-8 were subjected to the following performance tests, and the test results are shown in Table 3:
[0124] (1) Processing magnesium-based composite material plates into dog-bone test pieces of national standard (GB / T 228.1-2010) size and testing their mechanical properties;
[0125] (2) Processing the magnesium-based composite material plate into a thermal diffusivity test disc of ASTM standard (ASTM E1461) size and testing its thermal conductivity;
[0126] (3) The magnesium-based composite material sheet was processed into samples with a size of 60 mm × 10 mm × 1.5 mm, and its elastic modulus was tested using the dynamic resonance method (ASTM E1876).
[0127] In addition, the magnesium-based composite material plates of Examples 1-8 were processed into mobile phone middle frames of the same size and model through CNC technology, and their specific stiffness was paid attention to, wherein the specific stiffness refers to the ratio of the elastic modulus of a material to its density, also known as "specific modulus" or "specific elastic modulus". A higher specific stiffness means that the material is lighter at the same stiffness, or has greater stiffness at the same mass.
[0128] Table 3 Performance test results of magnesium-based composite materials
[0129]
[0130]
[0131] It can be seen from Table 3 that the magnesium-based composite material of the embodiment of the present application has high thermal conductivity, high strength and toughness, and high modulus. The mobile phone middle frame processed by the magnesium-based composite material of the embodiment of the present application has a higher specific stiffness than the current conventional mobile phone middle frame molding materials (die-cast aluminum ADC12, die-cast magnesium AZ9D, aluminum alloy 6013, magnesium alloy AZ31B).
Claims
1. A magnesium-based composite material, characterized in that: The magnesium-based composite material includes a magnesium alloy matrix and a reinforcement distributed in the magnesium alloy matrix. Based on 100% by weight of the magnesium alloy matrix, the weight percentage of each component of the magnesium alloy matrix is: Zn 4%-7%, Ca 0.05%-0.8%, Al 0-4%, Zr 0-1%, Ce 0-0.8%, La 0-0.8%, Y 0-0.8%, Nd 0-0.8%, Si 0-0.8%, Mn 0-1.5%, Sr 0-0.5%, Sn 0-1%, Sc 0-0.5%, Gd 0-0.8%, and the balance is Mg and unavoidable impurity elements; in the magnesium alloy matrix, the total weight percentage of Ca, Zr, Ce, La, Y, Nd, Si, Mn, Sr, Sn, Sc, and Gd is greater than or equal to 0.15% and less than or equal to 2%.
2. The magnesium-based composite material according to claim 1, characterized in that: In the magnesium alloy matrix, the weight percentage of Zn is 4.5%-6%.
3. The magnesium-based composite material according to claim 1 or 2, characterized in that: In the magnesium alloy matrix, the weight percentage of Ca is 0.1%-0.5%.
4. The magnesium-based composite material according to claim 3, characterized in that: In the magnesium alloy matrix, the weight percentage of Ca is 0.2%-0.4%.
5. The magnesium-based composite material according to claim 1 or 2, characterized in that: In the magnesium alloy matrix, the weight percentage of Al is 0.2%-2%.
6. The magnesium-based composite material according to claim 1 or 2, characterized in that: In the magnesium alloy matrix, the weight percentage of Zr is 0.2%-0.4%.
7. The magnesium-based composite material according to claim 1 or 2, characterized in that: In the magnesium alloy matrix, the weight percentage of Ce is 0.1%-0.4%.
8. The magnesium-based composite material according to claim 1 or 2, characterized in that: In the magnesium alloy matrix, the weight percentage of La is 0.1%-0.4%.
9. The magnesium-based composite material according to claim 1 or 2, characterized in that: In the magnesium alloy matrix, the weight percentage of Y is 0.05%-0.4%.
10. The magnesium-based composite material according to claim 1 or 2, characterized in that: The weight percentage of inevitable impurity elements in the magnesium alloy matrix does not exceed 0.1%.
11. The magnesium-based composite material according to claim 1 or 2, characterized in that: In the magnesium-based composite material, the volume percentage of the reinforcement is 1%-20%.
12. The magnesium-based composite material according to claim 1, characterized in that: The reinforcement includes reinforcement particles and / or reinforcement fibers.
13. The magnesium-based composite material according to claim 12, characterized in that: The reinforcing particles include one or more of SiC, B4C, SiO2, ZrO2, Si3N4, AlN, BN, Al2O3, TiC, TiB2, diamond, graphite, graphene, and carbon nanotubes; the reinforcing fibers include carbon fibers.
14. The magnesium-based composite material according to claim 12 or 13, characterized in that: The size of the reinforcing particles is less than or equal to 50 μm; the reinforcing fibers are chopped fibers, and the chopped length is less than or equal to 2 mm.
15. The magnesium-based composite material according to claim 12, characterized in that: The reinforcement also includes an additional layer arranged on the surface of the reinforcement particles and / or reinforcement fibers, and the additional layer includes one or more of magnesium oxide, silicon dioxide, titanium dioxide, titanium and its alloys, copper and its alloys, zirconium and its alloys, titanium nitride, and silicon carbide.
16. The magnesium-based composite material according to claim 1 or 2, characterized in that: The magnesium-based composite material has a thermal conductivity of 90 W / mK-130 W / mK, a yield strength of ≥200 MPa, a tensile strength of ≥250 MPa, an elongation of ≥3%, and an elastic modulus of 45 GPa-70 GPa.
17. A method for preparing a magnesium-based composite material according to any one of claims 1 to 16, characterized in that: The following steps are involved: Obtaining a magnesium alloy matrix melt by smelting, and adjusting the temperature of the magnesium alloy matrix melt to a semi-solid temperature range to obtain a semi-solid melt; The semi-solid melt is subjected to vortex stirring, a preheated reinforcement is added to the center of the vortex, the mixture is continuously stirred and heated to a temperature above the liquidus temperature, and then cast to obtain a magnesium-based composite material ingot; The magnesium-based composite material ingot is hot extruded or rolled into shape, and then subjected to heat treatment to obtain the magnesium-based composite material.
18. A structural member, characterized in that: The structural component is prepared by using the magnesium-based composite material according to any one of claims 1-16.
19. A housing, characterized in that: The shell is made of the magnesium-based composite material according to any one of claims 1-16.
20. An electronic device, characterized in that: It comprises an outer shell and a mainboard located inside the outer shell, and the outer shell is wholly or partially the shell as described in claim 19.
Citation Information
Patent Citations
High conductivity magnesium alloy
WO2017205281A1
Cited By
High-strength magnesium alloy casting and preparation method and application thereof
CN120945263A
High-strength magnesium alloy castings, methods of making and using the same
CN120945263B