Magnesium-based composite material implant and preparation method and use thereof

By introducing iron tetraoxide into magnesium alloys to form a magnesium-based composite implant, the problems of inability to degrade and low heating efficiency of existing magnetothermal media are solved, efficient heating and rapid degradation in biological bodies are achieved, and significantly improved Effects of anti-tumor treatment.

CN117731845BActive Publication Date: 2024-11-01CAIHUI NEW MATERIALS (SHANGHAI) CO LTD
View PDF 22 Cites 0 Cited by

Patent Information

Application Number
CN202311655334.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-05
Publication Date
2024-11-01
Estimated Expiration
2043-12-05

AI Technical Summary

Technical Problem

The existing magnetothermal media cannot degrade in the body, and the non-magnetic nature of the magnesium alloy itself leads to low heating efficiency, poses safety risks, and the degradation rate in the body is slow, making it difficult to effectively inhibit tumors.

Method used

By introducing iron tetraoxide into the magnesium alloy, a magnesium-based composite implant is formed, which improves its magnetic properties and degradation rate, and uses an alternating magnetic field to perform magnetic induction heating and rapidly degrade in the biological body to inhibit tumors.

Benefits of technology

It is achieved efficient heating of tumor cells under low alternating magnetic field intensity, and at the same time, the microenvironment generated by rapid degradation inhibits tumor growth, reducing the risk of damage to normal tissues and improving the therapeutic effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117731845B_ABST
    Figure CN117731845B_ABST
Patent Text Reader

Abstract

The present application discloses a magnesium-based composite material implant and its preparation method and use. The magnesium-based composite material implant comprises, by weight, x parts of ferroferric oxide, with 0<x≤10, and the rest being magnesium alloy. The magnesium-based composite material implant described in the present application can not only be used as a magnetocaloric medium, but also has a faster degradation rate in a living body.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of alloy materials and biomedical engineering technology, and in particular to a magnesium-based composite material implant, a method for preparing the magnesium-based composite material implant, and uses of the magnesium-based composite material implant. Background Art

[0002] Magnetic induction thermal therapy is an interventional treatment for thermal ablation of tumors. It requires implanting a magnetic thermal medium near the lesion and applying an alternating magnetic field to heat the lesion, thereby directly ablating tumor cells or inducing apoptosis of tumor cells. The magnetic thermal medium currently used is mainly made of stainless steel and other materials, which cannot be degraded in the body and need to be removed by manual surgery.

[0003] Magnesium alloy is a good biomedical material with good biocompatibility, safety, non-toxicity and in vivo degradability. It has been used as a good demonstration material for human implants such as cardiovascular stents and bone screws. At the same time, the microenvironment generated by magnesium alloy during its degradation in the body can also inhibit tumor growth. Therefore, if magnesium alloy is used as a magnetothermal medium, it can simultaneously show the dual synergistic inhibitory effects of thermal ablation and microenvironment on tumors under magnetic induction heating, which has excellent application prospects.

[0004] However, magnesium alloys are non-magnetic, which results in low intrinsic heating efficiency. A larger alternating magnetic field strength is required, and excessive alternating magnetic field strength will heat normal human tissues, posing a major safety hazard. In addition, current medical magnesium alloys degrade slowly in the body, making it difficult to achieve the effect of inhibiting tumors.

[0005] Therefore, there is an urgent need in this field to develop a new magnesium-based composite implant that can not only serve as a magnetocaloric medium but also has a faster degradation rate in the body. Summary of the invention

[0006] The purpose of the present application is to provide a magnesium-based composite material implant that can not only serve as a magnetocaloric medium but also has a faster degradation rate in the body.

[0007] To achieve the above objectives, the technical solution of the present application provides a magnesium-based composite implant, the composition of which is, by weight: x parts of ferrosoferric oxide, with 0<x≤10, and the rest is magnesium alloy.

[0008] In some embodiments of the present application, the composition of the magnesium-based composite implant is, by weight: 1 to 8 parts of ferrosoferric oxide and the rest is magnesium alloy.

[0009] In some embodiments of the present application, the particle size of the ferrosoferric oxide is 1 micron to 50 microns.

[0010] In some embodiments of the present application, the composition of the magnesium alloy is: 1-3wt% aluminum, 3-5wt% zinc, and the rest is magnesium.

[0011] The technical solution of the present application also provides a method for preparing the above-mentioned magnesium-based composite material implant, comprising: heating the raw materials for preparing the magnesium alloy to a first temperature under the protection of a protective gas, melting and mixing the raw materials for preparing the magnesium alloy to obtain a magnesium alloy melt, and cooling the magnesium alloy melt to a second temperature; adding ferroferric oxide preheated to a third temperature to the cooled magnesium alloy melt to obtain a magnesium-based composite material melt; casting the magnesium-based composite material melt into a mold to obtain a magnesium-based composite material ingot; homogenizing the magnesium-based composite material ingot, and obtaining the magnesium-based composite material implant through a molding process.

[0012] In some embodiments of the present application, the preparation method satisfies at least one of the following conditions: a. the raw materials for preparing the magnesium alloy include pure magnesium, pure zinc and pure aluminum; b. the protective gas includes a mixture of carbon dioxide and sulfur hexafluoride or a mixture of argon and sulfur hexafluoride; c. the first temperature is 680°C to 750°C; d. the second temperature is 500°C to 650°C.

[0013] In some embodiments of the present application, the preparation method satisfies at least one of the following conditions: A. the third temperature is 300°C to 500°C; B. the stirring rate when adding the ferrosoferric oxide is 300r / min to 500r / min.

[0014] In some embodiments of the present application, the preparation method satisfies at least one of the following conditions: (1) the temperature of the homogenization treatment is 300°C to 420°C, and the time is 8 hours to 20 hours; (2) the temperature of the molding process is 250°C to 350°C.

[0015] The technical solution of the present application also provides the use of the above-mentioned magnesium-based composite material implant as an anti-tumor material, and the tumor is treated by the rapid degradation of the magnesium-based composite material implant; preferably, the degradation rate of the magnesium-based composite material implant in the organism is 100 mg / cm 2 / day~200mg / cm 2 / sky.

[0016] The technical solution of the present application also provides the use of the above-mentioned magnesium-based composite material implant as a magnetothermal induction medium, and the magnesium-based composite material implant is subjected to magnetic induction heating by an alternating magnetic field to treat tumors; preferably, the magnetic field strength of the alternating magnetic field is 500A / m to 1500A / m, the alternating frequency is 330kHz to 430kHz, the heating temperature of the magnesium-based composite material implant is 60°C to 80°C, and the degradation rate of the magnesium-based composite material implant in the organism is 100mg / cm 2 / day~200mg / cm 2 / sky.

[0017] Compared with the prior art, the magnesium-based composite implant of the technical solution of the present application has the following beneficial effects:

[0018] By introducing ferroferric oxide into the magnesium alloy, the magnetic properties of the magnesium alloy are improved, so that the resulting magnesium-based composite implant can have a higher heating temperature under a lower alternating magnetic field intensity. At the same time, due to the large potential difference between ferroferric oxide and the magnesium matrix, the magnesium-based composite implant has a faster degradation rate in the body.

[0019] When the magnesium-based composite material implant is implanted in a living body, the microenvironment generated during the rapid degradation of the magnesium-based composite material implant in the living body can be used to inhibit tumor growth, thereby achieving the purpose of treating the tumor.

[0020] When the magnesium-based composite material implant is implanted in a living body, the magnesium-based composite material implant can be magnetically heated by an alternating magnetic field to directly ablate tumor cells or induce tumor cell apoptosis, thereby achieving the purpose of treating tumors.

[0021] In summary, the magnesium-based composite material implant of the technical solution of the present application can simultaneously exhibit the dual synergistic inhibitory effects of thermal ablation and microenvironment on tumors in vivo, and has excellent application prospects in the anti-tumor field. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] The following drawings describe in detail the exemplary embodiments disclosed in this application. The same reference numerals represent similar structures in several views of the drawings. Those skilled in the art will understand that these embodiments are non-limiting, exemplary embodiments, and the drawings are only used for the purpose of illustration and description, and are not intended to limit the scope of this application. Other embodiments may also accomplish the inventive intent in this application. It should be understood that the drawings are not drawn to scale. Among them:

[0023] Figure 1 This is a scanning electron microscope image of the magnesium-based composite implant wire of Example 1 of the present application;

[0024] Figure 2This is a scanning electron microscope image of the magnesium-based composite implant wire of Example 2 of the present application;

[0025] Figure 3 This is a scanning electron microscope image of the magnesium alloy wire of Comparative Example 1 of the present application;

[0026] Figure 4 It is a schematic diagram of the inhibitory effect of the magnesium-based composite implant wire of Example 1 of the present application and the magnesium alloy wire of Comparative Example 1 on tumors;

[0027] Figure 5 Schematic diagram of the inhibitory effect of the magnesium-based composite implant wire of Example 1 of the present application and the magnesium alloy wire of Comparative Example 1 on larger tumors. DETAILED DESCRIPTION

[0028] The following description provides specific application scenarios and requirements of the present application, with the purpose of enabling those skilled in the art to make and use the content in the present application. It will be apparent to those skilled in the art that various local modifications to the disclosed embodiments are apparent, and the general principles defined herein may be applied to other embodiments and applications without departing from the spirit and scope of the present application. Therefore, the present application is not limited to the embodiments shown, but to the widest scope consistent with the claims.

[0029] Magnetic induction thermal therapy can directly ablate tumor cells or induce apoptosis of tumor cells, but the magnetic thermal medium used cannot be degraded in the body and needs to be removed by artificial surgery after the treatment. Although magnesium alloy can be degraded in the body, and the microenvironment generated during the degradation process can inhibit tumor growth, the degradation time of magnesium alloy in the body is relatively long, and it is often difficult to achieve the effect of inhibiting tumors. At the same time, magnesium alloy itself is non-magnetic, and its intrinsic induction heating effect is very low. It needs to be induced by a larger alternating magnetic field, but the larger alternating magnetic field strength will damage normal tissues in the body and pose a greater safety hazard. Therefore, magnesium alloy cannot be directly used as a magnetic thermal medium for interventional treatment of thermal ablation of tumors.

[0030] Based on this, the technical solution of the present application modifies the magnesium alloy so that when the modified magnesium alloy is implanted into the lesion site in the body as a magnetothermal medium, it can simultaneously exhibit the dual synergistic inhibitory effects of thermal ablation and microenvironment on the tumor through magnetic induction heating. Specifically, the technical solution of the present application obtains a magnesium-based composite implant by introducing magnetic ferroferric oxide into the magnesium alloy to achieve the above effect.

[0031] In a specific embodiment, the composition of the magnesium-based composite implant is, by weight, x parts of ferrosoferric oxide, and 0<x≤10, and the rest is magnesium alloy. For example, x can be 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9, 5, 5.1, 5.2 , 5.3, 5.4, 5.5, 5.6, 5.7, 5.8, 5.9, 6, 6.1, 6.2, 6.3, 6.4, 6.5, 6.6, 6.7, 6.8, 6.9, 7, 7.1, 7.2, 7.3, 7.4, 7.5, 7.6, 7.7, 7.8, 7.9, 8, 8.1, 8.2, 8.3, 8.4, 8.5, 8.6, 8.7, 8.8, 8.9, 9, 9.1, 9.2, 9.3, 9.3, 9.5, 9.6, 9.7, 9.8, 9.9, 10, or ranges or subranges between any two of them.

[0032] In the magnesium-based composite implant, the ferroferric oxide can improve the magnetic properties of the magnesium-based composite implant on the one hand, thereby enabling the magnesium-based composite implant to significantly reduce the alternating magnetic field intensity when used as a magnetothermal medium; on the other hand, the ferroferric oxide has a large potential difference with the magnesium matrix, and the dispersed ferroferric oxide particles form a micro-electric couple with the surrounding magnesium matrix, which accelerates the dissolution of the magnesium alloy around the ferroferric oxide, so that the magnesium-based composite implant has a faster degradation rate in the body. Therefore, when the magnesium-based composite implant of the embodiment of the present application is used as a magnetothermal medium for interventional treatment of thermal ablation of tumors, it can not only heat the lesion site at a lower alternating magnetic field intensity, thereby directly ablating tumor cells or inducing tumor cell apoptosis, but also has a faster degradation rate in the body, so that the microenvironment generated during the degradation process can inhibit tumor growth. Therefore, the magnesium-based composite implant of the embodiment of the present application can have a dual synergistic inhibitory effect on tumors, and has excellent application prospects in anti-tumor.

[0033] In a preferred embodiment, the magnesium-based composite implant comprises, by weight, 1 to 8 parts of ferroferric oxide and the rest of magnesium alloy. When the content of ferroferric oxide particles is within this range, they can be well dispersed in the magnesium alloy matrix and can better meet the requirements of alloy degradation and heating efficiency.

[0034] The size of the ferroferric oxide affects the processing performance of the magnesium-based composite implant. If the particle size of the ferroferric oxide is too small, it is difficult to disperse in the magnesium alloy; if the particle size of the ferroferric oxide is too large, the magnesium-based composite material formed by the ferroferric oxide dispersed in the magnesium alloy has poor ductility and is not easy to process and shape. In a preferred embodiment, the particle size of the ferroferric oxide is 1 micron to 50 microns.

[0035] In a preferred embodiment, the magnesium alloy comprises 1-3 wt% aluminum, 3-5 wt% zinc, and the remainder magnesium. The magnesium alloy has a relatively fast corrosion degradation rate and good ductility.

[0036] The present application also provides the use of the above-mentioned magnesium-based composite material implant as an anti-tumor material. The rapid degradation of the magnesium-based composite material implant is used to treat tumors or cancer. In some preferred embodiments, the degradation rate of the magnesium-based composite material implant in the organism is 100 mg / cm 2 / day~200mg / cm 2 / sky.

[0037] The embodiments of the present application also provide the use of the above-mentioned magnesium-based composite material implant as a magnetothermal induction medium, and the magnesium-based composite material implant is subjected to magnetic induction heating by an alternating magnetic field to treat tumors or cancer.

[0038] In some preferred embodiments, when the magnesium-based composite implant is used as a magnetothermal induction medium, the magnetic field strength of the alternating magnetic field used is 500A / m to 1500A / m, and the alternating frequency is 330kHz to 430kHz. Under the alternating magnetic field conditions, the heating temperature of the magnesium-based composite implant can be 60°C to 80°C, which can not only directly ablate tumor cells or induce tumor cell apoptosis, but also avoid causing damage to other normal parts of the body, and has a high safety factor. In some more preferred embodiments, the magnetic field strength of the alternating magnetic field is 1000A / m, and the alternating frequency is 380kHz.

[0039] It should be noted that when the magnesium-based composite material implant is used as a magnetothermal induction medium to treat tumors or cancer, it can not only ablate tumor cells or induce tumor cell apoptosis through magnetic induction heating, but also the microenvironment generated by its degradation in the organism can inhibit tumor growth. The degradation rate of the magnesium-based composite material implant in the organism is more important. If the degradation rate of the magnesium-based composite material implant in the organism is too high, it will cause the interventional treatment to be degraded in the organism before it is completed, affecting the ablation effect; if the degradation rate of the magnesium-based composite material implant in the organism is too low, it will affect the inhibitory effect of the microenvironment generated by the degradation of the magnesium-based composite material implant on the tumor. Therefore, if the degradation rate of the magnesium-based composite material implant in the organism is too high or too low, it will affect the effect of anti-tumor treatment. The embodiment of the present application designs the components of the magnesium-based composite material implant so that the magnesium-based composite material implant has a more suitable degradation rate in the organism. In some preferred embodiments, the degradation rate of the magnesium-based composite material implant in the organism is 100 mg / cm 2 / day~200mg / cm 2 / sky.

[0040] In some specific embodiments, the tumor or cancer is selected from lung malignancies or cancers, hepatobiliary malignancies or cancers, gastrointestinal malignancies or cancers, hematological malignancies or cancers, sarcomas, skin malignancies or cancers, bone malignancies or cancers, genitourinary malignancies or cancers, nervous system malignancies or cancers, gynecological malignancies or cancers, and adrenal malignancies or cancers. Preferably, the lung malignancies or cancers are selected from bronchial carcinoma (squamous cell carcinoma, undifferentiated small cells, undifferentiated large cells, or adenocarcinomas), non-small cell lung cancer, bronchial carcinoma, bronchial adenoma, sarcoma, lymphoma, chondroitinoma, or mesothelioma. The hepatobiliary malignancies or cancers are selected from liver cancer, bile duct cancer, hepatoblastoma, angiosarcoma, hepatocellular adenoma, hemangioma, gallbladder cancer, ampullary carcinoma, or bile duct cancer. The gastrointestinal malignancy or cancer is selected from the group consisting of esophageal malignancy or cancer (squamous cell carcinoma, adenocarcinoma, leiomyosarcoma or lymphoma), gastric malignancy or cancer (carcinoma, lymphoma or leiomyosarcoma), pancreatic malignancy or cancer (ductal adenocarcinoma, insulinoma, glucagonoma, gastrinoma, carcinoid tumor, uveal tumor), small intestine (adenocarcinoma, lymphoma, carcinoid, Kaposi's sarcoma, leiomyoma, hemangioma, lipoma, neurofibroma, fibroma), colorectal cancer malignancy or cancer (adenocarcinoma, adenoma, adenoma, tubular adenoma) or leiomyoma. The hematological malignancy or cancer is selected from the group consisting of acute or chronic myeloid leukemia, acute lymphocytic leukemia, chronic lymphocytic leukemia, myeloproliferative disease, multiple myeloma, myelodysplastic syndrome, Hodgkin's disease or non-Hodgkin's lymphoma. The sarcoma is selected from the group consisting of angiosarcoma, fibrosarcoma, rhabdomyosarcoma, liposarcoma, myxoma, rhabdomyomas, fibromas, lipomas, or teratomas. The skin malignancies or cancers are selected from the group consisting of malignant melanoma, basal cell carcinoma, squamous cell carcinoma, Kaposi's sarcoma, nevus nevus, hyperplastic nevus, lipomas, hemangiomas, dermatofibromas, keloids, or psoriasis. The bone malignancies or cancers are selected from the group consisting of osteogenic sarcoma, fibrosarcoma, malignant fibrous histiocytoma, chondrosarcoma, Ewing's sarcoma, malignant lymphoma, multiple myeloma, malignant giant cell tumor chordoma, osteochondroma, benign enchondroma, chondroblastoma, chondromucofibroma, osteoid osteoma, or giant cell tumor. The genitourinary tract malignancy or cancer is selected from the group consisting of a renal malignancy or cancer (adenocarcinoma, Wilms' tumor or Wilms' tumor), a lymphoma, a leukemia, a bladder or urethral malignancy or cancer (squamous cell carcinoma, transitional cell carcinoma or adenocarcinoma), a prostate malignancy or cancer (adenocarcinoma or sarcoma), a testicular malignancy or cancer (leukemia, teratoma, embryonal carcinoma or teratoma), choriocarcinoma, sarcoma, stromal cell carcinoma, fibroma, fibroadenoma, adenomatoid tumor or lipoma.The nervous system malignancy or cancer is selected from osteoma, hemangioma, granuloma, xanthomas, deforming osteitis, meningioma, meningiosarcoma, glioma, astrocytoma, medulloblastoma, glioma, ependymoma, genital tumor, glioblastoma multiforme, oligodendroglioma, schwannoma, retinoblastoma, congenital tumor, spinal neurofibroma, meningioma, glioma or sarcoma. The gynecological malignancy or cancer is selected from endometrial carcinoma (serous cystadenocarcinoma, mucinous cystadenocarcinoma or unclassified carcinoma), granulosa-theca cell tumor, testicular interstitial cell tumor, myometrial abnormal tumor, malignant teratoma, squamous cell carcinoma, fibroepithelial carcinoma, glandular epithelial carcinoma, melanoma, clear cell carcinoma, squamous cell carcinoma, grape-like sarcoma or fallopian tube cancer. The adrenal malignancy or cancer is selected from neuroblastoma.

[0041] The present application also provides a method for preparing the above-mentioned magnesium-based composite material implant. In some specific embodiments, the preparation method comprises the following steps:

[0042] S1: heating raw materials for preparing the magnesium alloy to a first temperature under the protection of a protective gas, melting and mixing the raw materials to obtain a magnesium alloy melt, and cooling the magnesium alloy melt to a second temperature;

[0043] S2: adding ferroferric oxide preheated to a third temperature into the cooled magnesium alloy melt to obtain a magnesium-based composite material melt;

[0044] S3: casting the magnesium-based composite material melt into a mold to obtain a magnesium-based composite material ingot;

[0045] S4: homogenizing the magnesium-based composite material ingot, and obtaining the magnesium-based composite material implant through molding.

[0046] In some specific embodiments, in step S1, the magnesium alloy is an aluminum-zinc-magnesium ternary alloy, and the raw materials for preparing the magnesium alloy include pure magnesium, pure zinc and pure aluminum. In some specific embodiments, the protective gas includes a mixed gas of carbon dioxide and sulfur hexafluoride or a mixed gas of argon and sulfur hexafluoride. In some specific embodiments, the first temperature is 680°C to 750°C. In some specific embodiments, the second temperature is 500°C to 650°C, and in this temperature range, the magnesium alloy melt is in a semi-solid state.

[0047] In some specific embodiments, in step S2, the third temperature is 300°C to 500°C to prevent the temperature difference from being too large and causing the melt temperature to drop sharply. The ferrosoferric oxide is added under stirring conditions so that the ferrosoferric oxide is evenly dispersed in the magnesium alloy melt. In some specific embodiments, the stirring rate when adding the ferrosoferric oxide is 300r / min to 500r / min.

[0048] In some specific embodiments, the temperature of the homogenization process is 300°C to 420°C, and the time is 8 hours to 20 hours. In some specific embodiments, the temperature of the molding process is 250°C to 350°C.

[0049] In some preferred embodiments, the molding process is hot extrusion molding, and the formed magnesium-based composite material implant is a wire material, and the wire material is more suitable for clinical interventional treatment that requires the material to be implanted into the lesion. In some preferred embodiments, the diameter of the magnesium-based composite material formed by hot extrusion is 1 mm to 2 mm.

[0050] The following will be combined with the embodiments of the present application to clearly and completely describe the technical solution of the present application. Unless otherwise specified, the reagents and raw materials used can be purchased through commercial channels. The experimental methods in the following examples that do not specify specific conditions are selected according to conventional methods and conditions, or according to the product specifications.

[0051] In the following examples, the scanning electron microscope images were characterized by a scanning electron microscope model GAIA3 produced by Tesken Corporation.

[0052] Example 1

[0053] The magnesium-based composite implant of this embodiment is composed of the following components by weight: 1 part of ferroferric oxide, wherein the particle size of the ferroferric oxide is 10 microns to 50 microns, and 99 parts of a magnesium alloy. The magnesium alloy comprises 1wt% aluminum, 3wt% zinc, and the rest magnesium.

[0054] The preparation method of the magnesium-based composite material implant of this embodiment comprises the following steps:

[0055] (1) heating pure magnesium, pure zinc and pure aluminum in a mass ratio of 96:3:1 to 700° C. under the protection of a mixed gas of carbon dioxide and sulfur hexafluoride (volume ratio of 50:1) to melt and mix the raw materials to obtain a magnesium alloy melt, and cooling the magnesium alloy melt to 550° C. to form a semi-solid slurry;

[0056] (2) stirring the semi-solid slurry at a rate of 350 r / min using a stirring paddle, adding ferroferric oxide preheated to 400° C. into the semi-solid slurry to obtain a magnesium-based composite material melt;

[0057] (3) casting the magnesium-based composite material melt into a mold to obtain a magnesium-based composite material ingot;

[0058] (4) The magnesium-based composite material ingot is homogenized at a temperature of 420° C. for 12 hours, and the magnesium-based composite material ingot after the homogenization treatment is processed into a cylinder with a diameter of 85 mm, and then hot extruded at 300° C. at an extrusion speed of 2 m / min to obtain a magnesium-based composite material implant wire with a diameter of 1.5 mm.

[0059] The scanning electron microscope image of the magnesium-based composite implant wire of this embodiment is shown in Figure 1 .Depend on Figure 1 It can be seen that ferroferric oxide is evenly distributed in the magnesium matrix.

[0060] The magnesium-based composite implant wire of this embodiment was subjected to a magnetic induction heating test using an induction coil (80 mm in diameter and 6 turns). The test results showed that the magnesium-based composite implant wire could be heated to 68.032°C under an alternating magnetic field with a magnetic field strength of 1000 A / m and an alternating frequency of 380 kHz.

[0061] The magnesium-based composite implant wire of this embodiment was immersed in a 0.9wt.% sodium chloride solution for degradation test. The degradation rate was calculated by the immersion weight loss method, degradation rate = weight lost after degradation (mg / cm2 / day) × 2.1. The test results showed that the degradation rate of the magnesium-based composite implant wire was 200mg / cm 2 / sky.

[0062] Example 2

[0063] The magnesium-based composite implant of this embodiment is composed of the following components by weight: 10 parts of ferroferric oxide, wherein the particle size of the ferroferric oxide is 10 microns to 50 microns, and 90 parts of a magnesium alloy. The magnesium alloy comprises 1wt% aluminum, 3wt% zinc, and the rest magnesium.

[0064] The preparation method of the magnesium-based composite material implant of this embodiment comprises the following steps:

[0065] (1) heating pure magnesium, pure zinc and pure aluminum in a mass ratio of 96:3:1 to 700° C. under the protection of a mixed gas of carbon dioxide and sulfur hexafluoride (volume ratio of 50:1) to melt and mix the raw materials to obtain a magnesium alloy melt, and cooling the magnesium alloy melt to 550° C. to form a semi-solid slurry;

[0066] (2) stirring the semi-solid slurry at a rate of 350 r / min using a stirring paddle, adding ferroferric oxide preheated to 400° C. into the semi-solid slurry to obtain a magnesium-based composite material melt;

[0067] (3) casting the magnesium-based composite material melt into a mold to obtain a magnesium-based composite material ingot;

[0068] (4) The magnesium-based composite material ingot is homogenized at a temperature of 420° C. for 12 hours, and the magnesium-based composite material ingot after the homogenization treatment is processed into a cylinder with a diameter of 85 mm, and then hot extruded at 300° C. at an extrusion speed of 2 m / min to obtain a magnesium-based composite material implant wire with a diameter of 1.5 mm.

[0069] The scanning electron microscope image of the magnesium-based composite implant wire of this embodiment is shown in Figure 2 .Depend on Figure 2 It can be seen that ferroferric oxide is evenly distributed in the magnesium matrix.

[0070] The magnesium-based composite implant wire of this embodiment was subjected to a magnetic induction heating test using an induction coil (80 mm in diameter and 6 turns). The test results showed that the magnesium-based composite implant wire could be heated to 63.418°C under an alternating magnetic field with a magnetic field strength of 1000 A / m and an alternating frequency of 380 kHz.

[0071] The magnesium-based composite implant wire of this embodiment was immersed in a 0.9wt.% sodium chloride solution for degradation testing. The test results showed that the degradation rate of the magnesium-based composite implant wire was 150mg / cm 2 / sky.

[0072] Comparative Example 1

[0073] This comparative example provides a magnesium alloy, the composition of which is: 1wt% aluminum, 3wt% zinc, and the rest is magnesium.

[0074] The preparation method of the magnesium alloy of this comparative example comprises the following steps:

[0075] (1) heating pure magnesium, pure zinc and pure aluminum in a mass ratio of 96:3:1 to 700° C. under the protection of a mixed gas of carbon dioxide and sulfur hexafluoride (volume ratio of 50:1) to melt and mix the raw materials to obtain a magnesium alloy melt;

[0076] (2) casting the magnesium alloy melt into a mold to obtain a magnesium alloy ingot;

[0077] (4) The magnesium alloy ingot is subjected to a homogenization treatment at a temperature of (same as in Example 1) and a time of (same as in Example 1). The magnesium alloy ingot after the homogenization treatment is processed into a cylinder with a diameter of 85 mm, and then hot extruded at 300° C. at an extrusion speed of 2 m / min to obtain a magnesium alloy wire with a diameter of 1.5 mm.

[0078] The scanning electron microscope image of the magnesium alloy wire of this comparative example is shown in Figure 3 .Depend on Figure 3 It can be seen that the alloy is a single-phase magnesium alloy without second phase particles.

[0079] The magnesium alloy wire of this comparative example was subjected to a magnetic induction heating test using an induction coil (80 mm in diameter and 6 turns). The test results showed that the magnesium alloy wire could only be heated to 30.902°C under an alternating magnetic field with a magnetic field strength of 1000 A / m and an alternating frequency of 380 kHz.

[0080] The magnesium alloy wire of this comparative example was immersed in a 0.9wt.% sodium chloride solution for degradation test. The test results showed that the degradation rate of the magnesium alloy wire was 9mg / cm 2 Since there are no second phase particles in the magnesium alloy of this comparative example, no micro-galvanic effect is generated to accelerate the corrosion degradation rate, so its degradation rate is relatively low.

[0081] It can be seen that adding ferroferric oxide to magnesium alloys can greatly increase the heating temperature and degradation rate.

[0082] Example 3

[0083] The tumor inhibition effects of the magnesium-based composite material implant wire of Example 1 and the magnesium alloy wire of Comparative Example 1 were tested through animal experiments.

[0084] The tumor volume of the nude mouse subcutaneous pancreatic cancer model is about 50mm 3 When the tumor inhibition effect of magnesium-based composite implant wire and magnesium alloy wire was compared. Tumor-bearing nude mice were divided into three groups, with 5 mice in each group. In the first group, 2 magnesium-based composite implant wires (diameter 1.5 mm, length 5 mm) in Example 1 were implanted into the tumor of each tumor-bearing nude mouse; in the second group, 2 magnesium alloy wires (diameter 1.5 mm, length 5 mm) in Comparative Example 1 were implanted into the tumor of each tumor-bearing nude mouse; the third group was a blank control group. The tumor volume was measured with a vernier caliper every 4 days, and the changes in tumor volume were monitored for a total of 28 days.

[0085] like Figure 4 As shown in the figure, by comparing the tumor growth curves of tumor-bearing mice implanted with magnesium-based composite implant wires, magnesium alloy wires and non-implanted tumor-bearing mice (Control), it can be seen that the degradation of magnesium alloys can inhibit tumor growth, and magnesium-based composite materials with faster degradation rates have better anti-tumor effects than magnesium alloys.

[0086] Example 4

[0087] Animal experiments were conducted to test the inhibitory effects of the magnesium-based composite implant wire of Example 1 and the magnesium alloy wire of Comparative Example 1 on larger tumors under induction heating.

[0088] When the tumor volume of the nude mouse subcutaneous pancreatic cancer model grows to about 120 mm 3 When the induction heating time is about 20min, the tumor inhibition effect of the magnesium-based composite implant wire of Example 1 and the magnesium alloy wire of Comparative Example 1 are compared. The tumor-bearing nude mice were divided into three groups, with 5 mice in each group. The first group implanted 2 magnesium-based composite implant wires (1.5mm in diameter and 5mm in length) in Example 1 into the tumor of each tumor-bearing nude mouse; the second group implanted 2 magnesium alloy wires (1.5mm in diameter and 5mm in length) in Comparative Example 1 into the tumor of each tumor-bearing nude mouse; the third group was a blank control group. Immediately after implantation, the mice were placed in an alternating magnetic field generated by an induction coil with a diameter of 80mm and 5 turns. The magnetic field strength was about 1500A / m, and the heating time was 5 minutes. The tumor volume was measured with a vernier caliper every 4 days, and the changes in tumor volume were monitored for a total of 20 days. If the mouse tumor volume exceeded 1000mm 3 , it was euthanized for animal ethical considerations.

[0089] like Figure 5 As shown in the figure, by comparing the tumor growth curves of tumor-bearing mice implanted with magnesium-based composite implant wires, magnesium alloy wires, and unimplanted tumor-bearing mice (Control), it can be seen that induction heating can effectively inhibit the growth of larger tumors through thermal ablation. Under the same heating parameters, magnesium-based composite implant wires have better anti-tumor effects than magnesium alloy wires.

[0090] The above description of the embodiments is to facilitate those of ordinary skill in the art to understand and apply the present application. It is obvious that those familiar with the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without having to pay creative labor. Therefore, the present application is not limited to the embodiments herein, and improvements and modifications made by those skilled in the art based on the contents disclosed in the present application without departing from the scope and spirit of the present application are within the scope of the present application.

Claims

1. An anti-tumor magnesium-based composite material implant, It is characterized in that In terms of weight, the composition of the anti-tumor magnesium-based composite material implant is: x parts of ferrosoferric oxide, with 0<x≤10, and the rest is magnesium alloy, and the composition of the magnesium alloy is: 1~3wt% aluminum, 3~5wt% zinc, and the rest is magnesium.

2. The anti-tumor magnesium-based composite material implant according to claim 1, It is characterized in that The magnesium-based composite material implant comprises, by weight, 1 to 8 parts of ferrosoferric oxide and the rest of magnesium alloy.

3. The anti-tumor magnesium-based composite material implant according to claim 1, It is characterized in that The particle size of the ferrosoferric oxide is 1 micron to 50 microns.

4. A method for preparing a magnesium-based composite implant, It is characterized in that Used to prepare the anti-tumor magnesium-based composite material implant according to any one of claims 1 to 3, the preparation method comprising: The raw materials for preparing the magnesium alloy are heated to a first temperature under the protection of a protective gas, the raw materials are melted and mixed to obtain a magnesium alloy melt, and the magnesium alloy melt is cooled to a second temperature; adding ferroferric oxide preheated to a third temperature into the cooled magnesium alloy melt to obtain a magnesium-based composite material melt; Casting the magnesium-based composite material melt into a mold to obtain a magnesium-based composite material ingot; The magnesium-based composite material ingot is homogenized and then formed to obtain the anti-tumor magnesium-based composite material implant.

5. The method for preparing a magnesium-based composite implant according to claim 4, It is characterized in that The preparation method satisfies at least one of the following conditions: a. The raw materials for preparing the magnesium alloy include pure magnesium, pure zinc and pure aluminum; b. The protective gas comprises a mixture of carbon dioxide and sulfur hexafluoride or a mixture of argon and sulfur hexafluoride; c. The first temperature is 680°C to 750°C; d. The second temperature is 500°C to 650°C.

6. The method for preparing a magnesium-based composite implant according to claim 4, It is characterized in that The preparation method satisfies at least one of the following conditions: A. The third temperature is 300°C to 500°C; B. The stirring rate when adding the ferrosoferric oxide is 300 r / min~500 r / min.

7. The method for preparing a magnesium-based composite implant according to claim 4, It is characterized in that The preparation method satisfies at least one of the following conditions: (1) The homogenization treatment is performed at a temperature of 300° C. to 420° C. for a time of 8 to 20 hours; (2) The molding process is performed at a temperature of 250°C to 350°C.

8. Use of the anti-tumor magnesium-based composite material implant according to any one of claims 1 to 3 for preparing anti-tumor materials, It is characterized in that The degradation rate of the magnesium-based composite implant in the organism is 100 mg / cm 2 / day~200mg / cm 2 / sky.

9. Use of the anti-tumor magnesium-based composite material implant according to any one of claims 1 to 3 for preparing a magnetothermal induction medium, It is characterized in that The anti-tumor magnesium-based composite material implant is subjected to magnetic induction heating through an alternating magnetic field.

10. The use according to claim 9, It is characterized in that The magnetic field strength of the alternating magnetic field is 500A / m~1500A / m, the alternating frequency is 330kHz~430kHz, the heating temperature of the anti-tumor magnesium-based composite material implant is 60℃~80℃, and the degradation rate of the anti-tumor magnesium-based composite material implant in the organism is 100mg / cm 2 / day~200mg / cm 2 / sky.

Citation Information

Patent Citations

  • Biodegradable macromolecule composite material with shape memory function and its preparation method and use

    CN101240116A

  • Method for preparing magnesium-based composite hydrogen storage material in magnetic field

    CN101279716A

  • Composite material, and method for manufacturing the same

    CN101981631A

  • Magnetic bone cement material and method for preparing magnetic bone cement

    CN102671245A

  • Multiphase hybrid micro-nano structure magnetic composite material and preparation method thereof

    CN106075589A