PMDQ, NTDQ, PTDQ and preparation method and application thereof
By using carboxylic dianhydride and 2,6-diaminoanthraquinone in lithium-ion battery electrode materials to synthesize PMDQ, NTDQ, and PTDQ at a molar ratio of 1:2, the problem of easy solubility and low conductivity of small molecule quinone materials was solved problem, achieving higher electrochemical performance and cycle stability, and is suitable for lithium-ion battery cathode materials.
Patent Information
- Application Number
- CN202310197202.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-03
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-03-03
AI Technical Summary
There is still room for improvement in the application of existing lithium-ion battery electrode materials in lithium-ion batteries, especially the problems of small-molecule quinone materials that are easy to dissolve, have low conductivity, and poor cycle performance.
Carboxylic dianhydride and 2,6-diaminoanthraquinone are used to perform a reflux reaction at a molar ratio of 1:2 to synthesize PMDQ, NTDQ, and PTDQ. These products have anthraquinone structures at both ends and are used as cathode materials for lithium ion batteries. , forming electrodes by mixing with acetylene black and polyvinylidene fluoride and coating onto aluminum foil.
It improves the electronic conductivity and cycle performance of lithium-ion battery cathode materials, has high yield and low cost, avoids complex synthesis steps and high equipment requirements, the preparation method is simple and easy, and the material uniformity and electrochemical performance are significantly improved.
Smart Images

Figure CN116082345B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium ion battery materials, and specifically relates to PMDQ, NTDQ, PTDQ and a preparation method and application thereof. Background Art
[0002] With the progress of society and the rapid development of economy, people's dependence on and demand for energy are increasing. In recent years, lithium-ion batteries have been widely used in electronic equipment, industrial fields, and aerospace fields due to their advantages such as high specific energy, high energy storage efficiency, long cycle life, wide operating temperature range, and safety and reliability. Due to the shortage of mineral resources and the deterioration of the ecological environment, organic materials with flexible structural design, large specific capacity, high energy density, and environmental friendliness have gradually become the focus of researchers on lithium-ion battery electrode materials. Among them, carbonyl compounds have been widely explored by researchers because of their advantages of high capacity and fast kinetics. Quinones are an important component of carbonyl compounds. Quinone compounds have the advantages of large theoretical specific capacity, strong electrochemical reversibility, and structural diversity. They have great potential to achieve high rate capability and long-term cycle stability. Quinone electrodes are usually not restricted by ion selection, making quinones and their derivatives promising candidate electrode materials for high-performance electrochemical energy storage devices. However, small molecule quinones are easily dissolved in electrolytes, which have the disadvantages of causing electrode material loss, low conductivity, and poor cycle performance.
[0003] Patent CN104810522A discloses an organic positive electrode active material, which is obtained by polymerizing two materials with oxidation active sites. The material not only has a large number of redox pairs, but also has a high molecular weight, which solves the problem of dissolution of small organic molecules. The material can be used to prepare alkali metal ion batteries or alkaline earth metal ion batteries.
[0004] Patent CN106328949A discloses an organic electrode material, which includes an anhydride part and an electrochemically active diamine part, wherein the anhydride is one or more of pyromellitic acid anhydride, naphthalene tetracarboxylic acid anhydride or perylene tetracarboxylic acid anhydride; the diamine is one or two of 2,6-diaminoanthraquinone and 1,4-diamino-2,3-dicyanoanthraquinone. The organic electrode material can be applied to sodium ion batteries, which increases the voltage of the material and increases the capacity of the material by increasing the electrochemical active centers of the material.
[0005] However, the above-mentioned organic electrode materials are all linear polymers obtained under the condition of a raw material ratio of about 1:1, and their application effect in lithium-ion battery materials still has room for further improvement. Summary of the invention
[0006] In view of the shortcomings and deficiencies of the above prior art, the primary purpose of the present invention is to provide a method for preparing PMDQ, NTDQ and PTDQ. The applicant unexpectedly found that when the molar ratio of the carboxylic acid dianhydride compound to diaminoanthraquinone reaches 1:2, the obtained product with an anthraquinone structure at both ends has better electrochemical properties than the linear polymer used as a positive electrode material for lithium ion batteries.
[0007] Another object of the present invention is to provide PMDQ, NTDQ and PTDQ prepared by the above method.
[0008] Another object of the present invention is to provide the application of the above-mentioned PMDQ, NTDQ, and PTDQ as positive electrode materials for lithium-ion batteries.
[0009] The purpose of the present invention is achieved through the following technical solutions:
[0010] A method for preparing PMDQ, NTDQ and PTDQ, comprising the following preparation steps:
[0011] The pyromellitic anhydride, 1,4,5,8-naphthalenetetracarboxylic anhydride and perylenetetracarboxylic anhydride are added to a solvent respectively, stirred and dissolved uniformly, heated, and then 2,6-diaminoanthraquinone is added and stirred and refluxed for reaction, wherein the molar ratio of pyromellitic anhydride, 1,4,5,8-naphthalenetetracarboxylic anhydride or perylenetetracarboxylic anhydride to 2,6-diaminoanthraquinone is 1:2-2.5, and the product is washed and dried to obtain 2,6-bis(6-amino-9,10-dioxy-9,10-dihydroanthraquinone-2-yl)pyrrolo[4,3-f]isoindole-1,3,5,7-tetraketone (P MDQ), 2,7-bis(6-amino-9,10-dioxyylidene-9,10-dihydroanthracen-2-yl)-1,2,3,6,7,8-hexahydroisoquinolino[6,5,4-def]isoquinoline-1,3,6,8-tetraone (NTDQ), 2,9-bis(6-amino-9,10-dioxyylidene-9,10-dihydroanthracen-2-yl)-1,2,3,8,9,10-hexahydroisoquinolino[6',5',4':9,1,2]anthraceno[6,5,10-def]isoquinoline-1,3,8,10-tetraone (PTDQ).
[0012] More preferably, the solvent is N,N-dimethylformamide.
[0013] More preferably, the molar ratio of the pyromellitic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride or perylenetetracarboxylic dianhydride to 2,6-diaminoanthraquinone is 1:2.
[0014] More preferably, the heating temperature is 120-160°C.
[0015] Further preferably, the stirring reflux reaction is carried out under N2 protection conditions, and the stirring reflux reaction time is 1 to 10 days.
[0016] Further preferably, the cleaning refers to cleaning with methanol and acetone; and the drying refers to drying at 40 to 80° C. for 10 to 24 hours.
[0017] A PMDQ, NTDQ, and PTDQ are prepared by the above method, and their structural formulas are as follows:
[0018]
[0019] The above-mentioned PMDQ, NTDQ and PTDQ are used as positive electrode materials for lithium-ion batteries.
[0020] Furthermore, the application steps are: PMDQ, NTDQ, PTDQ are mixed with acetylene black and polyvinylidene fluoride and ground respectively, then solvent is added for ball milling, the obtained paste is coated on aluminum foil, and dried to obtain a lithium ion battery positive electrode.
[0021] Preferably, the mass ratio of the mixed grinding of PMDQ, NTDQ or PTDQ with acetylene black and polyvinylidene fluoride is 50:40:10.
[0022] Preferably, the solvent for ball milling is N-methylpyrrolidone.
[0023] Preferably, the drying refers to drying in a drying oven at 80°C.
[0024] Preferably, the content of the PMDQ, NTDQ or PTDQ active substance is 2-5 mg.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] (1) The present invention uses three organic anhydrides to reflux with 2,6-diaminoanthraquinone to synthesize PMDQ, NTDQ, and PTDQ. The synthesis method is simple and easy, avoiding the cumbersome processing steps and high requirements for equipment in other synthesis technologies, and has low cost, high yield, energy saving and environmental protection.
[0027] (2) The PMDQ, NTDQ and PTDQ prepared by the present invention have a block structure and are synthesized relatively uniformly.
[0028] (3) The present invention uses a carboxylic acid dianhydride compound to react with diaminoanthraquinone at a molar ratio of 1:2, and improves its electronic conductivity by reacting with 2,6-diaminoanthraquinone. The resulting product has a two-terminal anthraquinone structure. Compared with linear polymers, the positive electrode material for lithium-ion batteries has higher conductivity, is not easily soluble in electrolytes, and has better cycle performance, further improving its overall electrochemical performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 are SEM images of PMDQ, NTDQ, and PTDQ obtained in Example 1 at different magnifications;
[0030] Figure 2 is the XRD pattern of PMDQ, NTDQ and PTDQ obtained in Example 1;
[0031] Figure 3 is the TGA graph of PMDQ, NTDQ and PTDQ obtained in Example 1;
[0032] Figure 4 1 is a cyclic voltammetry curve of the PMDQ, NTDQ and PTDQ electrodes obtained in Example 1;
[0033] Figure 5 1 is a charge and discharge curve diagram of the PMDQ, NTDQ and PTDQ electrodes obtained in Example 1 at a current density of 0.1C;
[0034] Figure 6 This is a cycle performance curve diagram of the PMDQ, NTDQ, and PTDQ electrodes obtained in Example 1. DETAILED DESCRIPTION
[0035] The present invention is further described in detail below in conjunction with embodiments and drawings, but the embodiments of the present invention are not limited thereto.
[0036] Example 1
[0037] 0.22 g of pyromellitic anhydride, 0.27 g of 1,4,5,8-naphthalenetetracarboxylic anhydride and 0.39 g of perylenetetracarboxylic anhydride were added into 40 ml of DMF respectively, stirred and dissolved evenly, and heated to 140°C. 0.48 g of 2,6-diaminoanthraquinone was added into the three solutions respectively, stirred and refluxed under N2 atmosphere for 7 days, and the products were washed with methanol and acetone and dried at 60°C for 12 hours to obtain PMDQ, NTDQ and PTDQ respectively.
[0038] The SEM images of PMDQ, NTDQ and PTDQ obtained in this example at different magnifications are shown in Figure 2. Figure 1 As shown in a, b, and c in Figure 1. SEM images show that PMDQ, NTDQ, and PTDQ all have block structures.
[0039] The XRD patterns and TGA patterns of PMDQ, NTDQ and PTDQ obtained in this example are shown in Figures 1 and 2. Figure 2 and Figure 3 As shown, it is shown that PMDQ, NTDQ, and PTDQ are organic quinone compounds with a crystal structure and good heat resistance.
[0040] The application performance test of PMDQ, NTDQ and PTDQ obtained in this example as positive electrodes of lithium-ion batteries:
[0041] (1) The PMDQ, NTDQ, and PTDQ obtained in this example were ground with acetylene black and polyvinylidene fluoride in a mass ratio of 50:40:10 in an agate mortar for 30 minutes, and the mixture was poured into an agate ball ink tank, and an appropriate amount of N-methylpyrrolidone was added and ball milled for 4 hours. The obtained paste was applied to aluminum foil, and then placed in a drying oven at 80°C for about 12 hours, and cut into discs, and dried in a vacuum drying oven to obtain a working electrode. The content of active substances in the PMDQ, NTDQ, and PTDQ electrodes was about 4 mg respectively.
[0042] (2) A two-electrode system was used, wherein the working electrode prepared in step (1) was the positive electrode, the lithium sheet was the negative electrode, the Celgard 2300 microporous film was the separator, and 1M LiPF6-EC+DMC solution (V EC :V DMC =1:1) as the electrolyte, and the button cells were assembled in a glove box filled with argon.
[0043] (3) Cyclic voltammetry test: The battery obtained in step (2) has the following test conditions: a scan rate of 0.1 mV / s and a scan potential range of 1 to 4 V.
[0044] (4) The battery obtained in step (2) was subjected to constant current charge and discharge test, and the test condition parameters were: constant current charge current density of 0.1C, charge and discharge potential range of 1 to 4 V. All charge and discharge performance tests were carried out at room temperature.
[0045] After testing, the cyclic voltammetry curves of the obtained PMDQ, NTDQ, and PTDQ electrodes are as follows: Figure 4 As shown in a, b, and c, Figure 4 From (a), we can conclude that PMDQ has two groups of reduction peaks at 1.72V and 1.87V, and two groups of oxidation peaks at 1.99V and 2.10V. Figure 4 From (b), we can conclude that NTDQ has two groups of reduction peaks at 1.75V and 2.20V, and two groups of oxidation peaks at 2.12V and 2.80V. Figure 4 In (c), it can be concluded that PTDQ has two groups of reduction peaks at 1.65V and 1.80, and the corresponding two groups of oxidation peaks are located at 1.86V and 2.32V; the cyclic voltammetry curves of PMDQ, NTDQ, and PTDQ have good coincidence in the last three circles, indicating that the subsequent cycle capacity is relatively stable. The charge and discharge curves of PMDQ, NTDQ, and PTDQ electrodes at 0.1C current density are shown in the figure below. Figure 5 As shown by Figure 5It can be concluded that PMDQ is 50mAh·g -1 At a current density of 1.5, the discharge capacity of the first cycle is 172 mAh g -1 After 200 cycles, the battery decays to 120 mAh g -1 ;NTDQ at 200mAh·g -1 At a current density of , the discharge capacity of the first cycle is 190 mAh g -1 After 200 cycles, the battery decays to 155 mAh g -1 ;PTDQ at 50mAh·g -1 At a current density of , the discharge capacity of the first cycle is 287 mAh g -1 After 200 cycles, the battery decays to 195 mAh g -1 The cycle performance curves of PMDQ, NTDQ and PTDQ electrodes are shown in Figure 2. Figure 6 As shown in a, b, and c, Figure 6 In (a), it can be concluded that PMDQ is 50mAh·g -1 At the current density, the initial capacity is 160 mAh g -1 , 120mAh·g after 200 cycles -1 ;Depend on Figure 6 In (b), it can be concluded that NTDQ is 200mAh·g -1 At the current density, the initial capacity is 190 mAh g -1 , 150mAh·g after 200 cycles -1 ,Depend on Figure 6 In (c), it can be concluded that PTDQ is 50 mAh g -1 At the current density, the initial capacity is 275 mAh g -1 , after 100 cycles, there is still 220mAh·g -1 From the above results, it can be seen that the PMDQ, NTDQ and PTDQ electrodes obtained in the present invention have good electrochemical properties.
[0046] Example 2
[0047] 0.22 g of pyromellitic anhydride, 0.27 g of 1,4,5,8-naphthalenetetracarboxylic anhydride and 0.39 g of perylenetetracarboxylic anhydride were added to 40 ml of DMF respectively, stirred and dissolved evenly, and heated to 120°C. 0.60 g of 2,6-diaminoanthraquinone was added to the three solutions respectively, stirred and refluxed under N2 atmosphere for 7 days, and the products were washed with methanol and acetone and dried at 40°C for 10 hours to obtain PMDQ, NTDQ and PTDQ respectively.
[0048] The application performance test results of PMDQ, NTDQ and PTDQ obtained in this embodiment as positive electrode materials for lithium-ion batteries are basically the same as those in Example 1 and are not listed one by one.
[0049] Example 3
[0050] 0.22 g of pyromellitic anhydride, 0.27 g of 1,4,5,8-naphthalenetetracarboxylic anhydride and 0.39 g of perylenetetracarboxylic anhydride were added into 40 ml of DMF respectively, stirred and dissolved evenly, and heated to 160°C. 0.52 g of 2,6-diaminoanthraquinone was added into the three solutions respectively, stirred and refluxed under N2 atmosphere for 7 days, and the products were washed with methanol and acetone and dried at 80°C for 24 hours to obtain PMDQ, NTDQ and PTDQ respectively.
[0051] The application performance test results of PMDQ, NTDQ and PTDQ obtained in this embodiment as positive electrode materials for lithium-ion batteries are basically the same as those in Example 1 and are not listed one by one.
[0052] Comparative Example 1
[0053] Compared with Example 1, the molar ratio of the addition amount of pyromellitic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride, perylenetetracarboxylic dianhydride and 2,6-diaminoanthraquinone in this comparative example is 1:1, and the specific steps are as follows:
[0054] 0.22 g of pyromellitic anhydride, 0.27 g of 1,4,5,8-naphthalenetetracarboxylic anhydride and 0.39 g of perylenetetracarboxylic anhydride were added to 40 ml of DMF respectively, stirred and dissolved evenly, and heated to 140°C. 0.24 g of 2,6-diaminoanthraquinone was added to the three solutions respectively, stirred and refluxed under N2 atmosphere for 7 days, and the products were washed with methanol and acetone and dried at 60°C for 12 hours to obtain products PMDQ-1, NTDQ-1 and PTDQ-1 respectively.
[0055] The application performance of the product obtained in this comparative example as a positive electrode material for lithium-ion batteries was tested according to the method of Example 1. The results showed that PMDQ-1 had a positive electrode performance of 50 mAh·g -1 At the current density, the initial capacity is 130 mAh g -1 , 110mAh·g after 200 cycles -1 ; NTDQ-1 at 200mAh·g -1 At the current density, the initial capacity is 160 mAh g -1 , 200 cycles still have 50mAh·g -1 ;PTDQ-1 at 50mAh·g -1 At the current density, the initial capacity is 139 mAh g -1 , after 100 cycles, there is still 135mAh·g -1. From the above results, it can be seen that the electrochemical performance of the product obtained by the reaction of the carboxylic acid dianhydride compound and diaminoanthraquinone at a molar ratio of 1:2 is further significantly improved compared with the linear polymer obtained under the condition of 1:1, especially the effect of PTDQ is particularly significant. The reason may be that the product obtained under the condition of 1:2 has an anthraquinone structure at both ends, which is more conductive than linear polymers when used as positive electrode materials for lithium-ion batteries, is not easily soluble in electrolytes, and has better cycle performance, which further improves its overall electrochemical performance, and the performance of products containing perylene ring structures is further significantly improved compared with products with benzene ring structures and naphthalene ring structures.
[0056] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. An application of PMDQ as a positive electrode material for a lithium-ion battery, characterized in that: The PMDQ is prepared by the following method: Add pyromellitic acid dianhydride to the solvent, stir and dissolve evenly, heat, then add 2,6-diaminoanthraquinone, stir and reflux for reaction, wherein the molar ratio of pyromellitic acid dianhydride to 2,6-diaminoanthraquinone is 1:2-2.5, wash and dry the product to obtain PMDQ; the structural formula of the PMDQ is as follows: 。 2. The use of PMDQ as a positive electrode material for lithium-ion batteries according to claim 1, characterized in that: The application steps are: PMDQ is mixed with acetylene black and polyvinylidene fluoride and ground respectively, then a solvent is added for ball milling, the obtained paste is coated on aluminum foil, and dried to obtain a positive electrode of a lithium ion battery.
3. The use of PMDQ as a positive electrode material for lithium-ion batteries according to claim 2, characterized in that: The mass ratio of the mixed grinding of PMDQ, acetylene black and polyvinylidene fluoride is 50:40:10; the solvent of the ball milling is N-methylpyrrolidone; the drying refers to drying in a drying oven at 80° C.; the content of the PMDQ active substance is 2-5 mg.