A method for preparing iron phosphate from lithium phosphate

By stirring and reacting in an acidic solution of lithium phosphate and an iron source to generate iron phosphate precipitate, the problems of high solution viscosity and insufficient utilization of raw materials in iron phosphate production are solved, and high-purity and high-yield iron phosphate preparation is achieved, which provides the basis for subsequent The preparation of lithium carbonate provides a pure solution suitable for industrial production.

CN116101991BActive Publication Date: 2024-10-15HEFEI GUOXUAN CIRCULATION TECH CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202211696368.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-28
Publication Date
2024-10-15
Estimated Expiration
2042-12-28

AI Technical Summary

Technical Problem

In the existing iron phosphate production process, the concentration of the solution after synthesis of the iron phosphate product is too high, which makes it difficult to filter and wash, affects the purity of the product, and the raw materials are not fully utilized, which increases the production cost.

Method used

By adding solid lithium phosphate to an acidic solution containing an iron source and stirring the reaction, iron phosphate precipitation is generated, which reduces the viscosity of the reaction solution to facilitate subsequent filtration and washing. Stirring reaction and solid-liquid separation are performed under acidic conditions, and then the pH is adjusted to 1 -2. Let it stand for aging to obtain iron phosphate with higher purity and yield, and use the filtrate to precipitate lithium to provide a pure solution.

Benefits of technology

It achieves the preparation of iron phosphate with higher purity and yield, reduces the viscosity of the iron phosphate solution, simplifies the washing process, improves the utilization rate of raw materials, is suitable for large-scale industrial production, and provides a pure solution for the subsequent preparation of lithium carbonate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116101991B_ABST
    Figure CN116101991B_ABST
Patent Text Reader

Abstract

The present invention proposes a method for preparing iron phosphate from lithium phosphate, comprising: adding solid lithium phosphate to an acidic solution containing an iron source and stirring the solution to obtain a mixture solution; after solid-liquid separation of the mixture solution obtained above, the obtained solid is iron phosphate, which is iron phosphate dihydrate, and after roasting, anhydrous iron phosphate is obtained, which can be used for battery electrodes. The present invention proposes a method for preparing iron phosphate from lithium phosphate. While preparing more and purer iron phosphate, the method provides a pure solution for precipitating lithium in the filtrate, which not only helps the subsequent preparation of lithium carbonate, but the overall method also effectively achieves the requirements of low cost and high environmental protection.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electrode material production, and in particular to a method for preparing iron phosphate from lithium phosphate. Background Art

[0002] Lithium iron phosphate has become a popular lithium-ion cathode material due to its good stability and high safety. Due to its good stability and controllable process, it has gradually become an ideal precursor material for the synthesis of lithium iron phosphate in the industry.

[0003] In the prior art, the production of ferric phosphate is divided into various processes such as the sodium method, ammonium method, iron powder, and fertilizer phosphate method. The main route is to use trivalent or divalent iron salt as raw material, add phosphoric acid or phosphate salt, adjust the pH to generate ferric phosphate precipitate, then age it, wash the precipitate, and dry it to obtain the finished product.

[0004] However, in the above method, during the production of ferric phosphate, the solution concentration of the ferric phosphate product after synthesis is too high, resulting in high viscosity during filtration and washing, making it difficult to wash the product, and the washing is incomplete, affecting the purity of the product. In addition, the raw materials are not fully utilized, and there are many impurities in the filtrate, which increases the difficulty of processing and increases the production cost. Summary of the invention

[0005] Based on the technical problems existing in the background technology, the present invention proposes a method for preparing iron phosphate from lithium phosphate. The method not only prepares more and purer iron phosphate, but also provides a pure solution for lithium precipitation in the filtrate, which not only helps the subsequent preparation of lithium carbonate, but the overall method also effectively achieves the requirements of low cost and high environmental protection.

[0006] The present invention proposes a method for preparing iron phosphate from lithium phosphate, comprising: S1, adding solid lithium phosphate to an acidic solution containing an iron source and stirring the mixture solution to obtain a mixture solution; S2, separating the mixture solution obtained in step S1 into solid and liquid, and the obtained solid is iron phosphate.

[0007] In the present invention, solid lithium phosphate is added to an acidic solution containing an iron source and stirred for reaction, lithium phosphate gradually dissolves in the acidic solution containing the iron source, local high-concentration phosphate directly reacts with iron ions to generate iron phosphate precipitation and reaction, a small amount of phosphate ions and iron ions exist in the solution, so the obtained reaction solution has low viscosity, which is helpful for subsequent filtering and washing of the iron phosphate, so as to obtain iron phosphate with higher purity and yield; thereby avoiding the defects in the prior art that when lithium phosphate reacts with an iron source solution in the form of a slurry or a solution, the concentration of the obtained reaction solution is too high due to the excessively violent reaction, resulting in high viscosity of the solution during filtering and washing, and difficulty in filtering and washing the product.

[0008] Preferably, the iron source comprises a ferric iron source and / or a divalent iron source;

[0009] Preferably, the method further comprises adding an oxidant to the acidic solution containing the iron source;

[0010] Preferably, the oxidant is at least one of hypochlorous acid or hydrogen peroxide, and the amount thereof is preferably not less than the theoretical amount of the oxidant required to completely oxidize the divalent iron source into a trivalent iron source.

[0011] Preferably, the iron source is at least one of ferric chloride, ferric sulfate, ferrous sulfate or ferrous chloride.

[0012] Preferably, in S1, the pH of the acidic solution containing the iron source is not greater than 1, preferably less than 0.5.

[0013] Preferably, in S1, the iron-phosphorus molar ratio of the lithium phosphate and the iron source is 0.96-1;

[0014] Preferably, the stirring rate of the stirring reaction is 150-600 r / min.

[0015] Preferably, in S2, before the solid-liquid separation of the mixture solution obtained in S1, the pH of the mixture solution obtained is adjusted to 1-2, and then allowed to stand for aging;

[0016] Preferably, the temperature of the static aging is 50-70°C and the time is 20-60 minutes.

[0017] Preferably, the obtained solid is further washed, dried, and calcined to obtain iron phosphate;

[0018] Preferably, the washing is performed by rinsing with deionized water; the drying temperature is 100-105° C. and the time is 1-2 h; the calcination temperature is 600-700° C. and the time is 2-4 h.

[0019] Preferably, in S2, the liquid obtained by the solid-liquid separation is a lithium-containing mother liquor;

[0020] Preferably, the process further comprises concentrating and removing impurities from the lithium-containing mother liquor, adding carbonate, stirring for reaction, and then performing solid-liquid separation to obtain lithium carbonate.

[0021] Preferably, the concentration and impurity removal of the lithium-containing mother liquor specifically comprises: adjusting the pH of the lithium-containing mother liquor to 7-9, heating and concentrating until solid impurities are precipitated, filtering and removing the solid impurities to obtain a filtrate;

[0022] Preferably, the pH of the lithium-containing mother liquor is adjusted to 7-9 by adding an alkaline solution, and the alkaline solution is at least one of sodium hydroxide, potassium hydroxide or lithium hydroxide solution.

[0023] Preferably, the solid-liquid separation after adding carbonate and stirring the reaction specifically comprises: adding a saturated carbonate solution to the filtrate to precipitate lithium carbonate, and washing and drying the solid obtained after solid-liquid separation to obtain lithium carbonate.

[0024] Compared with the prior art, the present invention has the following excellent effects:

[0025] (1) The present invention discloses a method for preparing iron phosphate from lithium phosphate, wherein solid lithium phosphate is added to an iron source solution. After the lithium phosphate is dissolved by acid in the iron source solution, locally high-concentration phosphate directly reacts with iron ions to generate iron phosphate precipitates. A small amount of phosphate ions and iron ions exist in the solution, and the viscosity of the solution is reduced. The pH value is then adjusted to between 1 and 2 by alkali to completely precipitate the iron phosphate in the solution. After an aging process, the solid and liquid are separated, and the resulting filtrate is clear and transparent, providing a pure solution for lithium precipitation in the filtrate.

[0026] (2) The present invention optimizes the synthesis process of ferric phosphate, reduces the viscosity of ferric phosphate solution, facilitates separation, improves the utilization rate of raw materials, and is easy to operate, with no waste residue discharged during the preparation process, and is suitable for large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a flow chart of the method for preparing iron phosphate from lithium phosphate according to the present invention;

[0028] Figure 2 This is the XRD pattern of the iron phosphate prepared in Example 1 of the present invention;

[0029] Figure 3 The XRD pattern of lithium carbonate prepared in Example 1 of the present invention;

[0030] Figure 4 The diagram is a solution state diagram of the reaction solutions obtained in Example 1 of the present invention and Comparative Example 1 after standing and aging. DETAILED DESCRIPTION

[0031] The technical solutions of the present invention are described in detail below through specific embodiments. However, it should be clearly stated that these embodiments are for illustration only and are not to be construed as limiting the scope of the present invention.

[0032] Example 1

[0033] Reference Figure 1 It can be seen that a method for preparing iron phosphate and lithium carbonate from lithium phosphate comprises the following steps:

[0034] (1) adding ferric chloride to water to prepare an iron source solution having an iron ion concentration of 1.5 mol / L, and then adding hydrochloric acid to adjust the pH to 0.1 to obtain an acidic solution containing an iron source;

[0035] (2) adding solid lithium phosphate to the acidic solution containing the iron source at an iron-phosphorus molar ratio of 0.98, stirring at a rate of 300 r / min until the reaction is complete, adding sodium hydroxide to the resulting reaction solution to adjust the pH to 1.5, standing and aging at 70° C. for 20 min, and then filtering to separate the solid and the lithium-containing mother solution;

[0036] (3) washing the obtained solid with deionized water four times, drying it at 105° C. for 1 h, and then calcining it at 600° C. for 2 h to obtain iron phosphate;

[0037] (4) adding lithium hydroxide solution to the lithium-containing mother liquor to adjust the pH to 8, heating and concentrating to precipitate solid impurities, filtering to remove the solid impurities, adding 90° C. saturated sodium carbonate solution to the obtained filtrate and stirring to react, precipitating lithium carbonate, filtering to separate the solid, washing with 90° C. deionized water, and drying to obtain lithium carbonate.

[0038] Example 2

[0039] Reference Figure 1 It can be seen that a method for preparing iron phosphate and lithium carbonate from lithium phosphate comprises the following steps:

[0040] (1) adding ferrous sulfate and hydrogen peroxide solution (30 wt%) to water at a molar ratio of 1:1 to prepare an iron source solution with an iron ion concentration of 1.5 mol / L, and then adding hydrochloric acid to adjust the pH to 0.3 to obtain an acidic solution containing an iron source;

[0041] (2) adding solid lithium phosphate to the acidic solution containing the iron source at an iron-phosphorus molar ratio of 0.96, stirring at a rate of 600 r / min until the reaction is complete, adding sodium hydroxide to the resulting reaction solution to adjust the pH to 2, standing and aging at 50° C. for 60 min, and then filtering to separate the solid and the lithium-containing mother solution;

[0042] (3) washing the obtained solid with deionized water four times, drying it at 100° C. for 2 h, and then calcining it at 700° C. for 4 h to obtain iron phosphate;

[0043] (4) adding lithium hydroxide solution to the lithium-containing mother liquor to adjust the pH to 7, heating and concentrating to precipitate solid impurities, filtering to remove the solid impurities, adding 90° C. saturated sodium carbonate solution to the obtained filtrate and stirring to react, precipitating lithium carbonate, filtering to separate the solid, washing with 90° C. deionized water, and drying to obtain lithium carbonate.

[0044] Example 3

[0045] Reference Figure 1 It can be seen that a method for preparing iron phosphate and lithium carbonate from lithium phosphate comprises the following steps:

[0046] (1) adding ferric chloride to water to prepare an iron source solution having an iron ion concentration of 1.5 mol / L, and then adding hydrochloric acid to adjust the pH to 0.1 to obtain an acidic solution containing an iron source;

[0047] (2) adding solid lithium phosphate to the acidic solution containing the iron source at a molar ratio of iron to phosphorus of 1, stirring at a rate of 150 r / min until the reaction is complete, adding sodium hydroxide to the resulting reaction solution to adjust the pH to 1, standing and aging at 60° C. for 40 min, and then filtering to separate the solid and the lithium-containing mother solution;

[0048] (3) washing the obtained solid with deionized water four times, drying it at 105° C. for 1 h, and then calcining it at 650° C. for 3 h to obtain iron phosphate;

[0049] (4) adding sodium hydroxide solution to the lithium-containing mother liquor to adjust the pH to 9, heating and concentrating to precipitate solid impurities, filtering to remove the solid impurities, adding 90° C. saturated sodium carbonate solution to the obtained filtrate and stirring to react, precipitating lithium carbonate, filtering to separate the solid, washing with 90° C. deionized water, and drying to obtain lithium carbonate.

[0050] Example 4

[0051] Reference Figure 1 It can be seen that a method for preparing iron phosphate and lithium carbonate from lithium phosphate comprises the following steps:

[0052] (1) adding ferrous chloride and hydrogen peroxide solution (30 wt%) to water at a molar ratio of 1:1 to prepare an iron source solution having an iron ion concentration of 1.5 mol / L, and then adding hydrochloric acid to adjust the pH to 0.5 to obtain an acidic solution containing an iron source;

[0053] (2) adding solid lithium phosphate to the acidic solution containing the iron source at a molar ratio of iron to phosphorus of 0.99, stirring at a rate of 400 r / min until the reaction is complete, adding sodium hydroxide to the resulting reaction solution to adjust the pH to 1.5, standing and aging at 60° C. for 50 min, and then filtering to separate the solid and the lithium-containing mother solution;

[0054] (3) washing the obtained solid with deionized water four times, drying it at 105° C. for 1 h, and then calcining it at 700° C. for 1 h to obtain iron phosphate;

[0055] (4) adding potassium hydroxide solution to the lithium-containing mother liquor to adjust the pH to 8, heating and concentrating to precipitate solid impurities, filtering to remove the solid impurities, adding 90° C. saturated sodium carbonate solution to the obtained filtrate and stirring to react, precipitating lithium carbonate, filtering to separate the solid, washing with 90° C. deionized water, and drying to obtain lithium carbonate.

[0056] Comparative Example 1

[0057] A method for preparing iron phosphate and lithium carbonate from lithium phosphate comprises the following steps:

[0058] (1) adding lithium phosphate to a large amount of water, grinding and dispersing the lithium phosphate to prepare a lithium phosphate slurry; adding ferric chloride to water to prepare an iron source solution with an iron ion concentration of 1.5 mol / L, and then adding hydrochloric acid to adjust the pH to 0.1 to obtain an acidic solution containing an iron source;

[0059] (2) adding the lithium phosphate slurry to the acidic solution containing the iron source at an iron-phosphorus molar ratio of 0.98, stirring at a rate of 300 r / min until the reaction is complete, adding sodium hydroxide to the resulting reaction solution to adjust the pH to 1.5, standing and aging at 70° C. for 20 min, and then filtering to separate the solid and the lithium-containing mother liquor;

[0060] (3) washing the obtained solid with deionized water four times, drying it at 105° C. for 1 h, and then calcining it at 600° C. for 2 h to obtain iron phosphate;

[0061] (4) adding lithium hydroxide solution to the lithium-containing mother liquor to adjust the pH to 8, heating and concentrating to precipitate solid impurities, filtering to remove the solid impurities, adding 90° C. saturated sodium carbonate solution to the obtained filtrate and stirring to react, precipitating lithium carbonate, filtering to separate the solid, washing with 90° C. deionized water, and drying to obtain lithium carbonate.

[0062] The iron phosphate and lithium carbonate obtained in the above Examples 1-4 were subjected to X-ray diffraction analysis (XRD). The XRD results of the iron phosphate and lithium carbonate prepared in Example 1 were taken as representative. The results are as follows: Figure 2 and 3 shown; reference Figure 2 , 3 It can be seen that the diffraction peaks of the iron phosphate and lithium carbonate prepared by the present invention are completely consistent with the diffraction characteristic peaks in the standard iron phosphate card (77-0094) and lithium carbonate card (22-1141), and there is no impurity peak. At the same time, the diffraction peaks are sharp and the half-height width is narrow; this shows that the iron phosphate and lithium carbonate prepared by the present invention are pure phase iron phosphate and lithium carbonate with good crystallinity.

[0063] The state of the reaction solution after standing and aging in step (2) of Example 1 and step (2) of Comparative Example 1 was observed, and the results were as follows: Figure 4 As shown, it can be seen that the reaction solution obtained in Example 1 has a lower viscosity, and it is obviously stratified after standing. The supernatant is clear and transparent, easy to separate, and provides a relatively pure filtrate for lithium precipitation in the filtrate; the reaction solution obtained in the comparative example has a higher viscosity. Although some precipitation is produced, the upper liquid is still relatively turbid after standing, which is not conducive to separation, so it cannot provide a pure solution for lithium precipitation in the filtrate.

[0064] The lithium content and phosphorus content in the lithium carbonate, iron phosphate, filtrate and washing liquid prepared in Examples 1-4 and Comparative Example 1 were detected, and the total yield of lithium and the yield of phosphorus in Examples 1-4 and Comparative Example 1 were shown in Table 1 below:

[0065] Table 1: Total yield of lithium and yield of phosphorus in Examples 1-4 and Comparative Example 1

[0066]

[0067]

[0068] It can be seen from the above table that the total yield of lithium and the yield of phosphorus in the embodiment of the present invention are both above 97%, which can achieve effective recycling of lithium and phosphorus, and the small amount of residual lithium in the solution can be recycled.

[0069] The physical and chemical indicators of the iron phosphate and lithium carbonate prepared in Examples 1-4 and Comparative Example 1 were tested, and the results are shown in Tables 2 and 3 below.

[0070] Table 2 Comparison of the physical and chemical indicators of the iron phosphate prepared in Examples 1-4 and Comparative Example 1

[0071]

[0072]

[0073] It can be seen from the above table that the impurity content of the iron phosphate prepared in Examples 1-4 of the present invention is extremely low, and the chemical composition is quite different from that of the iron phosphate prepared in Comparative Example 1, and can meet the standard of anhydrous iron phosphate for lithium iron phosphate.

[0074] Table 3 Comparison of the physical and chemical indicators of lithium carbonate prepared in Examples 1-4 and Comparative Example 1

[0075] <![CDATA[Li 2 CO 3 ]]> Fe Ca Mg Na K <![CDATA[Cl - ]]> <![CDATA[SO 4 2- ]]> Example 1 99.56 0.003 0.002 0.001 0.018 0.002 0.007 0.24 Example 2 99.61 0.003 0.002 0.002 0.020 0.004 0.013 0.29 Example 3 99.57 0.003 0.003 0.002 0.022 0.004 0.015 0.30 Example 4 99.64 0.003 0.003 0.001 0.016 0.002 0.008 0.26 Comparative Example 1 99.01 0.004 0.005 0.004 0.047 0.008 0.021 0.035

[0076] It can be seen from the above table that the lithium carbonate prepared in Examples 1-4 of the present invention has extremely low impurity content and is of good battery grade quality and can meet normal use. The lithium carbonate prepared in Comparative Example 1 is of industrial grade and has a greater impact on battery quality when preparing positive electrode materials.

[0077] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing iron phosphate from lithium phosphate, characterized in that: include: S1, adding solid lithium phosphate to an acidic solution containing an iron source and stirring to react to obtain a mixture solution; S2, after solid-liquid separation of the mixture solution obtained in step S1, the obtained solid is ferric phosphate; In S1, the iron source includes a ferric iron source and / or a divalent iron source; the ferric iron source is at least one of ferric chloride and ferric sulfate, and the divalent iron source is at least one of ferrous sulfate and ferrous chloride; When the iron source includes a ferrous iron source, an oxidant is added to the acidic solution containing the iron source; the oxidant is at least one of hypochlorous acid or hydrogen peroxide, and the amount thereof is not less than the theoretical amount of the oxidant required to completely oxidize the ferrous iron source into a ferric iron source; The pH of the acidic solution containing the iron source is not greater than 1, and the iron-phosphorus molar ratio of the lithium phosphate and the iron source is 0.96-1.

2. The method for preparing iron phosphate from lithium phosphate according to claim 1, characterized in that: In S2, before the solid-liquid separation of the mixed solution obtained in S1, the pH of the mixed solution obtained is adjusted to 1-2, and then allowed to stand for aging.

3. The method for preparing iron phosphate from lithium phosphate according to claim 1, characterized in that: In S2, the obtained solid needs to be washed, dried, and calcined to obtain iron phosphate.

4. The method for preparing iron phosphate from lithium phosphate according to claim 1, characterized in that: In S2, the liquid obtained by the solid-liquid separation is a lithium-containing mother liquor. The lithium-containing mother liquor is concentrated and impurities are removed, and carbonate is added to stir the reaction and then the solid-liquid separation is performed to obtain lithium carbonate.

5. The method for preparing iron phosphate from lithium phosphate according to claim 4, characterized in that: The concentration and impurity removal of the lithium-containing mother liquor specifically includes: adjusting the pH of the lithium-containing mother liquor to 7-9, heating and concentrating until solid impurities are precipitated, filtering and removing the solid impurities to obtain a filtrate.

6. The method for preparing iron phosphate from lithium phosphate according to claim 5, characterized in that: The solid-liquid separation after adding carbonate and stirring the reaction specifically includes: adding a saturated carbonate solution to the filtrate to precipitate lithium carbonate, and washing and drying the solid obtained after solid-liquid separation to obtain lithium carbonate.

Citation Information

Patent Citations

  • Process for recovering lithium phosphorous from lithium phosphate crude product to prepare battery-level lithium carbonate and iron phosphate

    CN107720716A

  • Method for simultaneously producing iron phosphate and lithium carbonate from battery waste

    CN115180604A

  • Preparation method of lithium salt or positive electrode material of lithium ion battery and lithium ion battery

    CN115286020A

  • Regeneration process of positive electrode material of waste lithium iron phosphate battery

    CN115432681A

  • Method for producing high-concentration lithium liquid from lithium-containing liquid and method for producing lithium carbonate

    JP2011168461A