Conductive ink and preparation method thereof, plastic material and preparation method thereof, electroplated plastic

By adding resin binder, conductive filler and pore-forming agent to the conductive ink, a microporous ink layer is formed, which solves the problem of insufficient binding force and conductivity of the conductive ink in electroplated plastics, and realizes an efficient and environmentally friendly electroplating process. , avoiding the high pollution and high cost of traditional processes.

CN116120784BActive Publication Date: 2024-10-22XIAMEN XIHE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211698816.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-28
Publication Date
2024-10-22
Estimated Expiration
2042-12-28

AI Technical Summary

Technical Problem

The existing conductive inks have insufficient bonding force and conductivity in electroplated plastics, and the traditional electroplating process has problems of high pollution and high cost.

Method used

Using conductive ink containing resin binder, conductive filler and pore-forming agent, a microporous ink layer is formed through mixing and drying to improve the adhesion and conductivity of the ink layer, and the microporous structure is used to enhance the coating and plastic during the electroplating process the binding force.

Benefits of technology

It achieves good bonding force and conductivity of conductive ink in plastic electroplating, reduces process complexity and pollution, and does not require the use of chromium and palladium, making it suitable for large-scale promotion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004023227530000011
    Figure BDA0004023227530000011
  • Figure BDA0004023227530000041
    Figure BDA0004023227530000041
  • Figure BDA0004023227530000042
    Figure BDA0004023227530000042
Patent Text Reader

Abstract

The present invention provides conductive ink and preparation method, plastic material and preparation method, electroplated plastic, and relates to the field of material technology. Conductive ink, by weight, includes the following raw materials: 5 to 50 parts of resin binder; 1 to 30 parts of conductive filler; 1 to 25 parts of pore former; and 5 to 50 parts of solvent. The conductive ink provided by the present invention has good bonding force and conductivity. When applied to the electroplating of plastics, the process is chromium-free and palladium-free, with little pollution and a simple electroplating process, which effectively avoids the use of traditional technologies with complicated processes, high pollution and high costs containing chromium and palladium, and also improves the bonding force problem of the current direct electroplating technology.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of material technology, and in particular to conductive ink and a preparation method thereof, plastic material and a preparation method thereof, and electroplated plastic. Background Art

[0002] Conductive ink (Electrically Conductive Printing Ink) is a paste ink made by dispersing conductive materials in a binder. It has a certain degree of conductivity and can be used for printing conductive dots or conductive lines. Gold conductive ink, silver conductive ink, copper conductive ink, carbon conductive ink, etc. have reached practical application and are often used in printed circuits, electrodes, electroplating bases, keyboard contacts, printed resistors and other fields. Based on the wide application and universality of conductive inks, the industry has put forward higher requirements for the conductivity and bonding strength of conductive inks. Therefore, it is necessary to develop conductive inks with better performance. Summary of the invention

[0003] The object of the present invention is to provide a conductive ink and a preparation method thereof, wherein the conductive ink has good bonding force and conductivity.

[0004] Another object of the present invention is to provide a plastic material and a preparation method thereof.

[0005] Another object of the present invention is to provide electroplated plastic, wherein the plastic material of the electroplated plastic has good bonding strength with the metal coating.

[0006] The present invention solves the technical problem by adopting the following technical solutions:

[0007] Conductive ink, measured by weight, comprises the following raw materials:

[0008]

[0009] Optionally, in some embodiments of the present invention, the resin binder is selected from one or more of epoxy resin, polyurethane, alkyd resin, silicone resin, thermosetting acrylic resin, and thermoplastic acrylic resin; and / or

[0010] The conductive filler is selected from one or more of graphene microsheets, conductive carbon black, carbon nanotubes, expanded graphite, conductive carbon fiber, copper powder, nickel powder, silver powder, and silver-coated copper powder; and / or

[0011] The pore former is selected from one or more of a volatile pore former, a decomposition pore former, a dissolution pore former, and an etching pore former.

[0012] Optionally, in some embodiments of the present invention, the volatile pore-forming agent is selected from one or more of a low saturated vapor pressure solvent and a high boiling point solvent; the saturated vapor pressure of the low saturated vapor pressure solvent is lower than the saturated vapor pressure of the solvent, and the boiling point of the high boiling point solvent is higher than the boiling point of the solvent;

[0013] The decomposable pore-forming agent is selected from one or more of bicarbonate and carbonate;

[0014] The soluble pore-forming agent is selected from one or more of polyethylene glycol and urea;

[0015] The etching pore former is selected from one or more of metal oxides and silicon oxide.

[0016] Optionally, in some embodiments of the present invention, the raw material further comprises 1 to 3 parts of auxiliary agent by weight.

[0017] In addition, the preparation method of the conductive ink comprises:

[0018] The above-mentioned raw materials of conductive ink are mixed.

[0019] In addition, the method for preparing the plastic material comprises:

[0020] Providing a plastic substrate and the conductive ink;

[0021] The conductive ink is applied to the surface of the plastic substrate and dried.

[0022] Optionally, in some embodiments of the present invention, the thickness of the dry film formed by the conductive ink after drying is 1 to 500 μm; and / or

[0023] The drying temperature is 25 to 120°C and the drying time is 0.5 to 12 hours; and / or

[0024] The coating method is selected from one or more of spraying, scraping, pulling, wire rod, screen printing, and gravure printing; and / or

[0025] The drying method is selected from one or more of oven treatment, ultraviolet light treatment, and room temperature treatment.

[0026] In addition, the plastic material obtained by the above-mentioned method for preparing the plastic material includes:

[0027] Plastic base; and

[0028] An ink layer is formed on the surface of a plastic substrate.

[0029] Optionally, in some embodiments of the present invention, the ink layer includes a plurality of micropores, and the pore diameter of the micropores is 0.05-100 μm.

[0030] Additionally, electroplating plastics, including:

[0031] The above-mentioned plastic materials; and

[0032] A metal plating layer, wherein the metal plating layer is formed on a side of the ink layer away from the plastic substrate;

[0033] The metal of the metal plating layer is selected from one or more of gold, silver, molybdenum, rhodium, palladium, copper, iron, tin, zinc, cobalt, nickel, chromium, cadmium, antimony, indium and bismuth.

[0034] Compared with the prior art, the present invention includes the following beneficial effects: the components of the conductive ink provided by the present invention cooperate with each other, so that the conductive ink has good bonding strength, and it contains a pore-forming agent. When the conductive ink is applied, the pore-forming agent can play a pore-forming role by heating, drying, soaking and other operations, and the formed ink layer contains micropores, so that the ink layer can further enhance the interlayer bonding strength between its adhesion layers. In particular, when the conductive ink is applied to the electroplating of plastics, the ink layer formed by the conductive ink can play a good transition and bonding role between the plastic and the plating layer, and the micropores of the ink layer can also play a role in enhancing conductivity and bonding strength, so that the bonding strength of the plastic and the plating layer can reach 9 to 25 N / cm. The application of the conductive ink provided by the present invention in the electroplating of plastics, the prepared electroplated plastic has good plating bonding strength, conductivity and stability, the preparation process is chromium-free and palladium-free, the pollution is small, the electroplating process is simple, and the use of traditional technologies with complicated processes, high pollution and high cost containing chromium and palladium is effectively avoided. At the same time, it also improves the bonding strength problem of the current direct electroplating technology, has high practicality, and is suitable for large-scale promotion. DETAILED DESCRIPTION

[0035] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention.

[0036] The technical solution provided by the present invention will be described in detail in the following content. It should be noted that the description order of the following embodiments is not intended to limit the preferred order of the embodiments. In addition, in the description of the present invention, the term "including" means "including but not limited to". Various embodiments of the present invention may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and simplicity and should not be understood as a rigid limitation on the scope of the present invention; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values ​​within the range.

[0037] The present invention provides a conductive ink, which comprises the following raw materials in parts by weight:

[0038]

[0039] Preferably, the conductive ink comprises the following raw materials by weight:

[0040]

[0041] More preferably, the conductive ink comprises the following raw materials by weight:

[0042]

[0043] In some embodiments, the resin binder can be selected from one or more of epoxy resin, polyurethane, alkyd resin, silicone resin, thermosetting acrylic resin, and thermoplastic acrylic resin. Among them, the thermosetting acrylic resin can be selected from but not limited to hydroxy acrylic resin.

[0044] In some embodiments, the conductive filler can be selected from one or more of graphene nanoplatelets, conductive carbon black, carbon nanotubes, expanded graphite, conductive carbon fiber, copper powder, nickel powder, silver powder, and silver-coated copper powder. Graphene nanoplatelets are different from graphene. Graphene nanoplatelets refer to ultra-thin graphene layered stacks with more than 10 carbon layers and a thickness in the range of 5 to 100 nm.

[0045] In some embodiments, the pore former can be selected from one or more of a volatile pore former, a decomposition pore former, a dissolving pore former, and an etching pore former. Further, the volatile pore former can be selected from one or more of a low saturated vapor pressure solvent and a high boiling point solvent; wherein the saturated vapor pressure of the low saturated vapor pressure solvent is lower than the saturated vapor pressure of the solvent in the raw material, and the low saturated vapor pressure solvent can be selected from one or more of ethyl acetate, ethanol, water, and tetrahydrofuran; the boiling point of the high boiling point solvent is higher than the boiling point of the solvent in the raw material, and the high boiling point solvent can be selected from one or more of ethylene glycol, dibasic acid ester, and N-dimethylpyrrolidone; that is, the volatile pore former can be selected from but not limited to one or more of ethyl acetate, ethanol, water, tetrahydrofuran, ethylene glycol, dibasic acid ester, and N-dimethylpyrrolidone, and such pore formers can cause phase separation of the polymer film based on the difference in volatilization rate to produce a microporous structure. The decomposition type pore former can be selected from one or more of bicarbonate and carbonate. Further, the decomposition type (gas escaping type) pore former can be selected from one or more of ammonium bicarbonate, ammonium carbonate and sodium bicarbonate. This type of pore former forms a microporous structure based on the generation and escape of gas. The dissolving type pore former can be selected from one or more of polyethylene glycol and urea. The etching type pore former can be selected from one or more of metal oxide and silicon oxide. Further, the etching type pore former can be selected from one or more of aluminum oxide, iron oxide, silicon oxide and copper oxide.

[0046] In some embodiments, the solvent may be a polar solvent or a non-polar solvent. The choice of solvent is not limited as long as it can dissolve the material. If multiple solvents are selected, the solvents can be mutually soluble. Further, the solvent may be selected from but not limited to acetone, dibasic acid esters, N,N-dimethylformamide, ethyl acetate, dimethyl sulfoxide, butanone, toluene, xylene, dichloromethane, cyclohexanone, water, ethanol, propanol, isopropanol, isobutanol, ethylene glycol, glycerol, terpineol, methanol, dipropylene glycol methyl ether, tetrahydrofuran, one or more thereof.

[0047] In some embodiments, the raw materials further include 1 to 3 parts of additives by weight. The addition of additives can improve the performance of the conductive ink. Preferably, the additives are 1.5 to 2.5 parts, and more preferably, the additives are 1.5 to 1.8 parts. Further, the additives can be selected from one or more of dispersants, anti-settling agents, leveling agents, wetting agents, defoamers, and thickeners. The materials that can be selected for various additives such as dispersants and anti-settling agents can be selected from the range known in the existing material field. The specific materials of various additives can be selected differently according to needs, which will not be repeated here.

[0048] In addition, the present invention also provides a method for preparing the conductive ink, comprising:

[0049] The above-mentioned raw materials of conductive ink are mixed.

[0050] In order to improve the conductivity and dispersibility of the material, after the above mixing, grinding may be further included. The grinding method may be selected from but not limited to sand milling, ball milling, and three-roller milling. The grinding time may be 0.5 to 24 hours.

[0051] In order to improve the uniformity of the ingredients, the mixed materials can be dispersed after mixing and before grinding. The dispersion operation can promote the uniformity of mixing and avoid material agglomeration, which is beneficial to subsequent grinding. Dispersion can be performed using a high-speed disperser, ultrasonic (dispersion) equipment, etc.

[0052] In addition, the present invention also provides a method for preparing a plastic material, comprising:

[0053] Providing a plastic substrate and the conductive ink;

[0054] The conductive ink is applied to the surface of the plastic substrate and dried.

[0055] The conductive ink can be coated on a part or all of the surface of the plastic substrate as required, and then dried. The preparation method is simple to operate, has low equipment dependence, and uses cheap and readily available materials, with low cost.

[0056] When the pore former in the conductive ink is selected as a volatile pore former or a decomposition pore former, the pore former undergoes phase separation or generates gas to form pores during the drying process, so that the conductive ink forms an ink layer with micropores after drying. When the pore former in the conductive ink is selected as a dissolving pore former or an etching pore former, the dissolving pore former can be dissolved in the pore forming solution to form pores, and the etching pore former can be etched in the etching solution to form pores. Therefore, when a dissolving pore former or an etching pore former is selected in some embodiments, after drying, it can also include: soaking the dried material in a pore forming solution or an etching solution, and drying. In this way, the ink layer is porous. In addition, for an etching pore former, pores can also be formed during the electroplating process. For example, when the conductive ink is applied to the electroplating of plastics, the conductive ink can be applied to the plastic substrate and dried, and then the obtained material is electroplated. In this case, the etching pore former forms pores in the acidic and alkaline environment of the electroplating solution.

[0057] For the soluble pore-forming agent, the pore-forming solution used is not limited, as long as it can dissolve the pore-forming agent and form pores. Further, the pore-forming solution can be selected from but not limited to one or more of water, N,N-dimethylformamide, ethanol, propanol, ethylene glycol butyl ether, and acetone, and the soaking temperature of the dried material can be 50-80°C, and the soaking time can be 0.5-12h.

[0058] In some embodiments, the thickness of the dry film formed by the conductive ink after drying may be 1 to 500 μm. A dry film of appropriate thickness is beneficial to promoting the bonding between different media in the case of electroplating.

[0059] In some embodiments, the drying temperature may be 25 to 120° C., and the drying time may be 0.5 to 12 hours.

[0060] In some embodiments, the coating method can be selected from one or more of spraying, blade coating, pulling, wire rod, screen printing, and gravure printing.

[0061] In some embodiments, the drying method can be selected from one or more of oven treatment, ultraviolet light treatment, and room temperature placement. One of the aforementioned methods can be selected for treatment, or multiple methods can be selected for treatment in different time periods. Further, oven treatment can be selected from but not limited to oven drying and vacuum oven heating, and room temperature placement can generally be selected for long-term static treatment.

[0062] In addition, the present invention also provides a plastic material obtained by the above-mentioned method for preparing a plastic material, comprising:

[0063] Plastic base; and

[0064] An ink layer is formed on the surface of a plastic substrate.

[0065] The ink layer is easy to construct, environmentally friendly, stable and easy to control. The material of the plastic substrate can be selected from but not limited to one or more of polyimide, polyethylene terephthalate, polymethyl methacrylate, styrene-butadiene-acrylonitrile copolymer, polypropylene, polycarbonate, and polyethylene.

[0066] In some embodiments, the ink layer includes a plurality of micropores, and the pore size of the micropores is 0.05 to 100 μm. The micropores of the ink layer with appropriate pore size and high porosity are conducive to improving the bonding force of the coating during the electroplating process. In particular, when the pore size of the micropores is larger, it is more conducive to promoting the bonding of the coating. The present invention optimizes the solid content by adjusting the types and amounts of resin binders, conductive fillers, pore formers, and solvents, so that the pore size of the micropores formed in the ink layer is in the range of 0.05 to 100 μm, so that the ink layer can be better bonded to the coating.

[0067] In addition, the present invention also provides an electroplated plastic, comprising:

[0068] The above-mentioned plastic materials; and

[0069] A metal plating layer, wherein the metal plating layer is formed on a side of the ink layer away from the plastic substrate;

[0070] The metal of the metal plating layer is selected from one or more of gold, silver, molybdenum, rhodium, palladium, copper, iron, tin, zinc, cobalt, nickel, chromium, cadmium, antimony, indium and bismuth.

[0071] The preparation method of the above-mentioned electroplated plastic includes: electroplating the plastic material with a plating solution to deposit a conductive metal on the ink layer. The selection of the conductive metal is the selection of the metal of the above-mentioned metal plating layer. During preparation, the deposition of different metal plating layers can adopt corresponding deposition operations and conditions. Specifically, the metal deposition can be carried out according to the electroplating method known to technical personnel in the field. For example, the first layer of base plating is performed on the plastic material in the plating solution, followed by a second layer or multiple layers of electroplating. The materials of different plating layers are selected as needed to ensure lower costs, higher resistance to cold and heat shock and salt spray resistance and other properties. Taking the electroplating of copper pyrophosphate as an example, the electroplating temperature can be 25-60°C, and the current density can be 0.2-5A / dm 2 , the electroplating time is 1 to 120 minutes.

[0072] The conductive ink provided by the present invention and its application in electroplating innovatively introduces an ink layer (with micropores) into a plastic substrate as a pre-treatment for electroplating. The electroplating process after the introduction of the ink layer is simple to operate, and the coating bonding strength is guaranteed. The coating bonding strength can reach 9 to 25 N / cm. At the same time, the brightness of the electroplated plastic including the ink layer is also enhanced, and the practicability is high.

[0073] The following is further described with reference to the examples. The raw materials and reagents used in the examples are all commercially available products or can be prepared by known methods.

[0074] Example 1

[0075] This embodiment provides a conductive ink and a preparation method, a plastic material and a preparation method, and electroplated plastic. For ease of description, the steps are integrated as follows, including:

[0076] (1) By weight, 25 parts of polyurethane, 5 parts of expanded graphite, 1 part of conductive carbon black, 12.5 parts of N,N-dimethylformamide, 10 parts of dibasic acid ester, 20 parts of ethyl acetate, 0.5 parts of dispersant, 0.5 parts of defoamer, 0.5 parts of wetting agent and 0.1 parts of thickener were mixed and dispersed, and then ground with a sand mill for 4 hours to obtain a conductive ink;

[0077] (2) spraying the conductive ink onto a plastic substrate, and then drying it in an oven at 70° C. for 0.5 h to obtain a plastic material, wherein the dry film thickness of the ink layer after drying is 200 μm;

[0078] (3) The first layer of base plating is performed on the plastic material using copper pyrophosphate plating solution. The plating solution temperature is 40°C and the current density is 1.0 A / dm 2 , the electroplating time is 40min; then the second layer of electroplating is carried out in copper sulfate electroplating solution, the electroplating solution temperature is 25℃, and the current density is 2.0A / dm 2 , the electroplating time is 40min; then the third layer of electroplating is carried out in nickel sulfate electroplating solution, the electroplating solution temperature is 55℃, and the current density is 2.0A / dm 2 , the electroplating time is 10min; then chrome plating is carried out in the electroplating chromium solution at 6A / dm 2 The electroplating was carried out at a current density of 100 and a temperature of 38°C for 4 minutes to obtain the electroplated plastic.

[0079] Example 2

[0080] This embodiment provides a conductive ink and a preparation method, a plastic material and a preparation method, and electroplated plastic. For ease of description, the steps are integrated as follows, including:

[0081] (1) By weight, 30 parts of epoxy resin, 10 parts of expanded graphite, 5 parts of conductive carbon black, 48 parts of N,N-dimethylformamide, 2 parts of ethylene glycol, 0.5 parts of dispersant, 0.5 parts of defoamer, 0.5 parts of wetting agent and 0.10 parts of thickener were mixed and dispersed, and then ground with a sand mill for 8 hours to obtain a conductive ink;

[0082] (2) spraying the conductive ink onto a plastic substrate, and then drying it in an oven at 70° C. for 0.5 h to obtain a plastic material, wherein the dry film thickness of the ink layer after drying is 150 μm;

[0083] (3) Use nickel sulfate electroplating solution to perform the first layer of base electroplating on the plastic material. The electroplating solution temperature is 60°C and the current density is 2.0A / dm 2 , the electroplating time is 40min; then the second layer of electroplating is carried out in copper sulfate electroplating solution, the electroplating solution temperature is 25℃, and the current density is 5.0A / dm 2 , the electroplating time is 120min; then the third layer of electroplating is carried out in nickel sulfate electroplating solution, the electroplating solution temperature is 55℃, and the current density is 2.5A / dm 2 , the electroplating time is 10min; then chrome plating is carried out in the electroplating chromium solution at 4A / dm 2 The electroplating was carried out at a current density of 5000 and a temperature of 35°C for 5 minutes to obtain the electroplated plastic.

[0084] Example 3

[0085] This embodiment provides a conductive ink and a preparation method, a plastic material and a preparation method, and electroplated plastic. For ease of description, the steps are integrated as follows, including:

[0086] (1) 50 parts of alkyd resin, 30 parts of silver powder, 48 parts of cyclohexanone, 2 parts of sodium bicarbonate, 1 part of dispersant, 0.25 parts of defoamer, 0.25 parts of wetting agent and 0.20 parts of thickener were mixed and dispersed by weight, and then ground with a sand mill for 12 hours to obtain a conductive ink;

[0087] (2) spraying the conductive ink onto a plastic substrate, and then drying it in an oven at 70° C. for 0.5 h to obtain a plastic material, wherein the dry film thickness of the ink layer after drying is 400 μm;

[0088] (3) Use nickel sulfate electroplating solution to perform the first layer of base electroplating on the plastic material. The electroplating solution temperature is 60°C and the current density is 2.0A / dm 2 , the electroplating time is 20min; then the second layer of electroplating is carried out in copper sulfate electroplating solution, the electroplating solution temperature is 25℃, and the current density is 3.0A / dm 2 , the electroplating time is 60min; then the third layer of electroplating is carried out in nickel sulfate electroplating solution, the electroplating solution temperature is 50℃, and the current density is 3.0A / dm 2 , the electroplating time is 15min; then chrome plating is carried out in the electroplating chromium solution at 8A / dm 2 The electroplating was carried out at a current density of 300 and a temperature of 34°C for 3 minutes to obtain the electroplated plastic.

[0089] Example 4

[0090] This embodiment provides a conductive ink and a preparation method, a plastic material and a preparation method, and electroplated plastic. For ease of description, the steps are integrated as follows, including:

[0091] (1) By weight, 50 parts of alkyd resin, 30 parts of silver powder, 47 parts of cyclohexanone, 3 parts of ethylene glycol, 1 part of dispersant, 0.25 parts of defoamer, 0.25 parts of wetting agent and 0.20 parts of thickener were mixed and dispersed, and then ground with a sand mill for 12 hours to obtain a conductive ink;

[0092] (2) spraying the conductive ink onto a plastic substrate, and then drying it in an oven at 70° C. for 0.5 h to obtain a plastic material, wherein the dry film thickness of the ink layer after drying is 400 μm; then soaking the plastic material in water at 80° C. for 3 h, and then drying it at 80° C.;

[0093] (3) Use nickel sulfate electroplating solution to perform the first layer of base electroplating on the plastic material. The electroplating solution temperature is 60°C and the current density is 2.0A / dm 2 , the electroplating time is 20min; then the second layer of electroplating is carried out in copper sulfate electroplating solution, the electroplating solution temperature is 25℃, and the current density is 3.0A / dm 2 , the electroplating time is 60min; then the third layer of electroplating is carried out in nickel sulfate electroplating solution, the electroplating solution temperature is 50℃, and the current density is 3.0A / dm 2 , the electroplating time is 15min; then chrome plating is carried out in the chromium electroplating solution at 2A / dm 2 The electroplating was carried out at a current density of 1000 nm and a temperature of 45°C for 10 min to obtain the electroplated plastic.

[0094] Example 5

[0095] This embodiment provides a conductive ink and a preparation method, a plastic material and a preparation method, and electroplated plastic. For ease of description, the steps are integrated as follows, including:

[0096] (1) By weight, 10 parts of hydroxy acrylic resin, 1 part of carbon nanotubes, 1 part of conductive carbon fiber, 8 parts of dimethyl sulfoxide, 2 parts of urea, and 1 part of leveling agent are mixed to obtain a conductive ink;

[0097] (2) coating a conductive ink wire rod on a plastic substrate, and then standing and drying at room temperature of 25° C. for 11 hours to obtain a plastic material; then soaking the plastic material in water at 80° C. for 12 hours, and then drying at 80° C.;

[0098] (3) The first layer of base plating is performed on the plastic material using copper pyrophosphate plating solution. The plating solution temperature is 40°C and the current density is 1.0 A / dm 2 , the electroplating time is 40min; then the second layer of electroplating is carried out in copper sulfate electroplating solution, the electroplating solution temperature is 25℃, and the current density is 2.0A / dm 2, the electroplating time is 40min; then the third layer of electroplating is carried out in nickel sulfate electroplating solution, the electroplating solution temperature is 55℃, and the current density is 2.0A / dm 2 , the electroplating time is 10min; then chrome plating is carried out in the electroplating chromium solution at 12A / dm 2 The electroplating was carried out at a current density of 300 and a temperature of 40°C for 3 minutes to obtain the electroplated plastic.

[0099] Example 6

[0100] This embodiment provides a conductive ink and a preparation method, a plastic material and a preparation method, and electroplated plastic. For ease of description, the steps are integrated as follows, including:

[0101] (1) By weight, 40 parts of silicone resin, 22 parts of silver-coated copper powder, 20 parts of propanol and 10 parts of isopropanol, 5 parts of copper oxide, 0.1 parts of anti-settling agent, 1 part of defoaming agent and 1 part of wetting agent were mixed, and then ground with a three-roll mill for 17 hours to obtain a conductive ink;

[0102] (2) screen printing the conductive ink on a plastic substrate, and then drying it under ultraviolet light for 1 hour to obtain a plastic material;

[0103] (3) Use acid copper electroplating solution to perform the first layer of base electroplating on the plastic material. The electroplating solution temperature is 40°C and the current density is 2A / dm 2 , the electroplating time is 60min; then the second layer of electroplating is carried out in nickel sulfate electroplating solution, the electroplating solution temperature is 55℃, and the current density is 2.0A / dm 2 , the electroplating time is 10min; then chrome plating is carried out in the electroplating chromium solution at 12A / dm 2 The electroplating was carried out at a current density of 300 and a temperature of 40°C for 3 minutes to obtain the electroplated plastic.

[0104] Example 7

[0105] This embodiment provides a conductive ink and a preparation method, a plastic material and a preparation method, and electroplated plastic. For ease of description, the steps are integrated as follows, including:

[0106] (1) By weight, 30 parts of polyurethane, 5 parts of graphene microsheets, 1 part of conductive carbon black, 20 parts of N,N-dimethylformamide, 10 parts of ethyl acetate (as a pore former), 0.5 parts of a dispersant, 0.5 parts of a defoamer, 0.5 parts of a wetting agent and 0.1 parts of a thickener were mixed and dispersed, and then ground with a sand mill for 4 hours to obtain a conductive ink;

[0107] (2) spraying the conductive ink onto a plastic substrate, and then drying it in an oven at 70° C. for 0.5 h to obtain a plastic material, wherein the dry film thickness of the ink layer after drying is 200 μm;

[0108] (3) The first layer of base plating is performed on the plastic material using copper pyrophosphate plating solution. The plating solution temperature is 40°C and the current density is 1.0 A / dm 2 , the electroplating time is 40min; then the second layer of electroplating is carried out in copper sulfate electroplating solution, the electroplating solution temperature is 25℃, and the current density is 2.0A / dm 2 , the electroplating time is 40min; then the third layer of electroplating is carried out in nickel sulfate electroplating solution, the electroplating solution temperature is 55℃, and the current density is 2.0A / dm 2 , the electroplating time is 10min; then chrome plating is carried out in the electroplating chromium solution at 12A / dm 2 The electroplating was carried out at a current density of 300 and a temperature of 40°C for 3 minutes to obtain the electroplated plastic.

[0109] Example 8

[0110] This embodiment provides a conductive ink and a preparation method, a plastic material and a preparation method, and electroplated plastic. For ease of description, the steps are integrated as follows, including:

[0111] (1) By weight, 30 parts of polyurethane, 5 parts of expanded graphite, 2 parts of silver powder, 1 part of conductive carbon black, 20 parts of N,N-dimethylformamide, 10 parts of ethyl acetate (as a pore former), 0.5 parts of a dispersant, 0.5 parts of a defoamer, 0.5 parts of a wetting agent and 0.1 parts of a thickener were mixed and dispersed, and then ground with a sand mill for 4 hours to obtain a conductive ink;

[0112] (2) spraying the conductive ink onto a plastic substrate, and then drying it in an oven at 70° C. for 0.5 h to obtain a plastic material, wherein the dry film thickness of the ink layer after drying is 200 μm;

[0113] (3) The first layer of base plating is performed on the plastic material using copper pyrophosphate plating solution. The plating solution temperature is 40°C and the current density is 1.0 A / dm 2 , the electroplating time is 40min; then the second layer of electroplating is carried out in copper sulfate electroplating solution, the electroplating solution temperature is 25℃, and the current density is 3.0A / dm 2 , the electroplating time is 60min; then the third layer of electroplating is carried out in nickel sulfate electroplating solution, the electroplating solution temperature is 50℃, and the current density is 3.0A / dm 2 , the electroplating time is 15min; then chrome plating is carried out in the chromium electroplating solution at 2A / dm 2 The electroplating was carried out at a current density of 1000 nm and a temperature of 45°C for 10 min to obtain the electroplated plastic.

[0114] Example 9 (Phase separation and pore formation by mixing multiple resins)

[0115] This embodiment provides a conductive ink and a preparation method, a plastic material and a preparation method, and electroplated plastic. For ease of description, the steps are integrated as follows, including:

[0116] (1) According to weight, 20 parts of polyurethane and 10 parts of silicone resin (a multi-resin system is used to form phase separation pores), 5 parts of expanded graphite, 2 parts of silver powder and 1 part of conductive carbon black, 20 parts of N,N-dimethylformamide, 10 parts of ethyl acetate (as a pore-forming agent), 0.5 parts of dispersant, 0.5 parts of defoamer, 0.5 parts of wetting agent and 0.1 parts of thickener are mixed and dispersed, and then ground with a sand mill for 4 hours to obtain a conductive ink;

[0117] (2) spraying the conductive ink onto a plastic substrate, and then drying it in an oven at 70° C. for 0.5 h to obtain a plastic material, wherein the dry film thickness of the ink layer after drying is 200 μm;

[0118] (3) The first layer of base plating is performed on the plastic material using copper pyrophosphate plating solution. The plating solution temperature is 40°C and the current density is 1.0 A / dm 2 , the electroplating time is 40min; then the second layer of electroplating is carried out in copper sulfate electroplating solution, the electroplating solution temperature is 25℃, and the current density is 2.0A / dm 2 , the electroplating time is 40min; then the third layer of electroplating is carried out in nickel sulfate electroplating solution, the electroplating solution temperature is 55℃, and the current density is 2.0A / dm 2 , the electroplating time is 10min; then chrome plating is carried out in the electroplating chromium solution at 6A / dm 2 The electroplating was carried out at a current density of 100 and a temperature of 38°C for 4 minutes to obtain the electroplated plastic.

[0119] Comparative Example 1

[0120] (1) By weight, 30 parts of polyurethane, 10 parts of graphene, 1 part of conductive carbon black, 20 parts of N,N-dimethylformamide, 10 parts of ethyl acetate, 0.5 parts of dispersant, 0.5 parts of defoamer, 0.5 parts of wetting agent and 0.1 parts of thickener were mixed and dispersed, and then ground with a sand mill for 4 hours to obtain a conductive ink;

[0121] (2) spraying the conductive ink onto a plastic substrate, and then drying it in an oven at 70° C. for 0.5 h to obtain a plastic material;

[0122] (3) The first layer of base plating is performed on the plastic material using copper pyrophosphate plating solution. The plating solution temperature is 40°C and the current density is 1.0 A / dm 2 , the electroplating time is 40min; then the second layer of electroplating is carried out in copper sulfate electroplating solution, the electroplating solution temperature is 25℃, and the current density is 2.0A / dm 2, the electroplating time is 40min; then the third layer of electroplating is carried out in nickel sulfate electroplating solution, the electroplating solution temperature is 55℃, and the current density is 2.0A / dm 2 , the electroplating time is 10min; then chrome plating is carried out in the electroplating chromium solution at 6A / dm 2 The electroplating was carried out at a current density of 100 and a temperature of 38°C for 4 minutes to obtain the electroplated plastic.

[0123] Performance Testing

[0124] The electroplated plastics prepared in Examples 1 to 9 and Comparative Example 1 were subjected to a coating adhesion test (ASTM B533-85 (2013)), an ink layer uniformity test (visual inspection), a square resistance test (tested using a four-probe tester, converted to a square resistance of 25 μm thickness), a salt spray resistance test (the plated part was placed in a salt spray chamber, and the plated part was sprayed with 5wt% sodium chloride salt water at 35°C for 2 hours, then taken out, and then the plated part was placed in another constant temperature and humidity chamber at a temperature of 40°C and a relative humidity of 80%, and the plated part was observed, and it was recorded how long it took for the surface of the plated part to be abnormal), and a cold and hot shock resistance test (the plated part was placed in a cold and hot shock test chamber, the test temperature was lowered to minus 40°C, and placed for 2 hours, and then within 3 minutes, the test temperature was raised to 85°C and placed for 2 hours. After repeating the above operation 5 times, the plated part was placed in a room temperature environment to observe whether the surface of the plated part was abnormal). The test results are shown in Table 1.

[0125] Table 1 Performance test results of electroplated plastics prepared in Examples 1 to 9 and Comparative Example 1

[0126]

[0127]

[0128] It can be seen from Table 1 that, compared with the electroplated plastic prepared in Comparative Example 1, the electroplated plastics prepared in Examples 1 to 9 of the present invention have better coating adhesion, conductivity (lower square resistance) and salt spray resistance, and the film uniformity and resistance to cold and hot shock are also similar to those of the electroplated plastic prepared in Comparative Example 1, meeting the commercial application requirements of electroplated plastics.

[0129] The technical solutions provided by the embodiments of the present invention are introduced in detail above. Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the methods and core ideas of the present invention. At the same time, for those skilled in the art, according to the ideas of the present invention, there will be changes in the specific implementation methods and application scopes. In summary, the content of this specification should not be understood as limiting the present invention.

Claims

1. A method for preparing electroplated plastics, It is characterized in that include: A plastic substrate and a conductive ink are provided, wherein the raw materials of the conductive ink are composed of 25 parts of polyurethane, 5 parts of expanded graphite, 1 part of conductive carbon black, 12.5 parts of N,N-dimethylformamide, 10 parts of dibasic acid ester, 20 parts of ethyl acetate, 0.5 parts of dispersant, 0.5 parts of defoamer, 0.5 parts of wetting agent and 0.1 parts of thickener, and the conductive ink is prepared by mixing and dispersing the raw materials of the conductive ink and then grinding them for 4 hours; Applying the conductive ink on the surface of the plastic substrate and drying at 70° C. for 0.5 h to obtain a plastic material, wherein the plastic material comprises the plastic substrate and an ink layer on the surface of the plastic substrate, wherein the ink layer has a thickness of 200 μm and comprises a plurality of micropores, wherein the pore diameter of the micropores is 0.05 to 100 μm; as well as The first layer of base plating is performed on the plastic material using copper pyrophosphate electroplating solution, the plating solution temperature is 40°C, and the current density is 1.0A / dm 2 , the electroplating time is 40min; then the second layer of electroplating is carried out in copper sulfate electroplating solution, the electroplating solution temperature is 25℃, and the current density is 2.0A / dm 2 , the electroplating time is 40min; then the third layer of electroplating is carried out in nickel sulfate electroplating solution, the electroplating solution temperature is 55℃, and the current density is 2.0A / dm 2 , the electroplating time is 10min; then chrome plating is carried out in the electroplating chromium solution at 6A / dm 2 The electroplating was carried out at a current density of 100 and a temperature of 38°C for 4 minutes to obtain the electroplated plastic.

2. Electroplating plastics, It is characterized in that The electroplated plastic is prepared by the method for preparing the electroplated plastic according to claim 1, wherein the electroplated plastic comprises: Plastic materials; and A metal plating layer is formed on a side of the ink layer away from the plastic substrate.