Titanium material for metal foil production, method for producing titanium material for metal foil production, and metal foil production roller

By controlling the chemical composition and thermal processing technology of the titanium material, the problem of macroscopic patterns during the use of the metal foil manufacturing roller is solved, the uniformity of the thickness and conductivity of the copper foil is achieved, and the quality of the copper foil is improved.

CN116134165BActive Publication Date: 2024-10-22NIPPON STEEL CORPORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080104712.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-07-27
Publication Date
2024-10-22
Estimated Expiration
2040-07-27

AI Technical Summary

Technical Problem

Existing metal foil manufacturing drums are prone to produce macroscopic patterns during use, resulting in uneven thickness and uneven conductivity of the copper foil, affecting the quality of the copper foil.

Method used

By controlling the chemical composition and thermal processing process of the titanium material, the resistivity uniformity on the surface of the titanium material is ensured, and a specific titanium material chemical composition and manufacturing method are adopted, such as containing appropriate amounts of Sn, Zr, Al, N, C, H, O , Fe, Cr, Ni, Cu, Mo and other elements, and use electron beam melting or plasma melting to manufacture titanium ingots, which are then heat treated and rolled to form a uniform metallographic structure.

Benefits of technology

It effectively suppresses the generation of macroscopic patterns, ensures the uniformity of thickness and conductivity of copper foil, and improves the manufacturing quality of copper foil.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116134165B_ABST
    Figure CN116134165B_ABST
Patent Text Reader

Abstract

When a pair of energized electrode probes are brought into contact with the titanium material to supply a constant current, and a pair of potential detection probes are brought into contact with the surface of the titanium material with a certain probe interval to measure the voltages at multiple locations on the surface, the voltage ratio between two adjacent locations among the multiple locations is greater than 0.95 and less than 1.05.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a titanium material for metal foil manufacturing, a method for manufacturing the titanium material for metal foil manufacturing, and a metal foil manufacturing roller. Background Art

[0002] Copper foil is often used as a material for wiring of wiring boards such as multilayer wiring boards and flexible wiring boards, or for conductive parts of electronic components such as current collectors of lithium-ion batteries.

[0003] Copper foil for such purposes is produced, for example, by the following method. A copper sulfate solution formed by dissolving a copper raw material in a sulfuric acid solution is provided with a roller of an insoluble metal such as lead or titanium having a width of more than 1 meter and a diameter of several meters as an anode and a cathode, and copper is continuously electrodeposited on the roller while the roller is rotated. The deposited copper is continuously peeled off and rolled into a roll. Copper foil is produced by the above process.

[0004] As the material of the roller, titanium is generally used from the perspectives of excellent corrosion resistance and excellent copper foil peeling properties. However, even if titanium with excellent corrosion resistance is used, the surface of the titanium material constituting the roller will gradually be affected by corrosion in the copper sulfate solution when copper foil is manufactured for a long time. In addition, the state of the roller surface affected by corrosion will be transferred to the copper foil during copper foil manufacturing.

[0005] Regarding the corrosion of metal materials, it is known that the corrosion state and degree of corrosion will vary depending on various intrinsic factors derived from the metallographic structure, including the crystal structure, crystal orientation, defects, segregation, processing strain, residual strain, etc. of the metal material. When a roller using a metal material with uneven metallographic structure between parts is affected by corrosion during copper foil manufacturing, the uniform surface state of the roller cannot be maintained, and an uneven surface will be generated on the surface of the roller. The uneven surface generated on the surface of the roller can be identified as a pattern. Among the patterns caused by such uneven metallographic structure, the pattern that can be discerned by the naked eye due to the macroscopic structure of a larger area is called a "macro pattern". In addition, the macro pattern generated on the surface of the roller may be transferred to the copper foil during the manufacture of the copper foil.

[0006] Therefore, in order to manufacture a copper foil with high precision and uniform thickness, it is important to make the metallographic structure of the titanium material constituting the roller uniform to achieve uniform corrosion of the roller and reduce macroscopic patterns caused by non-uniform macroscopic structures.

[0007] In order to suppress macroscopic patterns, Patent Document 1 proposes a titanium plate for electrolytic copper foil manufacturing rollers, characterized in that it contains, by mass%, Cu: greater than 0.15% and less than 0.5%, oxygen: greater than 0.05% and less than 0.20%, Fe: less than 0.04%, and the remainder is titanium and unavoidable impurities, and is composed of a uniform and fine recrystallized structure of α phase with an average grain diameter of less than 35μm.

[0008] Patent document 2 proposes a titanium plate for electrolytic copper foil manufacturing rollers, characterized in that it contains, by mass%, Cu: 0.3-1.1%, Fe: less than 0.04%, oxygen: less than 0.1%, hydrogen: less than 0.006%, an average grain size of 8.2 or more, and a Vickers hardness of 115 or more and 145 or less. In the part parallel to the plate surface, its texture is as follows: in the (0001) plane pole figure of the α phase along the normal direction (ND axis) from the rolling surface, the total area of ​​the grains existing within the range of an ellipse with the normal inclination angle of the (0001) plane being ±45° in the rolling width direction (TD) as the major axis and ±25° in the final rolling direction (RD) as the minor axis is set to A, and when the total area of ​​the grains other than this is set to B, the area ratio A / B is greater than 3.0.

[0009] Prior art literature

[0010] Patent Literature

[0011] Patent Document 1: Japanese Patent Application Publication No. 2009-41064

[0012] Patent Document 2: Japanese Patent Application Publication No. 2012-112017 Summary of the invention

[0013] Problem that the invention aims to solve

[0014] However, the titanium plate for the electrolytic copper foil manufacturing roller described in Patent Document 1 or Patent Document 2 contains elements such as Fe that are easily distributed to the liquid phase side during the solidification process when the titanium plate is manufactured. Therefore, segregation, that is, unevenness, of the chemical composition in the titanium plate is easily generated. If the chemical composition is uneven, the titanium plate may be unevenly corroded during the metal foil manufacturing process, resulting in macroscopic patterns on the titanium plate, and the macroscopic patterns are transferred to the manufactured metal foil.

[0015] The present invention aims to solve the above-mentioned problems. The purpose of the present invention is to provide a titanium material for metal foil manufacturing, a method for manufacturing a titanium material for metal foil manufacturing, and a metal foil manufacturing roller, which can suppress the generation of macro patterns during the use of the metal foil manufacturing roller.

[0016] Solutions for solving problems

[0017] The inventors of the present invention have noticed that the macro patterns existing in the polishing state of the metal foil manufacturing drum and the generation of macro patterns caused by uneven corrosion during use are affected by various internal factors derived from the metallographic structure, including the chemical composition, crystal structure, crystal orientation, defects, segregation, processing strain, residual strain, etc. of the metal material. They have also found that when the electrical resistance at various locations on the surface of the titanium material for metal foil manufacturing satisfies the specified conditions, the macro patterns are suppressed, thereby completing the present invention.

[0018] The main contents of the present invention completed based on the above-mentioned knowledge are as follows.

[0019] (1) A first aspect of the present invention is a titanium material for metal foil production having the following chemical composition:

[0020] Contains by mass%

[0021] Sn: 0% or more and 2.0% or less,

[0022] Zr: 0% or more and 5.0% or less,

[0023] Al: 0% or more and 7.0% or less,

[0024] N: 0% or more and 0.100% or less,

[0025] C: 0% or more and 0.080% or less,

[0026] H: 0% or more and 0.0150% or less,

[0027] O: 0% or more and 1.000% or less,

[0028] Fe: 0% or more and 0.500% or less,

[0029] Cr: 0% or more and 0.500% or less,

[0030] Ni: 0% or more and 0.090% or less,

[0031] Cu: 0% or more and 1.5% or less, and

[0032] Mo: 0% or more and 0.750% or less,

[0033] The balance includes Ti and impurities,

[0034] The total content of Fe, Cr and Ni is 0% or more and 0.500% or less;

[0035] When a pair of powered electrode probes are brought into contact with the titanium material for metal foil manufacturing to supply a constant current, and a pair of potential detection probes are brought into contact with the surface of the titanium material for metal foil manufacturing with a certain probe interval to measure the voltages at multiple locations on the surface, the voltage ratio between two adjacent locations among the multiple locations is greater than 0.95 and less than 1.05.

[0036] (2) The titanium material for metal foil production described in (1) above contains Fe, Cr, Ni and Mo,

[0037] The content of Ni is 0 mass % or more and 0.090 mass % or less,

[0038] The content of Mo may be 0.5 times or more and 1.2 times or less the total content of Fe, Cr, and Ni on a mass basis.

[0039] (3) The titanium material for metal foil production described in (1) or (2) above may contain, in terms of mass %,

[0040] N: 0% or more and 0.100% or less,

[0041] C: 0% or more and 0.080% or less,

[0042] H: 0% or more and 0.0150% or less,

[0043] O: 0% or more and 0.400% or less,

[0044] Fe: 0.02% or more and 0.500% or less,

[0045] Ni: 0% or more and 0.090% or less, and

[0046] Cu: 0% or more and 1.5% or less.

[0047] (4) The titanium material for metal foil production described in (1) above may contain, in total mass %, 0.2% to 5.0% selected from

[0048] Sn: 0.2% or more and 2.0% or less,

[0049] Zr: 0.2% or more and 5.0% or less, and

[0050] Al: one or more of the group consisting of 0.2% to 3.0%,

[0051] And it can contain in mass %

[0052] N: 0% or more and 0.100% or less,

[0053] C: 0% or more and 0.080% or less,

[0054] H: 0% or more and 0.0150% or less,

[0055] O: 0% or more and 1.000% or less, and

[0056] Fe: 0% or more and 0.500% or less.

[0057] (5) The titanium material for metal foil production described in (1) above contains more than 1.8 mass % and not more than 7.0 mass % of Al,

[0058] When the Al content is expressed as [Al%], the Zr content is expressed as [Zr%], the Sn content is expressed as [Sn%], and the O content is expressed as [O%] in terms of mass%, the Al equivalent Aleq represented by the following formula (1) can be 7.0 mass% or less.

[0059] Aleq=[Al%]+[Zr%] / 6+[Sn%] / 3+10×[O%] Formula (1)

[0060] (6) The titanium material for metal foil production described in any one of (1) to (5) above may be a titanium material for a metal foil production roll.

[0061] (7) A second aspect of the present invention is a method for producing a titanium material for metal foil production, comprising the following steps:

[0062] A process for producing a titanium ingot by continuous casting, wherein molten titanium is poured into a coolable mold with openings on the upper and lower surfaces, the liquid surface of the molten titanium in the mold is heated, the titanium is cooled and solidified by means of the mold, and the solidified titanium is pulled downward using a clamp;

[0063] The titanium ingot is heated to a temperature of 750° C. or higher and lower than the β transformation point, and rolled at a reduction ratio of 90% or higher to produce a rolled plate; and

[0064] A process of performing heat treatment at a temperature of 600°C to 750°C for 20 minutes to 120 minutes, cooling from the heat treatment temperature to 500°C at an average cooling rate of 20°C / min or more, and cooling from the heat treatment temperature to a temperature of 300°C or less at an average cooling rate of 10°C / min or less.

[0065] (8) The method for producing a titanium material for metal foil production described in (7) above comprises the steps of hot working the titanium ingot to produce a slab,

[0066] In the step of manufacturing the rolled plate, the slab may be rolled instead of the titanium ingot.

[0067] (9) In the method for producing a titanium material for metal foil production described in (7) or (8), the casting method is electron beam melting.

[0068] The electron beam irradiation amount to the inner space of the mold in the electron beam melting method is 150W / cm 2 The titanium may be melted by irradiating the electron beam to the titanium when the melting rate of the titanium is less than 2.5 tons / h.

[0069] (10) In the method for producing a titanium material for metal foil production described in (9) above, the ratio X of the horizontal cross-sectional area of ​​the internal space of the mold to the circumference of the inner circumference of the horizontal cross-sectional area of ​​the mold and the irradiation amount Y of the electron beam in the electron beam melting method can satisfy the relationship of the following formula (2), where the unit of X is cm and the unit of Y is W / cm 2 ,

[0070] Y = -3.8X + (135 ± 25) formula (2).

[0071] (11) In the method for producing a titanium material for metal foil production described in (7) or (8), the casting method is a plasma melting method,

[0072] The plasma irradiation amount of the plasma in the mold in the plasma melting method is 380W / cm 2 The titanium can be melted by irradiating the titanium with the plasma when the melting rate of the titanium is 2.5 tons / h or less.

[0073] (12) In the method for producing a titanium material for metal foil production described in (7) to (11) above, the unit of the horizontal cross section of the space inside the mold is cm 2 The ratio of the area to the perimeter in cm can be greater than 7.5 cm and less than 22.5 cm.

[0074] (13) A third aspect of the present invention is a metal foil manufacturing roll comprising: the titanium material for metal foil manufacturing described in (6) above, which is coated along the outer peripheral surface of a cylindrical inner roll; and

[0075] A welding portion is arranged at the butting portion of the titanium material.

[0076] Effects of the Invention

[0077] As described above, according to the above aspect of the present invention, when the titanium material for metal foil production is used for a roller for metal foil production, the generation of macro patterns can be suppressed. BRIEF DESCRIPTION OF THE DRAWINGS

[0078] Figure 1This is a schematic diagram for explaining a method for inspecting a titanium material for metal foil production or a metal foil production roll according to one embodiment of the present invention.

[0079] Figure 2 This is a schematic diagram of the surface of a titanium material for producing metal foil, and is used to illustrate an example of the arrangement of a current-carrying electrode probe and a potential detection probe in a method for inspecting a titanium material for producing metal foil or a metal foil producing roller according to an embodiment of the present invention.

[0080] Figure 3 is a micrograph showing an example of the macroscopic pattern observed on the surface of titanium after corrosion.

[0081] Figure 4 This is a micrograph showing an example of a macro pattern observed on the surface of a titanium plate after corrosion, and is a reference image in which the macro pattern is emphasized in order to show the position of the macro pattern.

[0082] Figure 5 This is a schematic diagram of a copper foil manufacturing apparatus showing one usage of a metal foil manufacturing roller.

[0083] Figure 6 This is a schematic diagram showing a metal foil production drum according to one embodiment of the present invention.

[0084] Figure 7 This is a cross-sectional view showing an example of a horizontal cross section of a mold used in electron beam melting or plasma arc melting.

[0085] Figure 8 This is a cross-sectional view showing another example of a horizontal cross section of a mold used in the electron beam melting method or the plasma arc melting method. DETAILED DESCRIPTION

[0086] The preferred embodiments of the present invention are described in detail below.

[0087] Background

[0088] First, before describing the titanium material for metal foil manufacturing of the present embodiment, the background of the present inventors' attention to the voltage on the surface of the titanium material for metal foil manufacturing is described. In order to manufacture a metal foil (e.g., copper foil) with high precision and uniform thickness by using a metal foil manufacturing roller made of titanium, it is important to make the chemical composition and metallographic structure of the titanium material constituting the metal foil manufacturing roller uniform, prevent the macro pattern on the titanium material surface, and achieve uniform corrosion of the roller, thereby reducing the macro pattern caused by the uneven macro structure. The present inventors have found that by making the conductivity of the titanium material surface uniform, the macro pattern can be significantly suppressed, and in addition, the generation of macro patterns caused by uneven corrosion on the titanium material surface during the copper foil manufacturing process can be significantly suppressed.

[0089] Factors that cause the conductivity of the titanium material surface for metal foil manufacturing to fluctuate include chemical composition inhomogeneity, strain, crystal structure, crystal orientation distribution and other metallographic structural inhomogeneities. Therefore, the resistivity of the titanium material surface for metal foil manufacturing can comprehensively reflect various internal factors derived from the metallographic structure, such as chemical composition, crystal structure, crystal orientation, defects, segregation, processing strain, and residual strain.

[0090] For example, regarding the chemical composition, it can be estimated that the resistivity (μΩ·cm) of the surface of the titanium material for metal foil production is linearly positively correlated with the total concentration of O, N, and C, the total concentration of Fe, Cr, Ni, and Mo, and the hydrogen concentration. The resistivity of the portion where these elements are segregated is higher than that of the portion where they are not segregated. The present inventors have found that among the intrinsic factors, segregation in particular has an influence on the resistivity of the surface of the titanium material for metal foil production.

[0091] In addition, for example, regarding the metallographic structure, it is speculated that the resistivity (μΩ·cm) on the surface of the titanium material used to manufacture the metal foil is linearly positively correlated with the strain. In addition, it is speculated that the resistivity (μΩ·cm) on the surface of the titanium material used to manufacture the metal foil is linearly negatively correlated with the angle between the current direction and the c-axis of the α-phase crystal structure. It is further speculated that the resistivity (μΩ·cm) on the surface of the titanium material used to manufacture the metal foil is proportional to the inverse of the grain diameter in the metallographic structure (inversely proportional to the grain diameter). It should be noted that, of course, the resistivity (μΩ·cm) on the surface of the titanium material used to manufacture the metal foil is also related to the temperature of the surface of the titanium material used to manufacture the metal foil.

[0092] In summary, it can be inferred that the resistivity (μΩ·cm) of the surface of the titanium material for metal foil manufacturing is correlated with the main internal factors that cause the formation of macro patterns, etc. Therefore, by understanding the resistance of each part of the surface of the titanium material for metal foil manufacturing, the unevenness of the internal factors at each part of the surface of the titanium material for metal foil manufacturing can be understood.

[0093] The above is the background for the inventors of the present invention to pay attention to the voltage on the surface of the titanium material for producing the metal foil.

[0094] <Titanium materials for metal foil manufacturing>

[0095] Based on the above knowledge, the present inventors have invented a titanium material for metal foil manufacturing that can suppress the generation of macro patterns on metal foil manufacturing rollers when in use. In the titanium material for metal foil manufacturing of this embodiment, when a pair of energized electrode probes are brought into contact with the titanium material to supply a constant current, and a pair of potential detection probes are brought into contact with the surface of the titanium material with a certain probe interval to measure the voltage at multiple locations on the surface, the voltage ratio between two adjacent locations among the multiple locations is greater than 0.95 and less than 1.05. This titanium material can particularly suppress segregation and the generation of macro patterns. The titanium material for metal foil manufacturing of this embodiment is described in detail below.

[0096] (Voltage ratio)

[0097] The titanium material for metal foil manufacturing of the present embodiment has a voltage ratio of 0.95 or more and 1.05 or less between two adjacent parts of the plurality of parts on its surface. When the voltage ratio between two adjacent parts of the plurality of parts is 0.95 or more and 1.05 or less, the two adjacent parts are uniform with each other. As a result, there are no macro patterns on the adjacent parts, and the generation of macro patterns can also be suppressed during the metal foil manufacturing process. On the other hand, when the voltage ratio between two adjacent parts of the plurality of parts is less than 0.95 or greater than 1.05, the two parts are not uniform with each other, and macro patterns exist on the surface of the titanium material. In addition, when the voltage ratio between two adjacent parts of the plurality of parts is less than 0.95 or greater than 1.05, the non-uniformity will lead to uneven conductivity. During the metal foil manufacturing process, the corrosion rate between the non-uniform parts and other parts will differ, and macro patterns will be generated.

[0098] The titanium material for metal foil manufacturing of this embodiment preferably has a voltage ratio of 0.95 to 1.05 at least 95% of the two adjacent parts among the plurality of parts, and more preferably has a voltage ratio of 0.95 to 1.05 at least 98%. Thus, the titanium material for metal foil manufacturing is uniform over a wide range, and macro patterns are further suppressed.

[0099] The titanium material for metal foil manufacturing of the present embodiment is more preferably such that the voltage ratio of two adjacent parts among the plurality of parts is 0.95 or more and 1.05 or less. When the voltage ratio of two adjacent parts is 0.95 or more and 1.05 or less, a titanium material for metal foil manufacturing having no macro pattern in all parts can be obtained, and when the titanium material for metal foil manufacturing is used to manufacture metal foil, the generation of macro pattern in a wide area of ​​the surface of the titanium material for metal foil manufacturing can be suppressed.

[0100] Here, see Figure 1 , 2 , a method for measuring the voltage at various locations of the titanium material for producing metal foil according to the present embodiment will be described. Figure 1 This is a schematic diagram for explaining a method for inspecting a titanium material for metal foil production or a metal foil production roll according to one embodiment of the present invention. Figure 2 It is a schematic diagram of the surface of the titanium material for metal foil production, for illustrating an example of the arrangement of the current-carrying electrode probe and the potential detection probe in the inspection method of the titanium material for metal foil production or the metal foil production roller according to the present embodiment.

[0101] First, if Figure 1As shown, a pair of current-carrying electrode probes 20A and 20B are brought into contact with the surface 11 of the titanium material 10 for producing metal foil, and a constant current I is supplied. Thus, the constant current I flows between a-a' where the current-carrying electrode probes 20A and 20B contact the surface 11, generating a predetermined potential difference.

[0102] Next, the potential detection probe pair 30A and 30B are brought into contact with the plurality of locations on the surface 11 to which the constant current I is supplied, with the probe interval L, to detect a plurality of voltages V1 to V n The potential detection probe pair 30A, 30B can be contacted with the surface 11 one pair at a time, and multiple voltages V1 to V can be detected by repeating this process multiple times. n , multiple pairs can also be in contact with the surface 11 at the same time to detect multiple voltages V1~V n .

[0103] Here, the probe interval L is not particularly limited, and can be determined, for example, according to the size of the macro pattern. According to the experience of the inventors, the macro pattern is about 2 to 3 mm. In addition, the inventors found that when the probe interval L is 3% or more of the macro pattern, the voltage difference between other parts can be sufficiently clearly detected. Therefore, the probe interval L is, for example, 67 mm or less, preferably 33 mm or less.

[0104] In addition, the probe interval L can be determined based on, for example, the average grain size of the titanium material for metal foil 10. That is, the resistance of the surface 11 of the titanium material for metal foil 10 is also affected by the number of grain boundaries of the titanium material for metal foil 10 in the measurement portion. Therefore, from the perspective of balancing the influence of grain boundaries on resistance, it is preferred that the surface 11 include a sufficient number of grain boundaries within the probe interval L.

[0105] For example, when the grain diameter observed in the surface 11 is in the range of 20 to 40 μm, there are 50 to 100 grain boundaries in the 2 mm macro pattern. In order to fully separate the influence of the macro pattern on the resistance from the influence of the number of grain boundaries, it is preferred that at least 125 grain boundaries exist in the probe interval L on the surface 11. From this perspective, the probe interval L is, for example, 125 times or more of the average grain diameter, preferably 140 times or more.

[0106] In summary, the probe interval L between bi-bi' (i is an integer selected from 1 to n) contacted by the potential detection probes 30A and 30B can be determined according to the average grain diameter and / or the size of the macro pattern of the titanium material 10 for metal foil manufacturing. And, if the average grain diameter and the size of the macro pattern are considered at the same time, the probe interval L is, for example, 125 times or more of the average grain diameter and 67 mm or less, preferably 140 times or more of the average grain diameter and 33 mm or less.

[0107] The resistance at each part of the surface of the titanium material for metal foil manufacturing corresponds to the voltage at each part when a constant current I is supplied. Therefore, by measuring the voltages V1 to Vn at the parts b1-b1' to bn-bn' between a-a' where the current-carrying electrode probes 20A and 20B contact the surface 11 and comparing them, the unevenness of the internal factors at each part of the surface of the titanium material for metal foil manufacturing can be grasped. Furthermore, by comparing the voltages V1 to Vn at the parts b1-b1' to bn-bn' n , the uniformity of corrosion and the quality of the metal foil manufacturing roller can be evaluated.

[0108] For example, Figure 1 In the case where there is an uneven portion 12 such as a macro pattern in the portion bn-bn', the voltage V on the portion bn-bn' n By detecting a voltage value different from that at other locations, it is possible to understand that an uneven location 12 exists at the location bn-bn'.

[0109] In addition, for measuring voltage V i The arrangement of the parts bi-bi' (i is an integer selected from 1 to n) is as follows Figure 2 As shown, between a-a', a certain measuring target site bi-bi' connects another measuring target site bm-bm' (m is an integer selected from 1 to n) on a straight line L1, arranged along the plate width direction of the titanium material for metal foil production.

[0110] After detecting the voltage at the part bi-bi', move a pair of powered electrode probes 20A and 20B from the straight line L1 in a direction perpendicular to the plate width direction and bring them into contact. At a position deviated from the straight line L1, measure the voltages V1' to V2 of the parts c1-c1' to cn-cn' arranged on the straight line L2 parallel to the straight line L1. n The interval between the straight line L1 and the straight line L2 is not particularly limited, and is preferably set to a level corresponding to the size of a macro pattern or defect considered as a problem, for example.

[0111] By appropriately repeating the above operation, a plurality of voltages V1 to Vn are detected at a plurality of locations on the surface 11 to which the constant current I is supplied.

[0112] Next, the voltage ratio of two adjacent locations among the plurality of locations is calculated. Specifically, for example, Figure 2 In the example, the voltage V at the position bi-bi' (i is an integer selected from 1 to n) is i The voltage V of the adjacent part b(i-1)-b(i-1)' i-1 and the voltage V at position b(i+1)-b(i+1)' i+1 Compare them respectively and calculate V i / V i-1 and Vi+1 / V i (or V i-1 / V i and V i / V i+1 ). So far, the method for calculating the voltage ratio between two adjacent locations on the surface of the titanium material for producing the metal foil has been described.

[0113] (Chemical Composition)

[0114] The titanium material for metal foil manufacturing of the present embodiment has the following chemical composition: in mass %, it contains Sn: 0% to 2.0%, Zr: 0% to 5.0%, Al: 0% to 7.0%, N: 0% to 0.100%, C: 0% to 0.080%, H: 0% to 0.0150%, O: 0% to 1.000%, Fe: 0% to 0.500%, Cr: 0% to 0.500%, Ni: 0% to 0.090%, Cu: 0% to 1.5%, and Mo: 0% to 0.750%, the balance includes Ti and impurities, and the total content of Fe, Cr and Ni is 0% to 0.500%.

[0115] The titanium material for metal foil manufacturing of the present embodiment may contain Fe, Cr or Ni. Since Fe, Cr and Ni are β-phase stabilizing elements, the β-phase is easily formed by containing Fe, Cr and Ni. Since the β-phase is corroded before the α-phase, when a titanium roller having a titanium material containing a β-phase on its surface is used to manufacture metal foil, the β-phase is corroded first, and a macro pattern is generated on the roller surface. As a result, the macro pattern may be transferred to the metal foil. Therefore, the less Fe, Cr and Ni, the better. For example, the total content of Fe, Cr and Ni is preferably greater than 0 mass % and less than 0.500 mass %.

[0116] It is known that Fe, Cr and Ni will form compounds with Ti if their concentrations are high. Fe, Cr and Ni will form TiFe, TiCr2, and Ti2Ni together with Ti, for example. Among them, Ni is more likely to form compounds with Ti than Fe and Cr. Therefore, in the temperature domain where Ni or Ti can diffuse during hot rolling and annealing, a precursor stage, that is, a stage before the formation of Ti2Ni, will appear earlier, forming a Ni-enriched micro-region. If a Ni-enriched micro-region is formed, the hardness of the titanium material surface will be uneven, and polishing streaks will easily occur. As a result, macroscopic patterns are easily generated. In order to suppress this Ni enrichment, the Ni content is, for example, 0 mass% or more and 0.090 mass% or less. The Ni content is preferably 0.012 mass% or more. This is because, as a special phenomenon, there is a behavior that is prone to recrystallization when containing a very small amount of Ni, and it is easy to obtain a metallographic structure with uniform thickness as a whole, such as an equiaxed structure or a recrystallized structure, during heating in the rolling process or in the heat treatment process. In addition, the Ni content is preferably 0.070 mass% or less.

[0117] It should be noted that Cu also combines with Ti to form Ti2Cu. The ease with which Cu combines with Ti is similar to that of Fe and Cr.

[0118] The Fe content is, for example, 0.02 mass % or more and 0.500 mass % or less. As described above, the smaller the Fe, Cr, and Ni, the better, but the Fe content may be, for example, 0.040 mass % or more.

[0119] In addition, Fe, Cr and Ni are elements that distribute more to the liquid phase than to the solid phase during the solidification process of titanium. Therefore, these elements are elements that are easily segregated in titanium materials. When these elements segregate and cause uneven chemical composition, the surface state of the titanium material becomes uneven.

[0120] In order to reduce the non-uniformity of the chemical composition, the titanium material for metal foil manufacturing of the present embodiment preferably contains Mo. Although Mo is a β-phase stabilizing element like Fe, Cr, and Ni, unlike these elements, Mo is an element that distributes more to the solid phase than to the liquid phase during the solidification process of titanium. By containing Mo, the chemical composition in the titanium material becomes uniform, and the conductivity of the titanium material surface becomes uniform. As a result, the surface state of the titanium material becomes uniform, and the generation of macro patterns can be further suppressed.

[0121] The content of Mo is preferably 0.5 times or more and 1.2 times or less relative to the total content of Fe, Cr and Ni in mass %. When the content of Mo is 0.5 times or more and 1.2 times or less relative to the total content of Fe, Cr and Ni in mass %, the chemical composition becomes uniform, the surface state becomes uniform, and the generation of macro patterns can be suppressed. In addition, when the content of Mo is 0.5 times or more and 1.2 times or less relative to the total content of Fe, Cr and Ni in mass %, the formation of β phase can be suppressed to the extent that the difference in corrosion rate between α phase and β phase is not significant. As a result, the etching behavior of titanium and the electrodeposition state of copper in the electrolyte used for metal foil manufacturing can be made more stable. The content of Mo is more preferably 0.7 times or more relative to the total content of Fe, Cr and Ni in mass %. In addition, the content of Mo is more preferably 1.0 times or less relative to the total content of Fe, Cr and Ni in mass %.

[0122] For example, when the content of Fe in the titanium material is 0.0300 mass%, the content of Cr is 0.010 mass%, and the content of Ni is 0.020 mass%, the total content of Fe, Cr, and Ni is 0.060 mass%. Therefore, the content of Mo at this time is preferably 0.030 mass% or more and 0.072 mass% or less. It should be noted that Mo is not necessarily included, so the lower limit of the content of Mo is 0 mass%.

[0123] In addition, the titanium material for metal foil production according to the present embodiment may contain O, N, C, and H.

[0124] O helps to improve the strength of the titanium material and helps to increase the surface hardness. However, when the strength of the titanium material is too high, it is difficult to polish the titanium material when it is made into a roller. Therefore, when the titanium material for metal foil manufacturing contains O, the content of O is preferably 1.000 mass% or less. The content of O is more preferably 0.120 mass% or less, further preferably 0.065 mass% or less, and further preferably 0.055 mass% or less.

[0125] Since the solid solubility limit of N in α-Ti is lower than that of O, N tends to form nitrides with Ti. If nitrides are formed, streaks due to polishing or streaks due to corrosion during use may occur on the drum surface. Therefore, it is preferable to suppress the content of N as much as possible. The content of N may be, for example, 0.100 mass % or less, and more preferably 0.020 mass % or less.

[0126] Since C has a lower solid solubility limit in α-Ti than O, it tends to form carbides with Ti. If carbides are formed, similar to nitrides, streaks may be generated on the drum surface due to polishing or corrosion during use. Therefore, it is preferable to minimize the content of C. The content of C may be, for example, 0.080% by mass or less, and more preferably 0.020% by mass or less.

[0127] H forms hydrides together with Ti. If hydrides are formed, the titanium material may become brittle. In addition, hydrides may sometimes cause macroscopic patterns. Therefore, it is preferred to suppress the content of H as much as possible. The content of H is more preferably 0.013 mass % or less.

[0128] O, N, and C are elements that distribute to the solid phase more than to the liquid phase during the solidification process of titanium, similarly to Mo. Therefore, the above-mentioned Mo content can also be determined in consideration of the O, N, and C contents.

[0129] The titanium material for producing metal foil according to the present embodiment may contain at least any one of Cu, Sn, Zr, and Al.

[0130] The balance of the chemical composition of the titanium material for metal foil production of the present embodiment may be Ti and impurities. Specifically, impurities include Cl, Na, Mg, Si, Ca mixed in the refining process and Nb, Ta, V mixed in from scraps, and the amount of impurities is not a problem as long as it is 0.5% by mass or less in the total amount.

[0131] In the present embodiment, as described above, V is contained as an impurity. V is an element that slows down recrystallization. If V is contained too much, it is difficult to obtain a metallographic structure with uniform thickness as a whole, such as an equiaxed structure or a recrystallized structure, during heating in the rolling process or in the heat treatment process. Therefore, V is not added in the present embodiment.

[0132] More specifically, if possible impurities are also taken into consideration, the titanium material for metal foil production of the present embodiment may be

[0133] In terms of mass %, it may contain

[0134] N: 0% or more and 0.100% or less,

[0135] C: 0% or more and 0.080% or less,

[0136] H: 0% or more and 0.0150% or less,

[0137] O: 0% or more and 0.400% or less.

[0138] In addition, the titanium material for metal foil production of this embodiment is, for example,

[0139] Contains Fe, Cr, Ni and Mo,

[0140] The content of Ni is 0 mass % or more and 0.090 mass % or less,

[0141] The content of Mo is 0.5 times or more and 1.2 times or less the total content of Fe, Cr, and Ni on a mass basis.

[0142] In addition, the titanium material for metal foil production of this embodiment is, for example,

[0143] In terms of mass %, it may contain

[0144] N: 0% or more and 0.100% or less,

[0145] C: 0% or more and 0.080% or less,

[0146] H: 0% or more and 0.0150% or less,

[0147] O: 0% or more and 0.400% or less,

[0148] Fe: 0.02% or more and 0.500% or less,

[0149] Ni: 0% or more and 0.090% or less, and

[0150] Cu: 0% or more and 1.5% or less,

[0151] The balance contains Ti and impurities.

[0152] In addition, the titanium material for metal foil production of this embodiment is, for example,

[0153] The total amount of the compound selected from the group consisting of

[0154] Sn: 0.2% or more and 2.0% or less,

[0155] Zr: 0.2% or more and 5.0% or less, and

[0156] Al: one or more of the group consisting of 0.2% to 3.0%,

[0157] And contains by mass%

[0158] N: 0% or more and 0.100% or less,

[0159] C: 0% or more and 0.080% or less,

[0160] H: 0% or more and 0.0150% or less,

[0161] O: 0% or more and 1.000% or less, and

[0162] Fe: 0% or more and 0.500% or less,

[0163] The balance contains Ti and impurities.

[0164] In addition, the titanium material for metal foil production of the present embodiment contains, for example

[0165] Al is more than 1.8 mass % and less than 7.0 mass %, and the balance is Ti and impurities.

[0166] When the Al content is expressed as [Al%], the Zr content is expressed as [Zr%], the Sn content is expressed as [Sn%], and the O content is expressed as [O%], the Al equivalent Aleq represented by the following formula (1) is 7.0% by mass or less,

[0167] Aleq=[Al%]+[Zr%] / 6+[Sn%] / 3+10×[O%] Formula (1).

[0168] It should be noted that the lower limit of the content of each element described above is 0 mass %, and of course, the titanium material for metal foil production of the present embodiment does not need to contain the above elements.

[0169] The chemical composition of the titanium material for producing the metal foil according to the present embodiment has been described above.

[0170] In the titanium material for metal foil manufacturing of the present embodiment described above, since the voltage ratio between two adjacent sites among the plurality of sites on the surface is 0.95 or more and 1.05 or less, the influence of the chemical composition between the adjacent sites is uniform. As a result, there is no macro pattern between the adjacent sites, and the generation of macro patterns during metal foil manufacturing can be suppressed.

[0171] It should be noted that the macroscopic pattern can be observed by polishing the surface of the titanium plate with #800 sandpaper and corroding the surface with a 10 mass % nitric acid and 5 mass % hydrofluoric acid solution. As an example, Figure 3 , 4 The photo of the titanium surface with macroscopic patterns is shown. Figure 3 and Figure 4 These are photos of different titanium plates. "Macro pattern" refers to the part with different color stripes several mm long along the rolling direction. For example, Figure 4 in Figure 4 The arrow in (A) generates Figure 4 If such a macro pattern is produced on the titanium material, the macro pattern will be transferred to the metal foil finally manufactured.

[0172] As described above, the titanium material for metal foil manufacturing of the present embodiment can fully suppress the generation of macro patterns on the roller for metal foil manufacturing when in use, and is therefore suitable as a material for the roller for metal foil manufacturing. Therefore, one aspect of the present invention also relates to a metal foil manufacturing roller manufactured using the titanium material for metal foil manufacturing of the present invention. Such a metal foil manufacturing roller can suppress the generation of macro patterns and manufacture high-quality copper foil.

[0173] See also Figure 5 , 6 , a metal foil manufacturing roller manufactured using the titanium material for metal foil manufacturing of the present invention is described. Figure 5 This is a schematic diagram of a copper foil manufacturing device showing one way of using a metal foil manufacturing roller. Figure 6 Schematic diagram showing a metal foil manufacturing roller according to one embodiment of the present invention. Figure 5 As shown, it comprises: an electrolytic cell 110 storing a copper sulfate solution; an electrodeposition drum 120 disposed in the electrolytic cell 110, a part of which is immersed in the copper sulfate solution; and an electrode plate 130, which is immersed in the copper sulfate solution in the electrolytic cell 110 and is disposed opposite to the outer peripheral surface of the electrodeposition drum 120 at a predetermined interval. By applying a voltage between the electrodeposition drum 120 and the electrode plate 130, electrodeposition occurs on the outer peripheral surface of the electrodeposition drum 120 to generate copper foil F. The copper foil F having a predetermined thickness is peeled off from the metal foil manufacturing drum 120 by the winding unit 140, guided by the guide roller 150, and wound on the winding roller 160.

[0174] The electrodeposition drum 120 includes: a cylindrical inner drum 121; a titanium material 122 for metal foil production of the present embodiment coated along the outer circumference of the inner drum 121; a welding portion 123 arranged at the butt joint of the titanium material 122 for metal foil production; a side plate 124 provided on the side of the inner drum; and a rotating shaft 125. The metal foil production drum of the present embodiment is a part of the electrodeposition drum 120, and is composed of the titanium material 122 for metal foil production of the present embodiment coated along the outer circumference of the cylindrical inner drum 121, and the welding portion 123 arranged at the butt joint of the titanium material 122 for metal foil production. The side plate 124 covers both ends of the inner drum 121 and the titanium material 122 for metal foil production in the axial direction. In addition, the rotating shaft 125 is provided on the side plate 124 coaxially with the central axis A of the inner drum 121.

[0175] The metal foil manufacturing roller of this embodiment can be manufactured by a known method. For example, the titanium sheet for metal foil manufacturing of this embodiment is laid on the outer side surface of the inner roller, and the two butted ends of the titanium sheet for metal foil manufacturing processed into a cylindrical shape are welded.

[0176] The size of the metal foil production drum of the present embodiment is not particularly limited, and for example, the diameter may be 1 m or more, 2 m or more, or 5 m or less.

[0177] The metal foil manufacturing roller can suppress the generation of macro patterns and can manufacture high-quality copper foil.

[0178] The titanium material for metal foil production according to the present embodiment described above can be produced by any method, and can be produced, for example, by the method for producing the titanium material for metal foil production according to the present embodiment described below.

[0179] <Method for producing titanium material for metal foil production>

[0180] Next, the manufacturing method of the titanium material for metal foil manufacturing of the present embodiment is described. The manufacturing method of the titanium material for metal foil manufacturing of the present embodiment has the following steps: a step of manufacturing a titanium ingot by continuous casting, wherein molten titanium is poured into a coolable mold with openings on the upper and lower surfaces, and the liquid surface of the molten titanium in the mold is heated, while the titanium is cooled and solidified by means of the mold, and the solidified titanium is pulled downward using a clamp; a step of heating to a temperature of 750°C or more and less than the β transformation point, and rolling with a reduction rate of 90% or more to manufacture a rolled plate; and a step of heat treatment at a temperature of 600°C or more and 750°C or less for a time of 20 minutes or more and 120 minutes or less, cooling at an average cooling rate of 20°C / min or more from the heat treatment temperature to 500°C, and cooling at an average cooling rate of 10°C / min or less from the heat treatment temperature to a temperature of 300°C or less.

[0181] (Titanium ingot manufacturing process)

[0182] First, titanium having the above chemical composition is melted by electron beam melting (EBR) or plasma melting (PAM) to produce a titanium ingot. EBR is to emit an electron beam from an electron beam gun, and PAM is to emit a plasma arc from a plasma torch, irradiating a molten raw material mainly composed of titanium to melt it. Compared with the vacuum arc melting method (VAR) that relies on the arc between the titanium consumable electrode and the molten titanium in the water-cooled copper mold to melt the electrode, in EBR or PAM, the part where the molten titanium exists in the mold, that is, the molten pool, is shallower and the solidification rate is fast, so the solidification segregation of Fe, Cr, Ni, O, etc. can be reduced. By using a titanium ingot with suppressed solidification segregation, the titanium material for metal foil manufacturing can be made uniform. As a result, the surface state of the titanium material becomes uniform, and the generation of macro patterns can be suppressed.

[0183] For titanium melting, in order to stabilize the depth and shape of the molten pool, electron beam melting (EBR) is more preferably used because the irradiation scanning of the energy source is fast and easy, because the heat input distribution to the titanium liquid surface in the mold is uniform and stable.

[0184] Hereinafter, the electron beam melting method (EBR) and the plasma melting method (PAM) used in the method for producing the titanium material for metal foil production according to the present embodiment will be described in detail.

[0185] [Electron Beam Melting (EBR)]

[0186] Electron beam melting is a method of melting a metal such as titanium in a vacuum by using an electron beam emitted from an electron gun, and then pouring the molten metal into a water-cooled copper mold or other mold to solidify it to produce an ingot. Generally, the ingot is continuously cast while being drawn out using a bottomless mold. At this time, the molten metal liquid surface in the mold is heated by irradiating an electron beam, while maintaining the liquid surface in the mold.

[0187] In order to stabilize the depth and shape of the molten pool and maintain the liquid level, it is preferred that the irradiation power of the electron beam in the mold be divided by the area of ​​the mold, that is, the irradiation amount per unit area be 150 W / cm 2 The titanium is melted under the conditions of 0.5 to 2.0 t / h and a melting rate of 2.5 t / h or less. The melting rate is more preferably 0.5 to 2.0 t / h.

[0188] [Plasma Melting Method (PAM)]

[0189] Plasma melting is a method of producing an ingot by melting a metal such as titanium in an inert gas atmosphere such as an argon atmosphere using a plasma arc emitted from a plasma torch, pouring the molten metal into a water-cooled copper mold or other mold to solidify it. Generally, a bottomless mold is used to continuously cast the ingot while drawing it out. At this time, the plasma arc is irradiated onto the molten metal surface in the mold to heat it, while maintaining the liquid level in the mold.

[0190] In order to stabilize the depth and shape of the molten pool and maintain the liquid level, it is preferred that the irradiation power of the plasma into the mold be divided by the area of ​​the mold, that is, the irradiation amount per unit area be 380 W / cm 2 The titanium is melted under the conditions of 0.5 to 2.0 t / h and a melting rate of 2.5 t / h or less. The melting rate is more preferably 0.5 to 2.0 t / h.

[0191] An example of a horizontal cross section of a mold 40 used in EBR or PAM is as follows Figure 7 , Figure 8 As shown. Figure 7 The circular mold 40A shown in FIG. Figure 8The rectangular mold 40B shown is a representative example of a horizontal cross section of a mold used in EBR or PAM. In this horizontal cross section, the internal space 41A of the mold 40A and the internal space 41B of the mold 40B are each in cm. 2 The ratio of the area to the perimeter in cm, that is, the area / perimeter is preferably greater than 7.5 cm and less than 22.5 cm. As a result, the cooling rate of the titanium melt brought by the casting mold becomes faster, which can further suppress solidification segregation. The area / perimeter is more preferably less than 15.0 cm, and further preferably less than 11.0 cm. Such an area / perimeter casting mold can significantly suppress solidification segregation. From the perspective of productivity, the area / perimeter is preferably substantially greater than 7.5 cm. It should be noted that when the horizontal cross-section is in the shape of a rectangle, for example, its four corners C are often chamfered to form a polygon, so considering the following Figure 8 The above-mentioned area and perimeter are obtained by using the shape shown. It should be noted that the thickness of the mold is not particularly limited, and may be, for example, less than 300 mm.

[0192] As described above, EBR is suitable for stably maintaining the molten metal surface and the shape of the molten pool in the mold because the irradiation position of the electron beam is easily moved. Therefore, by using electron beam melting, the irradiation amount per unit area (Y) of the irradiation power of the electron beam to the mold is controlled within the range of formula (2) based on the area / perimeter (X), and the molten metal surface and the shape of the molten pool in the mold can be further stably maintained.

[0193] Y = -3.8X + (135 ± 25) Formula (2)

[0194] (Slab Manufacturing Process)

[0195] The manufacturing method of the titanium material for metal foil manufacturing of the present embodiment preferably has a slab manufacturing process of hot working the titanium ingot to manufacture the slab, and in the process of manufacturing the rolled plate, the above-mentioned slab is rolled to replace the titanium ingot. For example, as needed, the titanium ingot can be hot forged or initially rolled based on a known method before rolling to manufacture the slab from the titanium ingot. This process can be implemented whether it is a cylindrical ingot or a rectangular ingot, even if the thickness or width needs to be adjusted. By using this slab, it can be rolled more uniformly in the rolling process, and the metallographic structure can be made more uniform.

[0196] (Rolling process)

[0197] Next, the titanium ingot is directly rolled, or the slab that has been hot-worked into a rolling shape is rolled as needed to produce a rolled plate. In this process, the rolled billet is heated to a temperature of 750°C or higher and lower than the β transformation point, and rolled at a reduction ratio of 90% or higher. The heating temperature and reduction ratio are described below.

[0198] The heating temperature in this process is 750°C or higher and lower than the β phase transformation point. By heating to a temperature of 750°C or higher and lower than the β phase transformation point, the metallographic structure can be fully equiaxed, which can prevent the rolled plate from generating macroscopic patterns. The rolling temperature is preferably 200°C or higher. In addition, the rolling temperature is preferably (β phase transformation point - 50)°C or lower.

[0199] The reduction rate in this process is 90% or more. By making the reduction rate 90% or more, the coarse grains can be fully refined, the metallographic structure of the rolled plate can be equiaxed, and the generation of macroscopic patterns can be prevented. Since the higher the reduction rate in this process, the better the structure, it can be determined according to the required product size and the characteristics of the manufacturing rolling mill.

[0200] Furthermore, by heating the titanium ingot to a temperature of 750° C. or higher and lower than the β transformation point and rolling it at a reduction ratio of 90% or higher, recrystallization nuclei can be uniformly and sufficiently introduced into the entire rolled sheet.

[0201] Here, in the present embodiment, "β phase transition point" means the boundary temperature at which the α phase begins to be generated when the titanium alloy is cooled from the β phase single phase domain. The β phase transition point can be obtained from the phase diagram. The phase diagram can be obtained, for example, by the CALPHAD (Computer Coupling of Phase Diagrams and Thermochemistry) method. Specifically, the phase diagram of the titanium alloy can be obtained by the CALPHAD method using Thermo-Calc, a comprehensive thermodynamic calculation system of Thermo-CalcSotware AB, and a prescribed database (TI3), and the β phase transition point can be calculated.

[0202] (Heat treatment process)

[0203] Next, the rolled plate is heat treated at a temperature of 600°C or more and 750°C or less for a time of 20 minutes or more and 120 minutes or less, and cooled at an average cooling rate of 20°C / minute or more from the heat treatment temperature to 500°C, and cooled at an average cooling rate of 10°C / minute or less from the heat treatment temperature to a temperature below 300°C. By heat treating at a temperature of 600°C or more and 750°C or less for a time of 20 minutes or more and 120 minutes or less, a uniform recrystallized structure can be formed on the rolled plate as a whole. In addition, by making the average cooling rate from the heat treatment temperature to 500°C or more than 20°C / minute, the element distribution with the second phase formation generated during the cooling process as the driving force is reduced, and the fine component distribution unevenness caused by the element distribution is suppressed. In addition, by cooling at a rate of 10°C / minute or less from the heat treatment temperature to a temperature below 300°C, the residual strain caused by the thermal shrinkage generated by the cooling can be reduced. As a result, a high uniformity titanium plate with uniform component distribution and residual strain can be obtained.

[0204] (Inspection process)

[0205] For titanium materials obtained through the heat treatment process, the above method can be used to inspect the surface uniformity.

[0206] The titanium material manufactured by the manufacturing method of the titanium material for metal foil manufacturing of the present embodiment has uniform chemical composition and metallographic structure. Therefore, on the surface of the titanium material manufactured by the manufacturing method of the titanium material for metal foil manufacturing of the present embodiment, a constant current is supplied by making a pair of energized electrode probes contact the surface, and among the multiple voltages detected by making the potential detection probe pair contact multiple locations of the above-mentioned surface with a certain probe interval, the voltage ratio of two adjacent locations is 0.95 or more and 1.05 or less. As a result, when the titanium material manufactured by the manufacturing method of the titanium material for metal foil manufacturing of the present embodiment is used for a roller for metal foil manufacturing, the generation of macro patterns can be suppressed.

[0207] The method for producing the titanium plate according to the present embodiment has been described above.

[0208] It should be noted that the titanium material for metal foil manufacturing of the present embodiment is hot-mounted on the inner roller as described above, and the surface is polished to form the skin of the metal foil manufacturing roller. If the load during polishing is uneven, the amount of strain introduced directly below the roller surface may be uneven. If the amount of strain is uneven, the resistivity of the surface of the metal foil manufacturing roller may change. Therefore, the fluctuation range of the load when polishing the metal foil manufacturing roller is preferably less than 10%, more preferably less than 5%, and further preferably less than 3%.

[0209] It should be noted that the metal foil produced by the metal foil producing roll made of a metal foil producing titanium material is not particularly limited, and examples thereof include copper foil, nickel foil, aluminum foil, and iron foil.

[0210] The following specifically describes the embodiments of the present invention while showing examples. It should be noted that the following embodiments are merely examples of the present invention, and the present invention is not limited to the following examples.

[0211] [Example 1]

[0212] (Manufacturing of titanium materials)

[0213] First, a plurality of titanium raw materials having different chemical compositions are prepared, and the titanium raw materials are melted using the melting methods shown in Tables 1 to 6 to produce titanium ingots.

[0214] [Table 1]

[0215]

[0216] [Table 2]

[0217]

[0218] [Table 3]

[0219]

[0220] [Table 4]

[0221]

[0222] [Table 5]

[0223]

[0224] [Table 6]

[0225]

[0226] In the electron beam melting method, the irradiation power of the electron beam into the mold is adjusted according to the shape of the mold so that the irradiation amount (Y) per unit area is controlled within the range of formula (2) according to the area / perimeter (X) of the mold, and the target is set to the approximate center value of formula (2). Although there are cases where the electron beam irradiation power is different from the center value of formula (2), the irradiation amount of the electron beam in the electron beam melting method is 150W / cm 2 In addition, the target was set at 1.0 ton / h so that the melting rate would be 2.5 ton / h or less.

[0227] Y = -3.8X + (135 ± 25) Formula (2)

[0228] In the plasma melting method, the plasma irradiation power to the mold is 380W / cm 2 In addition, the target was set at 1.0 ton / h so that the melting rate would be 2.5 ton / h or less.

[0229] In the vacuum arc melting method, a water-cooled copper mold with a bottom (without an opening on the lower surface) and a diameter of 750 mm was used to melt an electrode formed of a titanium raw material.

[0230] The molds shown in Tables 1 to 6 were used for casting the molten titanium. The "horizontal cross-sectional shape of the inner space of the mold" shown in Tables 1 to 6 is the approximate shape of the horizontal cross section of the mold in the inner space of the mold, and the "specific cross-sectional dimensions of the mold" shows the diameter R, short side A, long side B, corner C, and its area and perimeter of the horizontal cross section of the inner space of the mold.

[0231] In addition, the "irradiation amount" in Tables 1 to 6 is the irradiation amount per unit area in the mold when the ingot production method is EBR and PAM.

[0232] For the manufactured titanium ingot, when it is cylindrical and 750mmφ and when it is rectangular and has a thickness of more than 350mm, after trimming the casting surface by cutting, hot forging is performed to form a slab with a thickness of 250mm. When the ingot is rectangular and has a thickness of less than 260mm, hot forging is not performed, and the casting surface is trimmed by cutting. These materials are heated to 800°C and rolled with a reduction rate of more than 90% to manufacture a rolled plate with a thickness of 8 to 15mm. Then, the rolled plate is heat treated at a temperature of 700°C for 30 minutes, and the heat-treated rolled plate is cooled in a manner such that the average cooling rate from the heat treatment temperature to 500°C is 20°C / minute and the average cooling rate from the heat treatment temperature to 300°C is 10°C / minute to manufacture a plate-shaped titanium material. It should be noted that temperature control is performed by airflow and a heater.

[0233] (Manufacture of metal foil production rolls)

[0234] The manufactured titanium material is formed into a tube, and then hot-fitted onto a cylindrical titanium material (inner roller), and its surface is polished to manufacture an electrodeposition roller. The fluctuation range of the load during polishing is less than 10%.

[0235] (Analysis and Evaluation)

[0236] The titanium materials of the examples and comparative examples were evaluated for their average chemical composition, voltage ratio, and macroscopic pattern. In addition, the electrodeposition rollers made of these titanium materials were evaluated for their voltage ratio.

[0237] For the average chemical composition, O and N were analyzed by the inert gas fusion method using an analysis device (device name ON736) produced by LECO Japan Contract Co., Ltd. Specifically: O was analyzed by the non-dispersive infrared absorption method, and N was analyzed by the thermal conductivity method. C was analyzed by the infrared absorption method using an analysis device (device name CS444) produced by LECO Japan Contract Co., Ltd. H was analyzed by the thermal conductivity method using an analysis device (device name EMGA-800M) produced by Horiba, Ltd. Fe, Ni, Cr, and Mo were analyzed by ICP emission spectrometry using an analysis device (device name ICPS8100) produced by Shimadzu Corporation.

[0238] The voltage ratio is calculated and evaluated by the following method. A pair of energized electrode probes are brought into contact with the surface of the titanium material to supply a constant current. Figure 2 The arrangement shown in the figure is made to contact the potential detection probe pair with the surface of the titanium material along the straight line L1 direction with a probe interval of 30 mm, and the voltage is measured. Next, the energized electrode probe is moved 30 mm in a direction perpendicular to the straight line L1, and the potential detection probe pair is brought into contact with the surface of the titanium material along the straight line L2, and the voltage is measured. This process is repeated to measure the voltage on the surface of the titanium material, and the voltage ratio of adjacent parts is calculated from the measured voltage.

[0239] The voltage ratio was evaluated as follows based on the ratio of data with a voltage ratio of less than 0.95 or greater than 1.05 to the total number of data of the calculated voltage ratio.

[0240] Excellent (A): The proportion of data with voltage ratio less than 0.95 or greater than 1.05 in the total number of calculated voltage ratio data is less than 2%

[0241] Good (B): The proportion of data with a voltage ratio less than 0.95 or greater than 1.05 to the total number of data with calculated voltage ratios is 2% or more and less than 5%

[0242] Acceptable (C): The proportion of data with a voltage ratio less than 0.95 or greater than 1.05 in the total number of calculated voltage ratio data is more than 5%

[0243] In addition, the examples evaluated as excellent (A) were evaluated as follows based on the calculated values ​​of the voltage ratio.

[0244] Excellent (AAA): All voltage ratios except for those less than 0.95 or greater than 1.05 are 0.98 or higher and 1.02 or lower

[0245] Better (AA): All voltage ratios of data other than the voltage ratio less than 0.95 or greater than 1.05 were 0.97 or more and 1.03 or less (excluding the case of excellent)

[0246] Good (A): All voltage ratios of data other than those less than 0.95 or greater than 1.05 were 0.95 or more and 1.05 or less (excluding excellent and better cases)

[0247] The macro pattern was observed by polishing the surface of 20 titanium plates of 50×100 mm in size in each invention example and comparative example with #800 sandpaper and corroding the surface with 10% nitric acid and 5% hydrofluoric acid solution. Then, the striped pattern with a length of more than 3 mm was regarded as the macro pattern, and the evaluation was performed as follows according to the proportion of the striped pattern.

[0248] Excellent (A): The ratio is less than 0.05 pieces / piece

[0249] Good (B): The ratio is greater than 0.05 pieces / piece and less than 0.15 pieces / piece

[0250] Acceptable (C): The ratio is greater than 0.15 pieces / piece

[0251] The above evaluation results are shown in Tables 7 to 12.

[0252] [Table 7]

[0253]

[0254] [Table 8]

[0255]

[0256] [Table 9]

[0257]

[0258] [Table 10]

[0259]

[0260] [Table 11]

[0261]

[0262] [Table 12]

[0263]

[0264] As shown in Tables 1 to 12, when the area / perimeter of the titanium material manufactured by the ingot melted by EBR or PAM is less than 22.5 cm, the data with a voltage ratio less than 0.95 or greater than 1.05 accounts for less than 2% of the total number of data of the calculated voltage ratio, and all voltage ratios of the data other than the voltage ratio less than 0.95 or greater than 1.05 are greater than 0.95 and less than 1.05. In addition, the macroscopic pattern on the surface of this titanium material is suppressed. When the area / perimeter of the horizontal cross-section of the inner space of the mold used for ingot manufacturing is less than 15.0 cm, the data with a voltage ratio less than 0.95 or greater than 1.05 accounts for less than 2% of the total number of data of the calculated voltage ratio, and all voltage ratios of the data other than the voltage ratio less than 0.95 or greater than 1.05 are greater than 0.97 and less than 1.03. In addition, the macroscopic pattern on the surface of this titanium material is further suppressed. When the area / perimeter is less than 11.0 cm, the proportion of data with a voltage ratio less than 0.95 or greater than 1.05 to the total number of data of the calculated voltage ratio is less than 2%, and all voltage ratios of data other than data with a voltage ratio less than 0.95 or greater than 1.05 are greater than 0.98 and less than 1.02. In addition, the macroscopic pattern on the surface of the titanium material is extremely suppressed.

[0265] In addition, when the content of Mo is 0.5 times or more and 1.2 times or less relative to the total content of Fe, Cr and Ni, the proportion of data with a voltage ratio less than 0.95 or greater than 1.05 to the total number of data of the calculated voltage ratio is less than 2%, and all voltage ratios of data other than data with a voltage ratio less than 0.95 or greater than 1.05 are 0.98 or more and 1.02 or less. In addition, the macroscopic pattern on the surface of such titanium material is extremely suppressed.

[0266] In addition, for the manufactured metal foil manufacturing roller, the evaluation results of the voltage ratio were equivalent to the evaluation results of the voltage ratio of the titanium material, and the evaluation results of the macro pattern of the roller surface were also the same as the evaluation results of the macro pattern of the titanium material surface. Therefore, it can be seen that the manufacturing process of the metal foil manufacturing roller has little effect on the intrinsic factors of the titanium material for metal foil manufacturing.

[0267] [Example 2]

[0268] The titanium material was produced, the metal foil production roll was produced, and the analysis and evaluation were carried out in the same manner as in Example 1 except that the Al content was changed.

[0269] [Table 13]

[0270]

[0271] [Table 14]

[0272]

[0273] [Table 15]

[0274]

[0275] [Table 16]

[0276]

[0277] [Table 17]

[0278]

[0279] [Table 18]

[0280]

[0281] [Table 19]

[0282]

[0283] [Table 20]

[0284]

[0285] As shown in Tables 13 to 20, when the voltage ratio of two adjacent sites in the plurality of sites is 0.95 to 1.05, the macro pattern of the surface is suppressed. In addition, when the Al content is greater than 1.8 mass % and less than 7.0 mass %, and Aleq is less than 7.0 mass %, the macro pattern of the surface is suppressed. In addition, when the Al content is greater than 1.8 mass % and less than 7.0 mass %, and Aleq is less than 7.0 mass %, the macro pattern of the surface is suppressed.

[0286] In addition, the evaluation results of the voltage ratio of the manufactured metal foil production roller were equivalent to the evaluation results of the voltage ratio of the titanium material, and the evaluation results of the macro pattern of the roller surface were also the same as the evaluation results of the macro pattern of the titanium material surface.

[0287] [Example 3]

[0288] For the titanium ingots shown in Tables 21 and 22, when they are rectangular and have a thickness of 350 mm or more, the casting surface is trimmed by cutting, etc., and then hot forging is performed to form a slab with a thickness of 250 mm. When the ingot is rectangular and has a thickness of 260 mm or less, hot forging is not performed, and the casting surface is trimmed by cutting, etc. Then, titanium materials are manufactured under the rolling conditions and heat treatment and cooling conditions shown in Tables 23 to 25. In addition, the manufacture, analysis and evaluation of the metal foil manufacturing roller were also carried out, which were carried out in the same manner as in Example 1.

[0289] The β transformation points shown in Tables 22 to 25 are values ​​calculated by obtaining a phase diagram of a titanium alloy based on the CALPHAD method using Thermo-Calc, a comprehensive thermodynamic calculation system of Thermo-Calc Sotware AB and a predetermined database (TI3).

[0290] [Table 21]

[0291]

[0292] [Table 22]

[0293]

[0294] [Table 23]

[0295]

[0296] [Table 24]

[0297]

[0298] [Table 25]

[0299]

[0300] As shown in Tables 21 to 25, when a titanium material is manufactured by heating a titanium ingot to a temperature of not less than 750°C and less than the β transformation point, rolling with a reduction rate of not less than 90%, heat treating at a temperature of not less than 600°C and not more than 750°C for a time of not less than 20 minutes and not more than 120 minutes, cooling from the heat treatment temperature to 500°C at an average cooling rate of not less than 20°C / min, and cooling from the heat treatment temperature to a temperature of not more than 300°C at an average cooling rate of not more than 10°C / min, the macroscopic pattern on the surface of the titanium material is suppressed.

[0301] In addition, the evaluation results of the voltage ratio of the manufactured metal foil production roller were equivalent to the evaluation results of the voltage ratio of the titanium material, and the evaluation results of the macro pattern of the roller surface were also the same as the evaluation results of the macro pattern of the titanium material surface.

[0302] [Example 4]

[0303] As shown in Tables 26 and 27, the titanium ingot is manufactured by changing the irradiation amount of the electron beam to the inner space of the mold or the irradiation amount of the plasma to the mold and the melting rate. Regarding the "irradiation amount" in Tables 26 and 27, when the manufacturing method of the titanium ingot is electron beam melting, it means the irradiation amount of the electron beam to the inner space of the mold; when the manufacturing method of the titanium ingot is plasma melting, it means the irradiation amount of the plasma to the mold.

[0304] For the titanium ingot manufactured, when it is cylindrical and 750mmφ and when it is rectangular and has a thickness of 350mm or more, after trimming the casting surface by cutting, hot forging is performed to make a slab with a thickness of 250mm. When the ingot is rectangular and has a thickness of less than 260mm, hot forging is not performed, and the casting surface is trimmed by cutting. These materials are heated to 800°C to manufacture a rolled plate with a thickness of 8mm. Then, the rolled plate is heat treated at a temperature of 700°C for 30 minutes, and the rolled plate after heat treatment is cooled in a manner such that the average cooling rate from the heat treatment temperature to 500°C is 20°C / minute and the average cooling rate from the heat treatment temperature to 300°C is 10°C / minute to manufacture a plate-shaped titanium material. It should be noted that temperature control is performed by airflow and heater. The results are shown in Table 28. It should be noted that the average chemical composition IG1 to IG9 of the titanium material shown in Table 28 represents the same average chemical composition as the symbols IG1 to IG9 shown in Table 22.

[0305] [Table 26]

[0306]

[0307] [Table 27]

[0308]

[0309] [Table 28]

[0310]

[0311] As shown in Tables 26 to 28, the electron beam irradiation dose to the inner space of the mold in the electron beam melting method is 150 W / cm 2 When the melting rate is less than 2.5 tons / h, the voltage ratio and macro pattern evaluation results are excellent, and the macro pattern is also extremely suppressed. In addition, the plasma irradiation dose to the mold in the plasma melting method is 380W / cm 2 When the melting rate was 2.5 tons / h or less, the evaluation results of the voltage ratio and the macro pattern were also excellent, and the macro pattern was also extremely suppressed.

[0312] In addition, the evaluation results of the voltage ratio of the manufactured metal foil production roller were equivalent to the evaluation results of the voltage ratio of the titanium material, and the evaluation results of the macro pattern of the roller surface were also the same as the evaluation results of the macro pattern of the titanium material surface.

[0313] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited to the examples. Obviously, a person with common knowledge in the technical field to which the present invention belongs can think of various variations or modifications within the scope of the technical concept recorded in the claims, and it should be understood that these also belong to the technical scope of the present invention.

[0314] Description of Reference Numerals

[0315] 10Titanium materials for metal foil manufacturing

[0316] 11 Surface

[0317] 12 Uneven parts

[0318] 20A, 20B powered electrode probe

[0319] 30A, 30B potential detection probe

[0320] 40, 40A, 40B casting mold

[0321] 41A, 41B internal space

[0322] 100 Copper foil manufacturing equipment

[0323] 110 Electrolyzer

[0324] 120 Electrodeposition Roller

[0325] 121 Inner drum

[0326] 122 Titanium

[0327] 123 Welding Department

[0328] 124 Side Panel

[0329] 125 Rotation axis

[0330] 130 Electrode Plate

[0331] 140 Coiling Department

[0332] 150 Guide Roller

[0333] 160 Take-up Roller

Claims

1. A titanium material for metal foil manufacturing, having the following chemical composition: Contains by mass% Sn: 0% or more and 2.0% or less, Zr: 0% or more and 5.0% or less, Al: 0% or more and 7.0% or less, N: 0% or more and 0.100% or less, C: 0% or more and 0.080% or less, H: 0% or more and 0.0150% or less, O: 0% or more and 1.000% or less, Fe: 0% or more and 0.500% or less, Cr: 0% or more and 0.500% or less, Ni: 0% or more and 0.090% or less, Cu: 0% or more and 1.5% or less, and Mo: 0% or more and 0.750% or less, The balance includes Ti and impurities, The total content of Fe, Cr and Ni is 0% or more and 0.500% or less; When a pair of powered electrode probes are brought into contact with the titanium material for metal foil manufacturing to supply a constant current, and a pair of potential detection probes are brought into contact with the surface of the titanium material for metal foil manufacturing with a certain probe interval to measure the voltages at multiple locations on the surface, the voltage ratio between two adjacent locations among the multiple locations is greater than 0.95 and less than 1.

05.

2. The titanium material for metal foil production according to claim 1, comprising Fe, Cr, Ni and Mo. The content of Ni is 0 mass % or more and 0.090 mass % or less, The content of Mo is 0.5 times or more and 1.2 times or less the total content of Fe, Cr, and Ni on a mass basis.

3. The titanium material for metal foil production according to claim 1 or 2, which contains, by mass %, N: 0% or more and 0.100% or less, C: 0% or more and 0.080% or less, H: 0% or more and 0.0150% or less, O: 0% or more and 0.400% or less, Fe: 0.02% or more and 0.500% or less, Ni: 0% or more and 0.090% or less, and Cu: 0% or more and 1.5% or less.

4. The titanium material for metal foil production according to claim 1, comprising a total amount of 0.2% to 5.0% by mass. Sn: 0.2% or more and 2.0% or less, Zr: 0.2% or more and 5.0% or less, and Al: one or more of the group consisting of 0.2% to 3.0%, And contains by mass% N: 0% or more and 0.100% or less, C: 0% or more and 0.080% or less, H: 0% or more and 0.0150% or less, O: 0% or more and 1.000% or less, and Fe: 0% or more and 0.500% or less.

5. The titanium material for metal foil production according to claim 1, comprising more than 1.8 mass % and 7.0 mass % or less of Al, When the Al content is expressed as [Al%], the Zr content is expressed as [Zr%], the Sn content is expressed as [Sn%], and the O content is expressed as [O%], the Al equivalent Aleq represented by the following formula (1) is 7.0% by mass or less, Aleq=[Al%]+[Zr%] / 6+[Sn%] / 3+10×[O%] Formula (1). The titanium material for metal foil production according to claim 1 or 2, which is a titanium material for a roll for metal foil production.

7. A method for producing a titanium material for metal foil production, the method comprising the following steps: The process of manufacturing titanium ingots by continuous casting. in, The molten titanium is poured into a coolable casting mold with openings on the upper and lower surfaces, and the liquid surface of the molten titanium in the casting mold is heated, and the titanium is cooled and solidified by the casting mold, and the solidified titanium is pulled downward using a clamp; The titanium ingot is heated to a temperature of 750° C. or higher and lower than the β transformation point, and rolled at a reduction ratio of 90% or higher to produce a rolled plate; and A process of performing heat treatment at a temperature of 600°C to 750°C for 20 minutes to 120 minutes, cooling from the heat treatment temperature to 500°C at an average cooling rate of 20°C / min or more, and cooling from the heat treatment temperature to a temperature of 300°C or less at an average cooling rate of 10°C / min or less.

8. The method for producing a titanium material for metal foil production according to claim 7, comprising the step of hot working the titanium ingot to produce a slab, In the step of manufacturing the rolled plate, the slab is rolled instead of the titanium ingot.

9. The method for producing a titanium material for metal foil production according to claim 7 or 8, in, The casting method is electron beam melting. The electron beam irradiation amount to the inner space of the mold in the electron beam melting method is 150W / cm 2 The titanium is irradiated with the electron beam to melt the titanium at a melting rate of 2.5 tons / h or less.

10. The method for producing a titanium material for metal foil production according to claim 9, in, The ratio X of the horizontal cross-sectional area of ​​the internal space of the mold to the circumference of the inner circumference of the horizontal cross-sectional area of ​​the mold and the irradiation amount Y of the electron beam in the electron beam melting method satisfy the relationship of the following formula (2), where the unit of X is cm and the unit of Y is W / cm 2 , Y = -3.8X + (135 ± 25) formula (2).

11. The method for producing a titanium material for metal foil production according to claim 7 or 8, in, The casting method is plasma melting method. The plasma irradiation amount of the plasma in the mold in the plasma melting method is 380W / cm 2 The titanium is irradiated with the plasma to melt the titanium at a melting rate of 2.5 tons / h or less.

12. The method for producing a titanium material for metal foil production according to claim 7 or 8, in, The unit of the horizontal cross section of the space inside the mold is cm 2 The ratio of the area to the perimeter in cm is greater than or equal to 7.5 cm and less than or equal to 22.5 cm.

13. A metal foil manufacturing roller, comprising: the titanium material for metal foil manufacturing according to claim 6 coated along the outer peripheral surface of a cylindrical inner roller; and A welding portion is arranged at the butting portion of the titanium material.