A PBT composite material and its preparation method and application
By using alkali-free flat glass fiber and diethyl aluminum hypophosphite-melamine polyphosphate flame retardant system in PBT materials, combined with phosphate esters and fatty acid salts, the problem of cracking of PBT materials in hot and cold shock environments has been solved and achieved PBT composite materials with high fluidity and strong welding lines meet the flame retardant and impact resistance requirements of the electronic and electrical industry.
Patent Information
- Application Number
- CN202310170046.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-27
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-02-27
AI Technical Summary
Existing halogen-free flame retardant reinforced PBT materials are prone to cracking in hot and cold shock environments, and the added modifiers have harmful odors or high costs.
Using a combination of alkali-free flat glass fiber, diethyl aluminum hypophosphite-melamine polyphosphate flame retardant system, phosphate ester and fatty acid salt, through high-speed stirring and twin-screw extruder processing, high fluidity and high welding are prepared Line strength PBT composite.
It achieves high fluidity, strong welding lines and excellent thermal and cold shock resistance of the material, meets the requirements of the electronic and electrical industry, and verifies the flame retardant performance through the UL-94 standard.
Smart Images

Figure FT_1 
Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, and in particular to a PBT composite material and a preparation method and application thereof. Background Art
[0002] As one of the five major engineering plastics, polybutylene terephthalate (PBT) is widely used in various fields due to its excellent processing performance, solvent resistance, electrical properties and heat resistance. At present, the research on PBT materials mainly focuses on flame retardant modification and reinforcement modification. With the promotion of EU ROHS and REACH regulations, halogen-free flame retardant reinforced PBT has received more and more attention. In the application of some plastic-coated metal products, due to the large difference in the linear expansion coefficient of plastic and metal inserts, when used in an environment with drastic temperature rise and fall caused by natural ambient temperature changes or their own working temperature rise (such as lighting, cooling fan applications), it is easy to cause cracking problems and make the functional parts fail. Therefore, it is necessary to further improve the cold and heat shock resistance of halogen-free flame retardant reinforced PBT.
[0003] Chinese patent application CN102056986A discloses a method of improving the thermal shock resistance of reinforced PBT materials by adding carbodiimide and elastomer. However, carbodiimide easily reacts with active hydrogen to produce isocyanate with a pungent odor, resulting in a bad production environment. In addition, the addition of elastomer significantly reduces the mechanical strength and fluidity of the material. Chinese patent application CN112625406A discloses adding PCTG resin, fluorine-containing processing aid and benzene plasticizer to glass fiber reinforced PBT material to obtain a polyester composition with low processing odor, high welding strength and good thermal shock resistance. However, the price of PCTG is high and the benzene plasticizer may precipitate during the use of the material. Summary of the invention
[0004] In order to overcome the deficiencies of the above-mentioned prior art, the object of the present invention is to provide a halogen-free flame retardant reinforced PBT composite material with high fluidity, high weld line strength and good resistance to cold and hot shock, no precipitation problem and easy processing.
[0005] Another object of the present invention is to provide a method for preparing the above-mentioned PBT composite material.
[0006] The present invention is achieved through the following technical solutions:
[0007] A PBT composite material, comprising the following components by weight:
[0008] 38-53 parts of PBT resin;
[0009] 27~33 parts of alkali-free flat glass fiber;
[0010] 15-18 parts of diethyl aluminum hypophosphite;
[0011] 2-5 parts of melamine polyphosphate;
[0012] Phosphate 1-3 parts;
[0013] 1-2 parts of fatty acid salt;
[0014] 1-3 parts of toughening agent.
[0015] The alkali-free flat glass fiber used in the present invention is beneficial to improving the fluidity of the material, and the linear expansion coefficient perpendicular to the flow direction is smaller, so that the material is not easy to crack when subjected to cold or hot shock. Preferably, the flatness ratio of the alkali-free flat glass fiber is 1: (3-4), preferably 1: (3.5-4). The flatness ratio is the ratio of the short diameter to the long diameter of the stripped fiber cross section.
[0016] Preferably, the weight ratio of diethyl aluminum hypophosphite to melamine polyphosphate is (3-9): 1, more preferably (5.5-9): 1. Adding a certain proportion of melamine polyphosphate is beneficial to improving the fluidity and weld line strength of the material, while when the amount of melamine polyphosphate added is too high, the fluidity and weld line strength of the material will decrease, and the thermal shock resistance will deteriorate.
[0017] Preferably, the pH value of the saturated aqueous solution of the melamine polyphosphate at 25° C. is 5-6.5, more preferably 5.5-6.5. The lower the pH value of the melamine polyphosphate, the stronger its acidity, which is likely to cause degradation of the PBT resin during production, resulting in decreased mechanical properties.
[0018] The invention can plasticize the PBT resin and improve its fluidity by adding a small amount of phosphate and fatty acid salt, and on the other hand, the phosphate and the diethyl aluminum hypophosphite-melamine polyphosphate flame retardant system have a synergistic effect to further stabilize the flame retardant performance of the material, while the fatty acid salt can improve the crystallization of the PBT resin and reduce its crystal size, which is beneficial to improving the cold and heat shock resistance of the material.
[0019] Preferably, the phosphate ester is selected from one or more of bisphenol A bis(diphenyl phosphate), resorcinol bis(diphenyl phosphate) or hydroquinone bis(diphenyl phosphate).
[0020] Preferably, the fatty acid salt is selected from lignite fatty acid salt; the lignite fatty acid salt is preferably any one or more of lignite fatty acid sodium salt or lignite fatty acid calcium salt.
[0021] Preferably, the toughening agent is selected from any one or more of ethylene-vinyl acetate copolymer, ethylene-methyl acrylate copolymer or ethylene-butyl acrylate copolymer.
[0022] According to the material performance requirements, the PBT composite material of the present invention further comprises 0-1 part of an auxiliary agent by weight. The auxiliary agent is selected from any one or more of an antioxidant or a lubricant.
[0023] Suitable lubricants include any one or more of aliphatic carboxylic acid esters, erucic acid amide, ethylene bisstearamide, montan esters, polyethylene wax or oxidized polyethylene wax; suitable antioxidants include a composite antioxidant system composed of any one or more of hindered phenol antioxidants, phosphite antioxidants or organic sulfur antioxidants, preferably a compound of antioxidant 1010 and antioxidant 168, with the compound mass ratio of the two being 1: (1-5).
[0024] The present invention also provides a method for preparing the above-mentioned PBT composite material, comprising the following steps:
[0025] (1) The PBT resin is pre-dried at 120-140°C for 4-6 hours, and the dried PBT resin and other components except the alkali-free flat glass fiber are mixed evenly in a high-speed stirring mixer according to the proportion or fed separately into a pre-mixer through a metering feeder to obtain a mixture;
[0026] (2) The mixed material is fed into a twin-screw extruder, and alkali-free flat glass fiber is added by side feeding. Under the conveying and shearing action of the twin-screw extruder, the mixed material is fully melted and plasticized, kneaded and mixed, extruded through a die head, drawn, cooled, pelletized, and dried to prepare a PBT composite material; wherein the feed rate of the twin-screw extruder is 450-800 kg / hour; the temperatures of each section of the screw of the twin-screw extruder from the feed port to the die head are 220-230°C, 230-240°C, 230-240°C, 240-250°C, 250-260°C, 240-250°C, 240-250°C, 230-240°C, and 230-240°C, respectively; and the screw speed is 250-400 rpm.
[0027] The present invention also provides the application of the above PBT composite material in plastic-coated metal products in the electronic and electrical industry, which can be used in the fields of lighting or cooling fans.
[0028] The present invention has the following beneficial effects:
[0029] The PBT composite material of the present invention adopts alkali-free flat glass fiber reinforcement, adopts a diethyl aluminum hypophosphite-melamine polyphosphate flame retardant system, and adds a certain amount of phosphate ester, fatty acid salt and toughening agent. It can achieve flame retardancy reaching UL-94 standard 0.8mmV-0 level, and has high fluidity (melt flow rate ≥8.0g / 10min), high weld line strength (weld line bending strength ≥46.3MPa), and excellent cold and hot shock resistance (cyclically withstands cold and hot shocks of -40°C to 90°C for 50 times without cracking), meeting the use requirements in the electronic and electrical industry. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 Schematic diagram of plastic-wrapped metal samples subjected to thermal shock tests of the embodiments and comparative examples. Implementation
[0031] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several variations and improvements may be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.
[0032] The raw materials used in the embodiments and comparative examples of the present invention are described as follows, but are not limited to these materials:
[0033] PBT resin 1: Yizheng PBT GX110;
[0034] PBT resin 2: Yizheng PBT GX111;
[0035] PBT resin 3: Yizheng PBT GX112;
[0036] PBT resin 4: Yizheng PBT GX121;
[0037] Glass fiber 1: alkali-free flat glass fiber, TFG-3.0-T436, flatness ratio 1: (3.5-4.0), Taishan Glass Fiber Co., Ltd.;
[0038] Glass fiber 2: alkali-free flat glass fiber, ECS3F-03-534A, flatness ratio: 1: (3.0-3.5), Jushi Group;
[0039] Glass fiber 3: ordinary round glass fiber, ECS13-3.0-T436W, Taishan Glass Fiber Co., Ltd.;
[0040] Diethylaluminum hypophosphite: Exolit OP 1230, Clariant Chemicals;
[0041] Melamine polyphosphate 1: Melapur 200, BASF, pH value of saturated aqueous solution at 25°C is 6.5;
[0042] Melamine polyphosphate 2: BUDIT 341, Budenheim, pH value of saturated aqueous solution at 25°C is 5.0;
[0043] Melamine polyphosphate 3: BZ-FP20, Chongqing Baozhuan, pH value of saturated aqueous solution at 25°C is 4.5;
[0044] Phosphate ester 1: ADK STAB FP-600, ADK, bisphenol A bis(diphenyl phosphate);
[0045] Phosphate 2: WSFR-RDP, Wansheng, resorcinol bis(diphenyl phosphate);
[0046] Phosphate 3: WSFR-PX200, Daba Chemical, hydroquinone bis (diphenyl phosphate);
[0047] Fatty acid salt 1: LICOMONT CAV 102 P, Clariant, lignite fatty acid calcium salt;
[0048] Fatty acid salt 2: LICOMONT NAV 101, Clariant, lignite fatty acid sodium salt;
[0049] Toughener 1: Elvaloy AC 1125 resin, DuPont, ethylene-methyl acrylate copolymer;
[0050] Toughener 2: Elvaloy AC 34035, DuPont, ethylene-butyl acrylate copolymer;
[0051] Toughener 3: EVATANE 28-25, Arkema, ethylene-vinyl acetate copolymer;
[0052] Auxiliary agent 1: antioxidant 1010 and antioxidant 168, compounding ratio 1:3, commercially available; the same antioxidant is used in the parallel examples and comparative examples;
[0053] Auxiliary agent 2: Lubricant PETs, aliphatic carboxylic acid ester, commercially available; the same lubricant was used in the parallel examples and comparative examples.
[0054] Preparation methods of embodiments and comparative examples:
[0055] (1) The PBT resin is pre-dried at 130°C for 4-6 hours, and the moisture content is controlled to be less than 0.03%. The dried PBT resin and the other components except the alkali-free flat glass fiber are mixed in a high-speed stirring mixer according to the proportions in Table 1 to obtain a mixture;
[0056] (2) The mixed material is fed into a twin-screw extruder, and alkali-free flat glass fiber is added in proportion to the side feed. Under the conveying and shearing action of the twin-screw extruder, the mixed material is fully melted and plasticized, kneaded and mixed, extruded through a die head, drawn into strips, cooled, pelletized, and dried to prepare a PBT composite material; wherein the feed rate of the twin-screw extruder is 450-800 kg / hour; the temperatures of each section of the screw of the twin-screw extruder from the feed port to the die head are 230°C, 240°C, 240°C, 250°C, 260°C, 250°C, 240°C, 230°C, and 230°C, respectively; and the screw speed is 400 rpm.
[0057] Related performance test methods:
[0058] (1) Hot and cold shock test method: Use the hot and cold shock mold designed by Kingfa to inject plastic-coated metal samples (such as Figure 1 10 samples were placed in a hot and cold shock box for hot and cold shock tests. The test conditions were: kept at -40°C for 30 minutes, and then quickly heated to 90°C for 30 minutes, with 50 cycles. The cracking of the weld line of the samples was observed, and the cracking ratio was calculated.
[0059] (2) Weld line bending strength (MPa): The weld line mold independently designed by Kingfa Science & Technology Co., Ltd. is used. The mold shape is the same as the 1A specimen in standard ISO 527-2:2012. The weld line tensile specimen is obtained by injecting glue at both ends. The weld line bending strength is tested according to ISO 178:2019.
[0060] (3) Melt flow rate (g / 10 min): The product obtained by extrusion and pelletization was dried at 120 °C for 4 h and tested according to ISO1133-2011 standard, with a test temperature of 270 °C and a weight of 2.16 kg;
[0061] (4) Flame retardant performance: Injection molded 0.8 mm flame retardant specimens, tested according to UL94-2021 standard.
[0062] Table 1: Distribution ratios of each group in Examples 1-7 (by weight) and related performance test results
[0063]
[0064] Compared with Examples 1-3, the weight ratio of diethylaluminum hypophosphite to melamine polyphosphate in the present invention is preferably (5.5-9):1.
[0065] Comparing Example 1 with Example 4, it is preferred to use alkali-free flat glass fiber with a flatness ratio of 1: (3.5-4.0).
[0066] Comparing Example 1 with Example 5, it is preferred to use melamine polyphosphate having a saturated aqueous solution pH value of 5.5-6.5 at 25°C.
[0067] Table 2: Distribution ratios of each group in Examples 8-13 (by weight) and related performance test results
[0068]
[0069] Table 3: Distribution ratios of each group in comparative examples 1-8 (by weight) and related performance test results
[0070]
[0071] The PBT composite material of the present invention is reinforced with alkali-free flat glass fiber, adopts a diethyl aluminum hypophosphite-melamine polyphosphate flame retardant system, and simultaneously adds a certain amount of phosphate ester, fatty acid salt and toughening agent, so that the flame retardancy reaches the UL-94 standard 0.8mmV-0 level, and at the same time, has high fluidity (melt flow rate ≥8.0g / 10min), high weld line strength (weld line bending strength ≥46.3MPa), and excellent thermal shock resistance (cyclically withstands thermal shocks of -40°C to 90°C for 50 times without cracking).
Claims
1. A PBT composite material, characterized in that: By weight, it includes the following components: 38-53 parts of PBT resin; 27~33 parts of alkali-free flat glass fiber; 15-18 parts of diethyl aluminum hypophosphite; 2-5 parts of melamine polyphosphate; Phosphate 1-3 parts; 1-2 parts of fatty acid salt; 1-3 parts of toughening agent; The phosphate ester is selected from one or more of bisphenol A bis(diphenyl phosphate), resorcinol bis(diphenyl phosphate) or hydroquinone bis(diphenyl phosphate); The fatty acid salt is selected from lignite fatty acid salts; The toughening agent is selected from any one or more of ethylene-vinyl acetate copolymer, ethylene-methyl acrylate copolymer or ethylene-butyl acrylate copolymer; The pH value of the saturated aqueous solution of the melamine polyphosphate at 25° C. is 5-6.
5.
2. The PBT composite material according to claim 1, characterized in that: The flatness ratio of the alkali-free flat glass fiber is 1:(3-4).
3. The PBT composite material according to claim 2, characterized in that: The flatness ratio of the alkali-free flat glass fiber is 1:(3.5-4).
4. The PBT composite material according to claim 1, characterized in that: The weight ratio of the diethyl aluminum hypophosphite to melamine polyphosphate is (3-9):
1.
5. The PBT composite material according to claim 4, characterized in that: The weight ratio of the diethyl aluminum hypophosphite to melamine polyphosphate is (5.5-9):
1.
6. The PBT composite material according to claim 5, characterized in that: The pH value of the saturated aqueous solution of the melamine polyphosphate at 25° C. is 5.5-6.
5.
7. The PBT composite material according to claim 1, characterized in that: The lignite fatty acid salt is selected from any one or more of lignite fatty acid sodium salt or lignite fatty acid calcium salt.
8. The PBT composite material according to claim 1, characterized in that: By weight, the invention also includes 0-1 part of auxiliary agent; the auxiliary agent is selected from any one or more of antioxidants or lubricants.
9. The method for preparing the PBT composite material according to any one of claims 1 to 8, characterized in that: The following steps are involved: (1) The PBT resin is pre-dried at 120-140°C for 4-6 hours, and the dried PBT resin and other components except the alkali-free flat glass fiber are mixed evenly in a high-speed stirring mixer according to the proportion or fed separately into a pre-mixer through a metering feeder to obtain a mixture; (2) The mixed material is fed into a twin-screw extruder, and alkali-free flat glass fiber is added by side feeding. Under the conveying and shearing action of the twin-screw extruder, the mixed material is fully melted and plasticized, kneaded and mixed, extruded through a die head, drawn, cooled, pelletized, and dried to prepare a PBT composite material; wherein the feed rate of the twin-screw extruder is 450-800 kg / hour; the temperatures of each section of the screw of the twin-screw extruder from the feed port to the die head are 220-230°C, 230-240°C, 230-240°C, 240-250°C, 250-260°C, 240-250°C, 240-250°C, 230-240°C, and 230-240°C, respectively; and the screw speed is 250-400 rpm.
10. Use of the PBT composite material according to any one of claims 1 to 8 in plastic-coated metal products in the electronic and electrical industry.