A large-size, high-performance Al-Mg-Zn aluminum alloy round ingot and its casting method

By using semi-continuous casting methods and high-purity smelting processes in large-size ingots, combined with electromagnetic stirring and high-purity argon gas degassing, the problems of grain refinement and structural uniformity are solved, and the casting of high-performance aluminum alloys is achieved , significantly improving the strength and quality of the material.

CN116179905BActive Publication Date: 2024-10-18SHANDONG YANCON LIGHT ALLOY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211656622.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-22
Publication Date
2024-10-18
Estimated Expiration
2042-12-22

AI Technical Summary

Technical Problem

It is difficult to achieve grain refinement and structural uniformity in large-sized ingots with existing technology, leading to problems of casting defects and poor quality.

Method used

Using a semi-continuous casting method, adding Zn, Zr, Be and rare earth element Er, through high-purity smelting process and electromagnetic stirring casting, combining the ingredients of high-purity aluminum ingots, magnesium ingots and zinc ingots, using high-purity argon gas degassing and ceramic Filtration, control of melt temperature and cooling rate, and homogenization treatment to achieve fine graining process.

Benefits of technology

It significantly improves the strength and material properties of aluminum alloys, ensures the uniformity and fine-grained structure of the ingot, reduces coarse grains and casting defects, and improves the overall quality of the ingot.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116179905B_ABST
    Figure CN116179905B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of aluminum alloys, and in particular to a large-scale, high-performance Al-Mg-Zn aluminum alloy round ingot and a casting method thereof. The casting method comprises the following steps: feeding; smelting: smelting at a temperature of 700-760°C, and the smelting time is within 5 hours; refining the aluminum alloy liquid; casting: adopting a hot top casting method, and installing an electromagnetic coil on the hot top tooling to achieve an electromagnetic stirring casting effect; homogenization: the first stage of homogenization is to keep the ingot at a furnace gas temperature of 41045°C for 8 hours, and the heating time is 5 hours; the second stage is to keep the ingot at a furnace gas temperature of 51045°C for 20 hours, and the heating time is 2.5. The present invention takes the traditional 5A06 alloy as the design prototype, adds Zn, Zr, Be and rare earth element Er, and obtains a high-performance high-purity ingot through a high-purity smelting process, a high-purity ingot casting fine crystal process, and a high-purity ingot homogenization process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aluminum alloys, and in particular to a large-size and high-performance Al-Mg-Zn aluminum alloy round ingot and a casting method thereof. Background Art

[0002] Al-Mg-Zn alloy has the characteristics of low density, high specific strength, good plasticity, and easy forming. It has broad application prospects and irreplaceable status in aerospace, shipbuilding, nuclear industry and weapons industry. Therefore, aluminum alloy technology is listed as a key technology of national defense science and technology and a basic technology for key development. With the technological development in the fields of rail transportation, aerospace and shipbuilding, higher requirements are put forward for the performance of Al-Mg-Zn alloy. A technical difficulty in the preparation of large aluminum alloy structural parts is the semi-continuous casting of large-sized ingots of high-alloyed aluminum alloy.

[0003] As the size of the ingot increases, the following control difficulties will arise: due to the difference in cooling rate and diffusion rate of alloy elements, the uniformity of chemical composition in various parts of the ingot is reduced for super-large diameter ingots. Due to the large ingot diameter and the limitations of cooling rate, it is difficult to achieve uniform and fine grain structure when the amount of grain refiner added is constant.

[0004] How to cast large homogeneous, high-purity, fine-grained ingots is the premise and basis for the preparation of high-performance aluminum materials. The methods to improve material performance are mainly achieved by adjusting alloy composition, purifying aluminum liquid purity, high supercooling fine-grain casting, etc. At present, large-scale ingots of high-performance aluminum alloys are generally prepared by semi-continuous direct water-cooling casting. Usually there are problems such as coarse grains, uneven structure, obvious casting defects, and poor ingot quality. Summary of the invention

[0005] Aiming at the technical problems of large-scale ingots of high-performance aluminum alloys, such as coarse grains, uneven structure, obvious casting defects, and poor ingot quality, the present invention provides a large-scale, high-performance Al-Mg-Zn aluminum alloy round ingot and a casting method thereof. The traditional 5A06 alloy is used as the design prototype, Zn, Zr, Be and rare earth element Er are added, and semi-continuous casting method is adopted for melting and casting. High-purity low-iron aluminum ingots, high-purity magnesium ingots, high-purity zinc ingots, AlMn alloys, AlEr alloys, AlTi5 alloys, AlZr alloys, and AlBe alloys are selected for batching. Through high-purity melting process, large-scale high-purity ingot casting fine crystal process, and large-scale high-purity ingot homogenization process, high-performance high-purity ingots are obtained.

[0006] In a first aspect, the present invention provides a casting method for a large-size high-performance Al-Mg-Zn aluminum alloy round ingot, wherein the element composition of the aluminum alloy round ingot is Si≤0.15%, Fe≤0.15%, Cu≤0.10%, Mn0.5%-0.9%, Mg 5.3%-6.0%, Cr≤0.05%, Zn 0.5%-1.2%, Ti 0.02%-0.05%, Be0.0005%-0.001%, Zr 0.09%-0.2%, Er 0.06%-0.1%, Na≤0.0005%, Ca≤0.0005%, a single impurity content ≤0.05%, a total impurity ≤0.15%, and the balance is Al;

[0007] The casting method comprises the following steps:

[0008] (1) Feeding: Recycled materials, aluminum ingots, master alloys of Mn, Be, Zr, and Er elements (such as AlMn10, AlBe5, AlZr3, AlEr5, etc.) are loaded into the furnace in the order of charge. AlTi alloy, Zn, and Mg are added before sampling and stirring of the smelting furnace;

[0009] (2) Melting: The melting temperature is 700-760℃, and the melting time is within 5 hours. After the charge collapses, the sodium-free covering agent is evenly spread to cover it completely. After all the charge is melted into aluminum alloy liquid, the aluminum alloy liquid is refined by a rotor refining car. Before loading and conducting the furnace, C2Cl6 mixed refining agent is sprinkled into the furnace. The amount of refining agent in the furnace is 7-9kg / ton of aluminum. After the aluminum alloy liquid in the melting furnace is refined, the sodium-free covering agent is sprinkled to cover it completely and adjust the temperature to 750-760℃, ready to be transferred to the static furnace;

[0010] (3) Casting: The hot top casting method is adopted, and an electromagnetic coil is installed on the hot top tooling. The electromagnetic field generated by the electromagnetic coil is used as an external field to assist in achieving the electromagnetic stirring casting effect. The casting speed is controlled at 15-20 mm / min and the cooling water flow rate is 45-50 m 3 / h, cooling water temperature is 24-28℃, Al-Ti-B grain refiner is used to refine grains, the speed of the grain refiner wire rod is controlled to 70-80rpm, the temperature of the static furnace aluminum liquid is controlled to 745-755℃, and the platform aluminum liquid temperature during the casting process is 695-705℃, the fluidity of the melt is improved to ensure the casting undercooling, and the grain size is refined to the greatest extent on the basis of ensuring the ingot molding;

[0011] (4) Homogenization: Homogenization includes two stages. The first stage is to keep the ingot at a furnace temperature of 41045°C for 8 hours. When the ingot is loaded into the furnace, the furnace temperature is >250°C and the heating time is 5 hours. The second stage is to keep the ingot at a furnace temperature of 51045°C for 20 hours. The heating time is 2.5 hours. After homogenization, the ingot is taken out of the furnace and naturally cooled to room temperature.

[0012] Furthermore, step (1) is as follows: after the furnace temperature is higher than 600° C., recycled materials, aluminum ingots, and intermediate alloys of Mn, Be, Zr, and Er elements are loaded into the furnace in the order of recycled materials, AlTi alloy, Zn, and Mg are added before sampling and stirring in the smelting furnace. The recycled materials used are first-class recycled materials, i.e., castings that are not scrapped due to impurity content exceeding the standard, are free of oil stains, and can be directly used for batching without remelting. The amount of recycled materials used is generally not more than 80%, and the mass ratio of recycled materials to the total feed amount is ≤40%; the aluminum ingot is a high-purity aluminum ingot with a purity of 99.80% or more; the Zn element is added in the form of a high-purity zinc ingot with a purity of 99.95% or more, and the Mg element is added in the form of a high-purity magnesium ingot with a purity of 99.95% or more.

[0013] Furthermore, after all the charge in step (2) is melted, the melt temperature is measured once every hour to ensure that the melt temperature is within the required range, and overheating is strictly prohibited. Because the melting temperature is high, especially in the liquid state, if the residence time of the melt is too long, it will not only increase the air absorption of the melt and increase the oxidation and burning loss, but also reduce the non-spontaneous crystal nuclei, and increase the tendency of the ingot to generate cracks, slag inclusions, and coarse crystals.

[0014] Furthermore, in step (2), a permeable brick is provided at the bottom of the static furnace, and 99.999% high-purity argon gas is blown upward through the permeable brick for 40 minutes. Free hydrogen will diffuse into the bubbles of the inert gas, and in the process of the high-purity inert gas rising, fine inclusions adsorbed on the surface can be brought out of the aluminum liquid, thereby achieving the purpose of slag removal.

[0015] Furthermore, before casting in step (3), the melt is degassed online in a degassing box, the degassing box is provided with a graphite rotor with blowing holes, and argon is introduced into the degassing box while the graphite rotor is stirring; then the melt is filtered online through a ceramic filter plate.

[0016] Furthermore, the online degassing uses 99.999% high-purity argon, controls the argon flow rate to 45L / min / rotor, the rotor speed to 450rpm, and the melt temperature in the degassing box to 720-740℃. The degassing efficiency is related to the argon gas volume, specific surface area and melt temperature, the original hydrogen content of the melt and the ambient humidity. In order to achieve a good degassing effect, the amount of argon introduced must be increased first to increase the specific surface area of ​​argon; secondly, the diameter of the bubble must be as small as possible, the time for the bubble to float up must be extended, and the diffusion must be as complete as possible. The reduction of the bubble diameter is mainly achieved by increasing the rotor speed, but too high a speed will reduce the service life of the shaft; finally, the melt must be kept at a suitable temperature, the fluidity of the melt must be maintained, and the inert bubbles can smoothly reach the surface of the melt. At the same time, the occurrence of severe hydrogen absorption of the melt caused by excessive temperature must be avoided. After online degassing, the hydrogen content can be reduced to below 0.10mL / 100g aluminum, thereby avoiding the tendency to loosen.

[0017] Furthermore, the online filtration adopts two-stage filtration, the first-stage filtration adopts a ceramic filter plate with a through-hole size of 40ppi, and the second-stage filtration adopts a ceramic filter plate with a through-hole size of 60ppi. The ceramic filter plate has corrosion resistance to molten metal, excellent high-temperature mechanical properties, and good thermal shock resistance.

[0018] Furthermore, during the casting in step (3), the current intensity of the alternating current in the electromagnetic coil is 8-15A and the frequency is 20-25Hz.

[0019] In a second aspect, the present invention provides an aluminum alloy round ingot produced by the above-mentioned casting method, and the aluminum alloy round ingot can be used as a material for rail transportation.

[0020] Furthermore, the diameter of the aluminum alloy round ingot is 816 mm.

[0021] The beneficial effects of the present invention are:

[0022] The invention adds Er and Zr elements to the aluminum alloy, and can significantly improve the strength of the alloy through composite microalloying.

[0023] Through the coordination of the feeding structure, the proportion of recycled materials, the quality control of the intermediate alloy, the mixed refining and purification process of high-purity argon and special refining agents, and the furnace bottom degassing process, the free hydrogen will diffuse into the argon bubbles, and in the process of the high-purity argon rising, the tiny inclusions adsorbed on the surface can be brought out of the aluminum liquid, so that the degassing and slag removal effect of the melt in the furnace is optimal, and the purity of the melt in the furnace is maximized.

[0024] The hot top casting method is adopted. The function of the hot top part is to keep the melt warm and keep a liquid column on the top of the ingot at all times, maintain a certain static pressure of the aluminum liquid, and reduce the solidification position of the melt in the crystallizer. The height of the cooling part is very small, usually only 15-40mm. Its function is to make the effective crystallization area of ​​the hot top crystallizer for ingot forming very small, effectively preventing the secondary remelting of the solidified shell, thereby inhibiting the formation of segregation nodules on the inner and outer surfaces. Under the premise of hot top casting, an electromagnetic coil is added. The electromagnetic field generated by the alternating current (current intensity 8-15A, frequency 20-25Hz) in the induction coil during the electromagnetic casting process is used as an external field auxiliary to obtain a better electromagnetic stirring casting effect, achieve the same level of flow supply, temperature field balance, increase the cooling rate of the ingot, make the intracrystalline structure of the ingot thinner, and then cooperate with the online refinement process to solve the problem of crack formation and coarse grains in large-sized ingots.

[0025] The present invention improves casting defects such as component segregation through homogenization treatment, eliminates network and block coarse phases, ensures uniform distribution of dispersed phases in the crystal, and improves the performance of ingot alloy; trace elements such as Er and Zr can form dispersed ErAl3 and ZrAl3 particles in the matrix, and these particles can also play a role in pinning dislocations during the homogenization process, significantly inhibiting grain coarsening. In the first stage of homogenization, ZrAl3 particles are uniformly pre-nucleated in the high-concentration area in the crystal, and do not grow too fast, making them dispersed and fine; at the same time, part of the low-melting point eutectic phase is dissolved; in the second stage, the high-melting point impurity phase is transformed and diffused, reducing its adverse effects, thereby improving the comprehensive performance of the material; then it naturally drops to room temperature to obtain a large-scale, high-purity, fine-grained, homogeneous round cast rod that has been homogenized. The final verification result: the degree of homogenization of the ingot is the best, and no burning is seen. The dendrite network at the edge of the ingot is discontinuous, and most of the continuous dendrite network structure in the center and at 1 / 2 radius has been dissolved. It is in the form of thin lines, and small open particles of β phase (Mg5AI6) and other phases are precipitated from the matrix. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0027] Figure 1 This is a high-magnification microstructure photograph of the aluminum alloy round ingot prepared in Example 1.

[0028] Figure 2 This is a high-magnification microstructure photograph of the aluminum alloy round ingot prepared in Comparative Example 1.

[0029] Figure 3 This is a high-magnification microstructure photograph of the aluminum alloy round ingot prepared in Comparative Example 2.

[0030] Figure 4 This is a high-magnification microstructure photograph of the aluminum alloy round ingot prepared in Comparative Example 3. DETAILED DESCRIPTION

[0031] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0032] A method for casting a large-scale, high-performance Al-Mg-Zn corrosion-resistant aluminum alloy round ingot for rail transportation comprises the following steps:

[0033] (1) Charge: Charge by self-charging solid materials. Before charging, make sure that the charge is clean and dry, without any mixture, and weigh it. When charging, the furnace temperature must be higher than 600℃. Charge the furnace in the order of primary recycled materials, aluminum ingots, and intermediate alloys (AlMn10, AlBe5, AlZr3, AlEr5, etc.) accounting for 95% of the weight of the loaded aluminum ingots. AlTi alloy (AlTi5, AlTi3B1, etc.) and 99.95% high-purity zinc ingots and 99.95% high-purity magnesium ingots are added before sampling and stirring the smelting furnace. According to the form of primary recycled materials, small pieces or thin sheets of recycled materials are loaded first, followed by large pieces such as rod heads. Strictly control the proportion of primary recycled materials, and the mass ratio of the primary recycled materials loaded to the total charge is ≤40%. Alloys such as AlMn10, AlTi5, AlTi3B1, AlBe5, AlZr3, and AlEr5 require uniform high-magnification structure and dense fine fracture structure. No obvious metal particle aggregates or unmelted materials that affect use are allowed. There should be no slag, pores, or defects.

[0034] The microstructure requirements for the three master alloys AlTi5, AlTi3B1 and AlEr5 are shown in Table 1 below.

[0035] Table 1 Microstructure requirements of master alloys

[0036]

[0037] (2) Melting: Ensure that the melting and holding furnace, launder and tools are clean. The magnesium frame, stirring rake, slag rake, refining tube and other tools that come into contact with the aluminum liquid should be thoroughly cleaned before each use, and painted with ZYP boron nitride to ensure that the purity of the metal is not polluted. Ensure that the raw materials, melting and holding furnace, launder and tools used for alloy smelting are clean. There should be no cracks in the launder lining, no aluminum infiltration, no depressions and cracks in the lining joints, and the joints should be flat and smooth; use a rag to clean the peeling or excess boron nitride on the launder surface and polish it; use aluminum silicate felt to seal the launder at the casting platform interface, and replace it after each casting. Clean the coating of the crystallizer adapter plate and the surface of the graphite ring after each casting. Before each batch of production, the boron nitride coating is thoroughly polished off with a special brush. Excess boron nitride on the platform iron block, adapter plate, etc. must be cleaned up. After the platform is repaired, baked and polished, it is sprayed with boron nitride. The cracks and joints of the adapter plate are filled and evenly spread with concentrated boron nitride; the casting platform is evenly sprayed with boron nitride. Finally, the inner wall of the diverter plate is gently wiped with a special tool, polished, and the powder is cleaned with a vacuum cleaner.

[0038] Use high temperature smelting below 700-760℃, and the smelting time is within 5h. After the charge collapses, evenly spread the sodium-free covering agent to fully cover it. After all the charge is melted, measure the melt temperature once every hour to ensure that the melt temperature is within the required range. Overheating is strictly prohibited.

[0039] After all the charges are melted into aluminum alloy liquid, the alloy liquid is refined with a rotor refining car. Before loading and conducting the furnace, C2Cl6 mixed refining agent is sprinkled into the furnace. The amount of refining agent in the furnace is 7-9kg / ton of aluminum. After refining in the furnace, 15kg of sodium-free covering agent is sprinkled in to cover it thoroughly and adjust to 750-760℃ to prepare for transfer to the static furnace. The bottom of the static furnace is equipped with air-permeable bricks, and 99.999% high-purity argon gas is blown from bottom to top through the air-permeable bricks for 40 minutes.

[0040] After the melt is purified in the furnace, it enters the subsequent online processing process and is degassed again in the degassing box. The degassing box is equipped with a graphite rotor with blowing holes. The graphite rotor introduces 99.999% high-purity argon into the degassing box while stirring. The argon flow rate is controlled to be 45L / min / rotor, the rotor speed is 450rpm, and the melt temperature in the degassing box is 720-740℃ to ensure that the online detected hydrogen content is reduced to below 0.10mL / 100g aluminum to reduce the loose tendency.

[0041] After online degassing, the melt is transferred to an online filtration device for online filtration. The online filtration device includes two-stage ceramic filter plates. The through-hole size of the first-stage ceramic filter plate is 40ppi, and the through-hole size of the second-stage ceramic filter plate is 60ppi.

[0042] (3) Casting:

[0043] ① Casting speed research: Increasing the casting speed will reduce the axial temperature gradient, increase the average crystallization speed of the ingot, thin the crystal wall, reduce the shrinkage resistance of the inner layer to the outer layer, refine the intracrystalline structure, and reduce the tendency of the ingot to produce cold cracks. Within a certain range, it will have a favorable effect on the mechanical properties of the ingot. However, with the increase of the casting speed, while increasing the lateral temperature gradient, the temperature distribution along the horizontal section becomes more uneven, the lateral tensile stress acting in the horizontal direction increases, and the tendency of the ingot to produce thermal cracks along the surface increases. The liquid cavity becomes deeper, the transition zone size becomes wider, the regional segregation intensifies, and the crystallization shrinkage feeding conditions deteriorate. When the casting speed is too fast, the inhomogeneity and looseness of the ingot's organization and composition increase, and the mechanical properties decrease; when the casting speed is too slow, the cooling intensity is large, the melt supply is insufficient, and it is very easy to form a cold shut. When the cold shut is serious, transverse cracks may occur at the cold shut.

[0044] ② Study on cooling intensity: As casting progresses, the melt temperature gradually increases, and the cooling intensity needs to be increased. If the casting speed is increased, the tendency to crack will increase, so the cooling water flow rate can only be increased. Increasing the cooling intensity will increase the crystallization rate of the ingot, refine the intracrystalline structure, reduce the size of the transition zone, increase the density of the ingot, and improve the average mechanical properties. But at the same time, the temperature gradient in the ingot increases, the shrinkage of various parts inside is not synchronized, and the tendency to crack increases. The tendency of cold shut on the surface of the ingot increases, and the tendency of surface tensile cracking decreases. Therefore, the cooling intensity must meet the requirements of preventing the ingot from cracking while eliminating the cold shut defects on the surface of the ingot.

[0045] ③ Casting temperature research: When aluminum alloy is cast, due to the long flow channel and large temperature drop, bright grains, slag inclusions and other defects are easy to be produced during the initial casting process. In order to improve the internal quality in the initial casting stage, a higher casting temperature is required. Increasing the casting temperature within a certain range can reduce the size of the suspended crystal area in the liquid cavity of the ingot, reduce the tendency to form primary crystal compounds, improve the exhaust and shrinkage conditions, improve the density of the ingot, improve the mechanical properties of the cast state, and reduce the tendency of cold shuts on the surface of the ingot and increase the tendency of cracks and scratches on the surface of the ingot. However, if the casting temperature is too high, the ingot grains will be coarse, the hot brittleness of the alloy will increase, the liquid cavity will deepen, the temperature gradient will increase, and the surface temperature of the ingot at the outlet of the crystallizer will be too high, resulting in too small a solidified shell thickness, thereby increasing the tendency of the ingot to crack. On the contrary, if the casting temperature is too low, it will not be conducive to the floating and escape of gas and oxide inclusions during the casting process and increase the primary crystals of compounds. If the casting temperature is too low, it will promote the formation of cold shuts on the surface of the ingot, resulting in uneven ingot structure and reduced mechanical properties. Therefore, the casting temperature should be increased as much as possible while preventing ingot cracking and surface cracking.

[0046] After comprehensive consideration, the hot top casting method is adopted. The function of the hot top part is to keep the melt warm and keep a liquid column on the top of the ingot, maintain a certain static pressure of the aluminum liquid, and reduce the solidification position of the melt in the crystallizer. The height of the cooling part is very small, usually only 15-40mm. Its function is to make the effective crystallization area of ​​the hot top crystallizer for ingot forming very small, effectively preventing the secondary remelting of the solidified shell, thereby inhibiting the formation of segregation nodules on the inner and outer surfaces. Under the premise of hot top casting, an electromagnetic coil is added. The electromagnetic field generated by the alternating current in the induction coil (current intensity 8-15A, frequency 20-25Hz) during the electromagnetic casting process is used as an external field auxiliary to obtain a better electromagnetic stirring casting effect, achieve the same level of flow supply, temperature field balance, and increase the cooling rate of the ingot, making the intracrystalline structure of the ingot thinner. Combined with the online refinement process, the problem of crack formation and coarse grains in large-sized ingots can be solved. The final casting speed is determined to be 15-20mm / min, and the cooling water flow rate is 45-50m 3 / h, cooling water temperature is 24-28℃, Al-Ti-B grain refiner is used to refine grains, the speed of the grain refiner wire rod is controlled to 70-80rpm, the temperature of the static furnace aluminum liquid is controlled to 745-755℃, and the platform aluminum liquid temperature during the casting process is 695-705℃, the fluidity of the melt is improved to ensure the casting undercooling, and the grain size is refined to the greatest extent on the basis of ensuring the ingot molding;

[0047] (4) Homogenization: Homogenization includes two stages. The first stage is to keep the ingot at a furnace temperature of 41045°C for 8 hours. When the ingot is loaded into the furnace, the furnace temperature is >250°C and the heating time is 5 hours. The second stage is to keep the ingot at a furnace temperature of 51045°C for 20 hours. The heating time is 2.5 hours. After homogenization, the ingot is taken out of the furnace and naturally cooled to room temperature.

[0048] According to the above casting method, an aluminum alloy round ingot with a diameter of 816 mm was prepared (Example 1), and three comparative examples were set up.

[0049] The element composition of the aluminum alloy round ingot of Example 1 satisfies the following range:

[0050] Si≤0.15%, Fe≤0.15%, Cu≤0.10%, Mn 0.5%-0.9%, Mg 5.3%-6.0%, Cr≤0.05%, Zn 0.5%-1.2%, Ti 0.02%-0.05%, Be 0.0005%-0.001%, Zr 0.09%-0.2%, Er0.06%-0.1%, Na≤0.0005%, Ca≤0.0005%, single impurity content ≤0.05%, total impurities ≤0.15%, the balance is Al;

[0051] The actual element composition of the aluminum alloy round ingot of Example 1 is:

[0052] Si 0.07213%, Fe 0.13869%, Cu 0.06014%, Mn 0.65756%, Mg 5.86962%, Cr0.00896%, Zn 0.57358%, Ti 0.04112%, Be 0.0007%, Zr 0.09268%, Er 0.0808%, Na0.0004%, Ca 0.00018%, the content of each impurity is ≤0.05%, the total impurities are ≤0.15%, and the balance is Al.

[0053] The element composition of the aluminum alloy round ingot of Comparative Example 1 satisfies the following range:

[0054] Si≤0.20%, Fe≤0.20%, Cu≤0.15%, Mn 0.4%-0.6%, Mg 4.5%-5.0%, Cr≤0.05%, Zn 0.2%-0.4%, Ti 0.02%-0.04%, Be 0.0001%-0.0003%, Zr 0.08%-0.1%, Er 0.05%-0.07%, Na≤0.01%, Ca≤0.01%, single impurity content ≤0.05%, total impurities ≤0.15%, the balance is Al.

[0055] The actual element composition of the aluminum alloy round ingot of Comparative Example 1 is:

[0056] Si 0.08354%, Fe 0.14561%, Cu 0.0803%, Mn 0.5324%, Mg 4.8243%, Cr0.00758%, Zn0.35241%, Ti 0.03561%, Be 0.00025%, Zr 0.09456%, Er 0.0681%, Na0.0006%, Ca 0.0008%, the content of each impurity is ≤0.05%, the total impurities are ≤0.15%, and the balance is Al.

[0057] The element composition of the aluminum alloy round ingot of Comparative Example 2 satisfies the following range:

[0058] Si≤0.20%, Fe≤0.20%, Cu≤0.15%, Mn 1.0%-1.1%, Mg 6.0%-6.2%, Cr≤0.05%, Zn 1.0%-1.5%, Ti≤0.05%, Be 0.001%-0.0015%, Zr 0.20%-0.30%, Er0.10%-0.15%, Na≤0.01%, Ca≤0.01%, single impurity content ≤0.05%, total impurities ≤0.15%, the balance is Al.

[0059] The actual element composition of the aluminum alloy round ingot of Comparative Example 2 is:

[0060] Si 0.0951%, Fe 0.13646%, Cu 0.0756%, Mn 1.0567%, Mg 6.1164%, Cr0.00659%, Zn1.3451%, Ti 0.02541%, Be 0.0013%, Zr 0.25127%, Er 0.13546%, Na0.0008%, Ca 0.0007%, the content of each impurity is ≤0.05%, the total impurities is ≤0.15%, and the balance is Al.

[0061] The element composition of the aluminum alloy round ingot of Comparative Example 3 satisfies the following range:

[0062] Si≤0.20%, Fe≤0.20%, Cu≤0.15%, Mn 1.5%-1.8%, Mg 6.2%-6.5%, Cr≤0.05%, Zn 1.5%-2.0%, Ti 0.04%-0.05%, Be 0.015%-0.0020%, Zr 0.20%-0.30%, Er 0.15%-0.20%, Na≤0.01%, Ca≤0.01%, single impurity content ≤0.05%, total impurities ≤0.15%, the balance is Al.

[0063] The actual element composition of the aluminum alloy round ingot of Comparative Example 3 is:

[0064] Si 0.07511%, Fe 0.14531%, Cu 0.0874%, Mn 1.6547%, Mg 6.4351%, Cr0.01354%, Zn1.8324%, Ti 0.04567%, Be 0.0018%, Zr 0.25417%, Er 0.18147%, Na0.0007%, Ca 0.0006%, the content of each impurity is ≤0.05%, the total impurities is ≤0.15%, and the balance is Al.

[0065] The feeding structure design and specific process parameters of Example 1 and Comparative Examples 1-3 are shown in Tables 2-5 below.

[0066] Table 2 Feeding structure design (unit: t)

[0067]

[0068] Table 3 Smelting process configuration

[0069]

[0070] Table 4 Casting process configuration

[0071]

[0072]

[0073] Table 5 Homogenization process configuration

[0074] project First stage heating time min First-level insulation temperature and time Secondary heating time min Secondary insulation temperature and time Example 1 300 41045℃4480min 150 51045℃41200min Comparative Example 1 300 41045℃4480min 150 54045℃41200min Comparative Example 2 300 35045℃4480min 150 48045℃41200min Comparative Example 3 180 32045℃41200min 150 45045℃41440min

[0075] The performance of the aluminum alloy round ingots obtained from Example 1 and Comparative Examples 1-3 was tested, and the results are shown in Tables 6 and 7 below.

[0076] Table 6 Performance test results 1

[0077]

[0078] Table 7 Performance test results 2

[0079] project Online measurement of hydrogen content Solid state hydrogen content measurement Hardness HB Unmelted phase area percentage Example 1 0.103 / 0.102 0.120 / 0.123 67 2.56 Comparative Example 1 0.141 / 0.147 0.134 / 0.137 71 2.65 Comparative Example 2 0.135 / 0.147 0.149 / 0.151 72 4.21 Comparative Example 3 0.121 / 0.132 0.147 / 0.146 69 4.56

[0080] By comparing Example 1 with Comparative Examples 1-3, it can be seen that Example 1 has the least unmelted phase and impurity phase, the smallest grains, and meets the requirements of large-scale ingot structure. Comparative Example 2 does not add electromagnetic coils to achieve external field assistance, and the grain size of large-scale cast rods is too large.

[0081] Although the present invention has been described in detail with reference to the accompanying drawings and in combination with the preferred embodiments, the present invention is not limited thereto. Without departing from the spirit and essence of the present invention, a person of ordinary skill in the art may make various equivalent modifications or substitutions to the embodiments of the present invention, and these modifications or substitutions shall be within the scope of the present invention. Any person of ordinary skill in the art may easily think of changes or substitutions within the technical scope disclosed by the present invention, and these shall be within the scope of protection of the present invention.

Claims

1. A method for casting a large-scale, high-performance Al-Mg-Zn aluminum alloy round ingot, characterized in that: The element composition of the Al-Mg-Zn aluminum alloy round ingot is Si≤0.15%, Fe≤0.15%, Cu≤0.10%, Mn 0.5%-0.9%, Mg 5.3%-6.0%, Cr≤0.05%, Zn 0.5%-1.2%, Ti 0.02%-0.05%, Be 0.0005%-0.001%, Zr0.09%-0.2%, Er 0.06%-0.1%, Na≤0.0005%, Ca≤0.0005%, the content of a single impurity is ≤0.05%, the total impurities are ≤0.15%, and the balance is Al; the casting method comprises the following steps: (1) Feeding; (2) Melting: The melting temperature is 700-760℃, and the melting time is within 5 hours. After the charge collapses, the sodium-free covering agent is evenly spread to cover it completely. After all the charge is melted into aluminum alloy liquid, the aluminum alloy liquid is refined by a rotor refining car. Before loading and guiding the furnace, C2Cl6 mixed refining agent is sprinkled into the furnace. The amount of refining agent in the furnace is 7-9kg / ton of aluminum. After the aluminum alloy liquid in the melting furnace is refined, the sodium-free covering agent is sprinkled to cover it completely and adjust the temperature to 750-760℃, ready to be transferred to the static furnace; (3) Casting: Use hot top casting method, install electromagnetic coil on the hot top tooling, control the casting speed to 15-20mm / min, and the cooling water flow rate to 45-50m 3 / h, cooling water temperature is 24-28℃, Al-Ti-B grain refiner is used to refine grains, the temperature of aluminum liquid in the static furnace is controlled at 745-755℃, and the temperature of aluminum liquid on the platform during casting is 695-705℃; (4) Homogenization: Homogenization includes two stages. The first stage is to keep the ingot at a furnace temperature of 410±5℃ for 8 hours. The furnace gas temperature is >250℃ when the ingot is loaded into the furnace, and the heating time is 5 hours. The second stage is to keep the ingot at a furnace temperature of 510±5℃ for 20 hours, and the heating time is 2.5 hours. After homogenization, the ingot is taken out of the furnace and naturally cooled to room temperature.

2. The casting method according to claim 1, characterized in that: Step (1) is to charge the furnace in the order of recycled material, aluminum ingot, and intermediate alloy of Mn, Be, Zr, and Er elements after the furnace temperature is higher than 600° C., and add AlTi alloy, Zn, and Mg before sampling and stirring the smelting furnace. The recycled material used is first-grade recycled material, and the mass ratio of recycled material to the total feed amount is ≤40%; the purity of the aluminum ingot is higher than 99.80%; the Zn element is added in the form of zinc ingot with a purity of higher than 99.95%, and the Mg element is added in the form of magnesium ingot with a purity of higher than 99.95%.

3. The casting method according to claim 1, characterized in that: In step (2), a permeable brick is provided at the bottom of the static furnace, and 99.999% high-purity argon gas is blown from bottom to top through the permeable brick for 40 minutes.

4. The casting method according to claim 1, characterized in that: In step (3), before casting, the melt is degassed online in a degassing box, wherein the degassing box is provided with a graphite rotor with air blowing holes, and argon gas is introduced into the degassing box while the graphite rotor is stirring; then the melt is filtered online through a ceramic filter plate.

5. The casting method according to claim 4, characterized in that: The online degassing uses 99.999% high-purity argon gas, the argon gas flow rate is controlled to be 45L / min / rotor, the rotor speed is 450rpm, and the melt temperature in the degassing box is 720-740℃.

6. The casting method according to claim 4, characterized in that: The online filtration adopts two-stage filtration. The first-stage filtration adopts a ceramic filter plate with a through-hole size of 40ppi, and the second-stage filtration adopts a ceramic filter plate with a through-hole size of 60ppi.

7. The casting method according to claim 1, characterized in that: During the casting of step (3), the current intensity of the alternating current in the electromagnetic coil is 8-15A and the frequency is 20-25Hz.

8. An aluminum alloy round ingot produced by the casting method according to any one of claims 1 to 7.

9. The aluminum alloy round ingot according to claim 8, characterized in that: The diameter of the aluminum alloy round ingot is 816 mm.

Citation Information

Patent Citations

  • High-strength corrosion-resistant AL-Mg alloy

    CN104195388A

  • Metal-Me gravity casting aluminum alloy material and preparation method thereof

    CN108467979A