Cold-rolled ultra-high strength steel with uniform coiling performance and production method

By optimizing the chemical composition and process parameters of ultra-high-strength steel, the problem of uneven performance of ultra-high-strength steel coils is solved, achieving high-efficiency, low-cost steel coil strength uniformity, and ensuring both tensile strength and production efficiency.

CN116200680BActive Publication Date: 2024-10-08武汉钢铁有限公司
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202310190078.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-02
Publication Date
2024-10-08
Estimated Expiration
2043-03-02

AI Technical Summary

Technical Problem

The existing production process of ultra-high-strength steel has the problem of performance non-uniformity, especially for steel types with high alloy content. The coil performance varies greatly, and the existing technology increases production costs and is low in efficiency, and cannot effectively improve the quality of the first and middle parts. , intensity uniformity of the tail.

Method used

By optimizing the chemical composition and process parameters, including controlling the contents of C, Mn, Si, Nb, Cr, and Ti, and using processes such as laminar cooling and continuous annealing, we ensure that the steel coils undergo sufficient phase transformation during the hot rolling process and are slowly cooled. and aging treatment to reduce the differences in structure and performance of the head, middle and tail, and achieve uniformity of steel coils.

Benefits of technology

On the premise of ensuring the tensile strength ≥780MPa, the strength difference between the head, middle and tail of the rolled steel coil is controlled within 40MPa, achieving uniform performance of the rolled steel coil without edge shielding, electromagnetic stirring, and edge heating, and reducing the Production costs and energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004105115190000081
    Figure BDA0004105115190000081
  • Figure BDA0004105115190000082
    Figure BDA0004105115190000082
  • Figure BDA0004105115190000091
    Figure BDA0004105115190000091
Patent Text Reader

Abstract

A cold-rolled ultra-high strength steel with uniform coiling performance, the chemical composition and wt% of which are: C: 0.070-0.14%, Mn: 1.80-2.40%, Als: 0.035-0.30%, Si: 0.10-0.80%, Nb: 0.005-0.050%, Cr: 0.25-0.65%, Ti: 0.005-0.060%, P: ≤0.015%, S: ≤0.004%, N: ≤0.003%; production method: conventional continuous casting after smelting; heating of the ingot; hot rolling; laminar cooling; coiling; cold rolling after conventional pickling; continuous annealing; slow cooling; rapid cooling; aging treatment; flattening. The invention controls the strength difference of the head, middle and tail of the coiled steel coil within 40MPa while ensuring the tensile strength ≥780MPa, and does not require edge shielding, electromagnetic stirring and edge heating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a cold-rolled steel for automobiles and a production method thereof, in particular to a cold-rolled ultra-high-strength steel with uniform coiling performance and a production method thereof. Background Art

[0002] In recent years, with the advancement of automobile energy conservation and emission reduction technology, automobile lightweighting has become a development trend. Ultra-high strength steel of 780MPa and above is one of the development directions of automobile lightweight materials. In the production process of ultra-high strength steel, more alloy elements such as Mn, Si, Nb, Cr are usually added, and due to the unevenness of the production process during the manufacturing process, the performance of the produced strip steel varies greatly.

[0003] Existing technical methods for increasing or improving the uniformity of the microstructure and performance of ultra-high strength steel include: 1) hood annealing of hot rolled coils; 2) coiling at 550-580°C to improve the uniformity of the microstructure and performance of hot rolled coils in the width direction; 3) controlling the composition fluctuation in molten steel to a narrower range; 4) reducing the amount of cooling water at the head and tail of the hot rolled coils, and using low temperature coiling for Nb-containing microalloyed steel to improve the uniformity of the performance of the strip. The following problems exist in the prior art: 1) hood annealing of hot rolled coils increases the production process and production cost, and reduces production efficiency; 2) some methods are only aimed at improving the uniformity of performance in the width direction; 3) controlling the composition fluctuation in molten steel can only reduce the performance fluctuation between different coils, and cannot improve the uniformity of the performance of the coiled steel; 4) the effect of reducing the amount of cooling water at the head and tail of hot rolling is weak, especially for steels with high alloy content, the effect is even smaller.

[0004] After searching:

[0005] The document with Chinese patent publication number CN 109576467A discloses a "Control Method for Improving the Uniformity of Coil Performance of Low-alloy High-strength Steel Containing Nb". Its technical measures are as follows: mainly using a low-temperature coiling process at 300-550°C to transplant the precipitation behavior of Nb carbonitrides during the cooling process of the steel coil during hot rolling, so that the Nb element is more solid-dissolved, and the statistical performance unevenness caused by the fluctuation of the precipitation behavior of the steel coil is avoided. This technology is mainly aimed at products with a tensile strength of less than 780MPa in the final product, which have a low alloy content. However, for products with high alloy content, especially high Mn content, low-temperature coiling causes high strength of hot-rolled products, poor plate shape, and difficulty in subsequent acid rolling. The document with Chinese patent publication number CN 113234906A discloses "A production method and high-strength steel for improving the uniformity of high-strength steel performance". Its technical measures include: appropriately lowering the coiling temperature to 550-580°C to reduce the temperature difference between the edge and the middle of the plate width, thereby reducing the difference in microstructure and performance in the plate width direction. Its main purpose is to improve the uniformity of microstructure and performance in the width direction of the steel coil, and does not involve technical measures for the uniformity of microstructure and performance of the steel coil through the coil.

[0006] The document with Chinese patent publication number CN 113025795A discloses "A method for improving the uniformity of cold-rolled high-strength steel structure", and its technical measures include: (1) reducing the fluctuation of molten steel composition, (2) compensating heating of the edge during hot rolling, and (3) hood annealing of the hot-rolled coil to improve the uniformity of the structure and performance of the steel coil in the length and width direction. The above scheme reduces the fluctuation of molten steel composition and has a significant effect on reducing the performance fluctuation of steel coils from different furnaces, but has no significant effect on the performance fluctuation of the head, middle and tail of a single coil; it is necessary to add edge compensating heating equipment during hot rolling, which increases investment; hood annealing increases production processes and production costs, resulting in reduced efficiency, while increasing energy consumption and emissions, which is not conducive to environmental protection. Summary of the invention

[0007] The present invention aims to overcome the shortcomings of the prior art and provide a cold-rolled ultra-high strength steel and a production method with uniform coiling performance, while ensuring that the tensile strength is ≥780MPa, the strength difference between the head, middle and tail of the coil is controlled within 40MPa, and there is no need to adopt edge shielding, electromagnetic stirring, and edge heating.

[0008] Measures to achieve the above objectives:

[0009] A cold-rolled ultra-high strength steel with uniform coiling performance, the components and weight percentage contents of which are: C: 0.070-0.14%, Mn: 1.80-2.40%, Als: 0.035-0.30%, Si: 0.10-0.80%, Nb: 0.005-0.050%, Cr: 0.25-0.65%, Ti: 0.005-0.060%, P: ≤0.015%, S: ≤0.004%, N: ≤0.003%, and the rest are Fe and unavoidable impurities.

[0010] Preferably, the weight percentage of Nb is 0.010-0.047%.

[0011] Preferably, the weight percentage content of Ti is 0.010-0.056%.

[0012] Preferably, the weight percentage content of Cr is 0.25-0.55%.

[0013] A method for producing cold-rolled ultra-high strength steel with uniform coiling performance, comprising the following steps:

[0014] 1) Conventional continuous casting after smelting, and RH and LF are used for refining during smelting;

[0015] 2) Heat the ingot and control the ingot outlet temperature to be between 1250 and 1280°C. The heating time is between 1250 and 1280°C.

[0016] Control within 40 to 60 minutes;

[0017] 3) Perform hot rolling, control the final rolling temperature at 860-900℃, and control the temperature difference between the head, middle and tail of the steel coil during final rolling.

[0018] ≤30℃;

[0019] 4) laminar cooling, during which: adopt the front-stage rapid water cooling method, stop water cooling when the bainite transformation temperature Bs is at any point in the range of Bs-20 to Bs-80°C; air cooling is performed after the strip stops water cooling and before coiling, and the air cooling time is ≥10s;

[0020] 5) Coil the coil, during which the cooling water is turned off;

[0021] 6) After conventional pickling, cold rolling is carried out, and the total reduction rate is controlled at 50-70%;

[0022] 7) Perform continuous annealing, control the annealing soaking temperature to be between 810 and 850° C., and the soaking time to be between 100 and 300 seconds;

[0023] 8) Slowly cool to 600-650°C;

[0024] 9) Rapid cooling, cooling to below Ms-20°C at a cooling rate of ≤50°C / s;

[0025] 10) Perform aging treatment, control the aging temperature at Ms-60~Ms-20℃, and the aging time at 400~

[0026] 700s;

[0027] 11) Leveling is carried out. Except for the head and tail, which are 50m each, the leveling elongation of the middle part is controlled at 0.40-1.20%. The leveling elongation within 50m of the head and tail is controlled to be less than the leveling elongation of the middle part, that is, the leveling elongation of the head and tail is controlled at 0.3-1.10%.

[0028] The bainite transformation temperature Bs is calculated according to the formula Bs=732-202C-85Mn+116Si-47Cr, wherein the values ​​of C, Mn, Si and Cr are all pure decimals.

[0029] Preferably, the annealing soaking time is between 145 and 300 seconds.

[0030] Preferably: Ms is calculated according to the formula Ms=439-346*C-38*Mn-12.1*Cr-11*Si, and the aging treatment time is 385-635s.

[0031] Preferably, the flattening elongation within 50 m of the head and tail is between 0.35% and 1.0%, and the elongation of the middle part is between 0.45% and 1.10%.

[0032] Functions and mechanisms of various raw materials and main processes in the present invention

[0033] C: Carbon plays a role in solid solution strengthening and improves the strength of steel, but high carbon content increases the sensitivity to the process, increases the difference in the organization of the coil, and reduces the uniformity of performance. Taking into account the strength and uniformity of performance, the C content in the steel is selected to be 0.070% to 0.14%.

[0034] Mn: Mn plays a role in solid solution strengthening in steel, improves strength, stabilizes austenite and promotes martensite formation. However, if the Mn content is too high, the phase transition temperature will be reduced, the austenite phase transition rate will be slowed down, and it will be difficult to completely transform before coiling. Taking all factors into consideration, the Mn content of the present invention is 1.80-2.40%.

[0035] Si: Si can improve the strength of steel, but Si will delay the transformation of pearlite and bainite, resulting in prolonged phase transformation time, making it difficult to achieve complete phase transformation before coiling, and ultimately resulting in large differences in head, middle and tail performance. Considering the effects of performance and phase transformation, the Si content in the present invention is 0.10-0.80%.

[0036] Al: Al expands the phase change range, reduces process sensitivity, is conducive to obtaining the same structure at the head, middle and tail of the steel coil, increases structural uniformity, and reduces performance differences, but adding too much Al increases the cost of steel. Therefore, the Al content in the present invention is 0.035-0.30%.

[0037] S: S is an impurity element in steel, which is easy to combine with Al in steel to form AlS, and serves as a particle for the nucleation of subsequent precipitates, inducing uneven precipitation of Nb and Ti. However, when the S content is too low, the production cost increases, so based on cost and performance control considerations, it should be controlled at ≤0.004%.

[0038] N: N is an impurity element in steel. It is easy to form nitride particles with Al, Nb, Ti, etc. in steel, and precipitate with Al and Ti in steel in molten steel to form AlN and TiN. These may become nucleation points for subsequent precipitates, causing uneven precipitation. Therefore, its content is reduced as much as possible. However, if the N content is controlled too low, the production cost needs to be increased. Considering the comprehensive performance and cost, N should be controlled below 0.003%.

[0039] Cr: Cr can promote the formation of B in steel at a certain coiling temperature, avoid the pearlite region with a long phase transformation time, and facilitate the phase transformation before coiling. Therefore, the Cr content in the present invention is 0.25-0.65%. Preferably, the weight percentage of Cr is 0.25-0.55%.

[0040] Nb: During the continuous annealing and soaking process, Nb will significantly hinder the recovery and recrystallization of ferrite grains, and precipitate NbC and other precipitates, affecting the uniformity of the strip structure and performance. Therefore, from the perspective of improving product uniformity, the lower the Nb content in the steel, the better. However, considering Nb and significantly improving the strength of the product, the Nb content in the present invention is 0.005-0.050%; preferably, the weight percentage of Nb is 0.010-0.047%.

[0041] Ti: Ti plays a similar role to Nb in steel, and can play a role in precipitation strengthening, but the precipitation of Ti is more affected by temperature. Considering the improvement of performance and uniformity, the content of Ti in the present invention is 0.010-0.060%. Preferably, the weight percentage of Ti is 0.010-0.056%.

[0042] The main process reasons in the present invention are described as follows:

[0043] Through research, it is found that one reason for the uneven performance of steel coils is the uneven organization during hot rolling, which is mainly reflected in the fact that the head and tail of the hot-rolled steel coils are bainite organizations, while the middle of the steel coil is coarse ferrite + pearlite organization. The difference in organization is caused by the fact that the steel coils do not undergo sufficient phase transformation before coiling. After coiling, the head and tail of the steel coils are cooled quickly while the middle is cooled slowly, thus causing the organizational difference between the head, the middle and the tail. To solve this problem, the present invention minimizes the alloy element S that slows down the phase transformation while ensuring the performance when designing the product composition process. i, Mn, Cr, etc., to promote the hot-rolled coil to undergo sufficient phase transformation before coiling, thereby reducing the difference in the head, middle and tail structures; by controlling the hot rolling laminar cooling method, the steel coil can quickly enter the bainite phase transformation zone, and increase the phase transformation time in this zone, thereby improving the phase transformation incidence rate; when coiling, the coiling cooling water used to cool the coil is turned off to reduce overcooling of the steel coil, thereby further reducing the difference in the structure and performance between the head and the middle; by controlling the final rolling temperature difference of the head, middle and tail of hot rolling, the phase transformation uniformity and precipitation uniformity of the head, middle and tail can be further improved.

[0044] During the continuous annealing process, Nb and Ti hinder the recovery and recrystallization of ferrite in the organization, and due to the influence of nucleation particles and process fluctuations, the size and number of precipitates in the head, middle and tail are uneven. Therefore, by increasing the soaking temperature and increasing the soaking time, the full recrystallization and recovery of the head, middle and tail are promoted, and the Nb and Ti in the steel are fully precipitated, reducing the organizational and performance differences in the head, middle and tail. It has been found through research that a slow cooling rate, a longer aging time and a higher aging temperature can improve the uniformity of organizational properties of the head, middle and tail of the steel coil, but at the same time, in order to ensure strength, the present invention adopts a rapid cooling rate of ≤50℃ / s, a rapid cooling temperature of Ms-20℃, an aging temperature of Ms-60~Ms-20℃ and an aging time of 400~700s. Research has found that cold-rolled strip can significantly improve the strength of steel by flattening to increase dislocations in the steel. However, due to the difference in the structure of the head, middle and tail, the same flattening elongation will also cause differences in performance improvement in the head, middle and tail. Therefore, the present invention adopts a lower flattening elongation of 50m at the head and tail, thereby improving the uniformity of the product's structure and performance.

[0045] Compared with the prior art, the present invention controls the strength difference between the head, middle and tail of the through-roll steel coil within 40 MPa while ensuring the tensile strength is ≥780 MPa, and there is no need to adopt edge shielding, electromagnetic stirring and edge heating. DETAILED DESCRIPTION

[0046] The present invention is described in detail below:

[0047] Table 1 is a list of chemical components of various embodiments and comparative examples of the present invention;

[0048] Table 2 is a list of main process parameters of various embodiments and comparative examples of the present invention;

[0049] Table 3 is a table of performance test results of various embodiments of the present invention and comparative examples.

[0050] Each embodiment of the present invention is produced according to the following steps

[0051] 1) Conventional continuous casting after smelting, and RH and LF are used for refining during smelting;

[0052] 2) Heat the ingot and control the ingot outlet temperature to be between 1250 and 1280°C. The heating time is between 1250 and 1280°C.

[0053] Control within 40 to 60 minutes;

[0054] 3) Perform hot rolling, control the final rolling temperature at 860-900℃, and control the temperature difference between the head, middle and tail of the steel coil during final rolling.

[0055] ≤30℃;

[0056] 4) laminar cooling, during which: adopt the front-stage rapid water cooling method, stop water cooling when the bainite transformation temperature Bs is at any point in the range of Bs-20 to Bs-80°C; air cooling is performed after the strip stops water cooling and before coiling, and the air cooling time is ≥10s;

[0057] 5) Coil the coil, during which the cooling water is turned off;

[0058] 6) After conventional pickling, cold rolling is carried out, and the total reduction rate is controlled at 50-70%;

[0059] 7) Perform continuous annealing, control the annealing soaking temperature to be between 810 and 850° C., and the soaking time to be between 100 and 300 seconds;

[0060] 8) Slowly cool to 600-650°C;

[0061] 9) Rapid cooling, cooling to below Ms-20°C at a cooling rate of ≤50°C / s;

[0062] 10) Perform aging treatment, control the aging temperature at Ms-60~Ms-20℃, and the aging treatment time at 400~700s;

[0063] 11) Leveling is carried out. Except for the head and tail, which are 50m each, the leveling elongation of the middle part is controlled at 0.40-1.20%. The leveling elongation within 50m of the head and tail is controlled to be less than the leveling elongation of the middle part, that is, the leveling elongation of the head and tail is controlled at 0.3-1.10%.

[0064] Table 1 Chemical composition list of various embodiments and comparative examples of the present invention (wt%)

[0065]

[0066] Table 2 List of main process parameters of various embodiments of the present invention and comparative examples

[0067]

[0068]

[0069] Table 2

[0070]

[0071]

[0072] Table 3 List of mechanical properties test results of various embodiments of the present invention and comparative examples

[0073]

[0074] It can be seen from Table 3 that the differences in yield strength and tensile strength of the products of Examples 1 to 8 of the present invention at the head, middle and tail are all less than 40 MPa, and the head, middle and tail performance uniformity is good.

[0075] Description: Comparative Example 1 contains relatively high Si and Mn elements, relatively low Al content, and relatively high N content. Comparative Example 2 contains relatively high Nb and Ti elements. Comparative Example 3 contains relatively high C and Cr elements. In addition, the laminar cooling water cooling stop temperature of Comparative Example 1 is high, resulting in the middle of the steel coil being in the pearlite transformation zone, while the head and tail are in the bainite transformation zone. After coiling, the coiling cooling water of Comparative Example 3 is turned on, resulting in high cooling intensity at the head. The laminar cooling air cooling time of Comparative Example 3 is short. Therefore, there are large differences in the head, middle, and tail structures of the steel coils of Comparative Examples 1 to 3 after hot rolling, resulting in uneven performance of the finished products.

[0076] In comparative example 3-1, the cooling water of the coiling was turned on after hot rolling, resulting in high cooling intensity at the head, which ultimately led to uneven performance of the finished product.

[0077] In comparative example 4-1, the final product performance is uneven due to the difference in flattening elongation at the head, middle and tail.

[0078] In comparative example 5-1, the final performance of the product is uneven due to the low rapid cooling temperature and aging temperature.

[0079] This specific implementation is only the best example and is not a restrictive implementation of the technical solution of the present invention.

Claims

1. A cold-rolled ultra-high strength steel with uniform coiling performance, wherein the components and weight percentages thereof are: C: 0.125-0.14%, Mn: 1.80-2.40%, Als: 0.057-0.30%, Si: 0.55-0.80%, Nb: 0.005-0.035%, Cr: 0.47-0.65%, Ti: 0.005-0.034% or Ti: 0.056-0.060%, P: ≤0.015%, S: ≤0.004%, N: ≤0.003%, and the rest are Fe and unavoidable impurities; Production method: 1) Conventional continuous casting after smelting, and RH and LF are used for refining during smelting; 2) Heat the ingot and control the ingot outflow temperature between 1255 and 1280°C. The heating time is between 1255 and 1280°C. Control within 40 to 60 minutes; 3) Perform hot rolling, control the final rolling temperature at 860-876°C, and control the temperature difference between the head, middle and tail of the steel coil during the final rolling to be ≤30°C; 4) Perform laminar cooling, during which: adopt the front-stage rapid water cooling method, stop water cooling when the bainite transformation temperature Bs is at any point in the range of Bs-20~Bs-80℃; air cooling is performed after the strip stops water cooling and before coiling, and the air cooling time is ≥10s; 5) Coil the coils, during which the cooling water is turned off; 6) After conventional pickling, cold rolling is carried out, and the total reduction rate is controlled at 50-70%; 7) Perform continuous annealing, control the annealing soaking temperature at 825-850°C, and the soaking time at 212-300s; 8) Slowly cool to 600-650°C; 9) Rapid cooling, cooling to below Ms-20℃ at a cooling rate of ≤50℃ / s; 10) Perform aging treatment, control the aging temperature at Ms-60~Ms-20℃, and the aging treatment time at 400~700s; 11) For leveling, the leveling elongation of the middle part except the head and tail which are 50m each is controlled within 0.40~1.20%. The leveling elongation within 50m of the head and tail is controlled to be less than the leveling elongation of the middle part, that is, the leveling elongation of the head and tail is controlled within 0.3~1.10%.

2. A method for producing cold-rolled ultra-high strength steel with uniform coiling performance as claimed in claim 1, comprising the following steps: 1) Conventional continuous casting after smelting, and RH and LF are used for refining during smelting; 2) Heat the ingot and control the ingot outflow temperature between 1255 and 1280°C. The heating time is between 1255 and 1280°C. Control within 40 to 60 minutes; 3) Perform hot rolling, control the final rolling temperature at 860-876°C, and control the temperature difference between the head, middle and tail of the steel coil during the final rolling to be ≤30°C; 4) Perform laminar cooling, during which: adopt the front-stage rapid water cooling method, stop water cooling when the bainite transformation temperature Bs is at any point in the range of Bs-20~Bs-80℃; air cooling is performed after the strip stops water cooling and before coiling, and the air cooling time is ≥10s; 5) Coil the coils, during which the cooling water is turned off; 6) After conventional pickling, cold rolling is carried out, and the total reduction rate is controlled at 50-70%; 7) Perform continuous annealing, control the annealing soaking temperature at 825-850°C, and the soaking time at 212-300s; 8) Slowly cool to 600-650°C; 9) Rapid cooling, cooling to below Ms-20℃ at a cooling rate of ≤50℃ / s; 10) Perform aging treatment, control the aging temperature at Ms-60~Ms-20℃, and the aging treatment time at 400~700s; 11) For leveling, the leveling elongation of the middle part except the head and tail which are 50m each is controlled within 0.40~1.20%. The leveling elongation within 50m of the head and tail is controlled to be less than the leveling elongation of the middle part, that is, the leveling elongation of the head and tail is controlled within 0.3~1.10%.

3. The method for producing cold-rolled ultra-high strength steel with uniform coiling performance according to claim 2, characterized in that: The bainite transformation temperature Bs is calculated according to the formula Bs=732-202C-85Mn+116Si-47Cr, where the values ​​of C, Mn, Si, and Cr are all pure decimals.

4. The method for producing cold-rolled ultra-high strength steel with uniform coiling performance according to claim 2, characterized in that: Ms is calculated according to the formula Ms=439-346*C-38*Mn-12.1*Cr-11*Si, and the aging treatment time is 385~635s.

5. The method for producing cold-rolled ultra-high strength steel with uniform coiling performance according to claim 2, characterized in that: The flat elongation within 50m of the head and tail is between 0.35~1.0%, and the elongation in the middle part is between 0.45~1.10%.

Citation Information

Patent Citations

  • Control method for improving uniformity of coiling performance of Nb-containing low alloy high-strength steel

    CN109576467A

  • Method for improving structural uniformity of cold-rolled high-strength steel

    CN113025795A

  • Production method for improving performance uniformity of high-strength steel and high-strength steel

    CN113234906A

  • Method for manufacturing cold-rolled ultrahigh-strength dual-phase steel with high local forming performance

    CN105543674A

  • Method for producing steel for door industry and elevators based on ESP sheet endless rolling

    CN106282796A