A kind of water-based styrene acrylic JS waterproof emulsion and preparation method thereof
By using the alternating dripping process and the combination of emulsifiers in the preparation of water-based JS waterproof emulsion, the problem of high viscosity and difficulty in improving strength and elongation at the same time under high solid content was solved, and the preparation of highly efficient water-based styrene-acrylic JS waterproof emulsion was achieved. Meet building waterproofing performance requirements.
Patent Information
- Application Number
- CN202111458377.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-02
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-12-02
AI Technical Summary
When the solid content of the existing water-based JS waterproof emulsion is increased, the process viscosity is larger, and the elongation is difficult to increase at the same time when the strength is increased, resulting in high equipment requirements and limited performance optimization.
Using a special dripping process, pre-emulsion I and pre-emulsion II are alternately added dropwise in the reaction kettle, and the combination of emulsifier and oxidant is used to control the particle size distribution of the emulsion and the distribution of monomers, reduce the process viscosity and improve the mechanical strength. and elongation.
The preparation of water-based styrene-acrylic JS waterproof emulsion with high solid content is achieved. The process viscosity is reduced, the mechanical strength and elongation are simultaneously improved, and the performance is optimized to meet the waterproofing needs of buildings.
Smart Images

Figure BDA0003388736300000021 
Figure BDA0003388736300000041 
Figure BDA0003388736300000121
Abstract
Description
Technical Field
[0001] The invention relates to a building coating, in particular to a water-based styrene acrylic JS waterproof emulsion and a preparation method thereof. Background Art
[0002] JS waterproof emulsion is a polymer cement emulsion. It achieves the expected performance through the mixture of liquid and powder, and is widely used in building exterior walls, ground roof waterproofing. The liquid is mainly composed of emulsion, which provides elasticity, and the powder is mainly composed of cement and other inorganic materials, which provide strength. The interpenetrating network structure formed by the mixture of liquid and powder has good mechanical strength and elongation.
[0003] JS waterproof emulsion generally requires high solid content, but high solid content in the emulsion, especially high solid content in the process, will lead to high viscosity in the production process, high requirements for equipment, and high requirements for emulsion stability. And when optimizing the performance of the emulsion formula, the strength is often increased while the elongation is reduced at the same time.
[0004] CN106832106B discloses a high-solid-content, low-viscosity aqueous acrylic emulsion, which is prepared by a high-shear pre-emulsification and seed emulsion method. The large particle size obtained by this method has large fluctuations and the particle size does not have a multi-distribution characteristic.
[0005] CN101838371A discloses a method for preparing a high-solid-content, low-viscosity styrene-acrylic emulsion, which first prepares a large-particle emulsion seed, and then drips only monomers without dripping emulsifiers, so that all the added monomers enter the formed latex particles. However, it does not involve the simultaneous improvement of mechanical strength and elongation by the process. Summary of the invention
[0006] The present invention aims to provide a water-based styrene acrylic JS waterproof emulsion and a preparation method thereof. The method of the present invention ensures that the emulsion has a high solid content while reducing the process viscosity; the soft and hard monomers are alternately distributed, and the mechanical strength and mechanical elongation are simultaneously improved.
[0007] To achieve the above objectives, the present invention adopts the following technical solutions.
[0008] A water-based styrene acrylic JS waterproof emulsion, with a solid content of 55%-57%, a particle size of 200-400nm, and comprises the following components:
[0009]
[0010] A method for preparing a water-based styrene acrylic JS waterproof emulsion comprises the following steps:
[0011] (1) Add deionized water to the reaction kettle, raise the temperature to 80-90° C., and add the emulsifier solution at the bottom of the kettle;
[0012] (2) At 80-90° C., a portion of the pre-emulsion I and the first oxidant solution are added to the reactor for seeding. After 10-20 minutes, the second oxidant solution and the pre-emulsion I are added dropwise for 110-130 minutes;
[0013] (3) synchronously adding a portion of the pre-emulsion II to the remaining pre-emulsion I, and at the same time, continuing to drop the mixture into the reactor until the pre-emulsion I is completely added;
[0014] (4) Continue to dropwise add the remaining pre-emulsion II to the reactor for 20-40 min, and then keep warm for 0.5-1.5 hours;
[0015] (5) Cooling to 65-75° C., adding post-treatment oxidant and reductant solutions dropwise for 30-60 min, then cooling to 40-50° C., adding alkali solution for neutralization, adjusting the pH to 7.5-8.5, continuing to add optional additives, and filtering the material.
[0016] In step (1) of the present invention, the emulsifier of the kettle bottom emulsifier solution is one or more of tridecyl alcohol polyoxyethylene ether sulfate sodium salt, sodium dodecylbenzene sulfonate, allyl propylene oxide ether, and fatty alcohol polyoxyethylene ether, and the amount of the emulsifier is 3-8 parts by weight.
[0017] In step (2) of the present invention, the first oxidant is ammonium persulfate and / or sodium persulfate, and the amount used is 1-3 parts by mass.
[0018] In step (2) of the present invention, the second oxidant is ammonium persulfate and / or sodium persulfate, and the amount used is 1-3 parts by mass.
[0019] The dripping time of the second oxidant described in the present invention is from the beginning of step (2) to the end of step (4).
[0020] In step (3) of the present invention, it takes about 80-100 minutes to complete the dropwise addition of the pre-emulsion I, as determined when the liquid level of the mixture in the dropwise addition container is substantially zero.
[0021] In step (5) of the present invention, the post-treatment oxidant is 1-3 parts by mass, preferably tert-butyl hydroperoxide.
[0022] In step (5) of the present invention, the post-treatment reducing agent is 0.5-1.5 parts by weight, preferably ascorbic acid.
[0023] The pre-emulsion I of the present invention comprises the following components, calculated based on 100 parts of the total amount of the pre-emulsion I:
[0024]
[0025]
[0026] The preparation method of the pre-emulsion I comprises the following steps: adding deionized water, a first emulsifier, a hard monomer, a functional monomer, and a soft monomer into a pre-emulsification kettle 1, and stirring at a high speed for 20 minutes.
[0027] The pre-emulsion II of the present invention comprises the following components, calculated based on 100 parts of the total amount of the pre-emulsion II:
[0028] 65-85 parts by mass of hard monomer, preferably 70-80 parts by mass;
[0029] 1-6 parts by mass, preferably 2-5 parts by mass, of the second emulsifier;
[0030] 10-30 parts by mass of water, preferably 15-25 parts by mass.
[0031] The preparation method of the pre-emulsion II comprises the following steps: adding deionized water, a second emulsifier and a hard monomer into a pre-emulsification kettle 2, and stirring at a high speed for 10-30 minutes.
[0032] The hard monomer of the present invention comprises one or more of styrene, methyl methacrylate and butyl methacrylate.
[0033] The soft monomer of the present invention comprises isooctyl acrylate and / or butyl acrylate.
[0034] The functional monomers of the present invention include acrylamide and / or hydroxypropyl acrylate.
[0035] The emulsifier of the present invention comprises one or more of tridecyl alcohol polyoxyethylene ether sulfate sodium salt, sodium dodecylbenzene sulfonate, allyl propylene oxide ether and fatty alcohol polyoxyethylene ether.
[0036] The amount of a portion of the pre-emulsion I in step (2) of the present invention is 1-8% of the total amount of the pre-emulsion I, preferably 2%-7%.
[0037] The alkali solution described in the present invention is preferably a NaOH solution and / or a KOH solution.
[0038] The auxiliary agent of the present invention comprises one or more of a stabilizing dispersant, a defoaming agent and a preservative.
[0039] The defoaming agent of the present invention is preferably Evonik Degussa Tego-825 and / or Tego-1488.
[0040] The preservative of the present invention is preferably an isothiazolinone MIT preservative.
[0041] The stabilizing dispersant of the present invention is preferably a mixed solution of sodium polycarboxylate, preferably Nopco SN5040.
[0042] The key step in the present invention is a special pre-emulsion dripping process, wherein the pre-emulsion II contains a hard monomer, and the pre-emulsion II is dripped into the remaining pre-emulsion I when the pre-emulsion I is dripped for 110-130 minutes. On the one hand, the addition of an emulsifier in the pre-emulsion II increases the number of latex particles entering the reactor, broadens the particle size distribution, ensures a high solid content of the emulsion, and reduces the process viscosity. On the other hand, after the pre-emulsion I is dripped, the pre-emulsion II is continued to be dripped, wherein the addition of the hard monomer can copolymerize with the residual soft monomer in the reactor, so that the soft and hard monomers are alternately distributed, and the mechanical strength and elongation are increased at the same time. DETAILED DESCRIPTION
[0043] The present invention is further illustrated by the following examples. In the following examples, parts are by weight unless otherwise specified.
[0044] Table 1 Raw materials used to prepare the polymerization seed emulsion
[0045] Abbreviation Chemical Type BA Butyl acrylate ST Styrene HEA Hydroxyethyl acrylate SDBS Sodium dodecylbenzenesulfonate COPS-1 Allyl Propylene Oxide Ether SPS Sodium Persulfate T-BHP Tert-Butyl Hydroperoxide IAA Erythorbic Acid SN5040 Polycarboxylate sodium salt Tego825 Deco Defoamer NaOH (32%) Sodium hydroxide Kordek MLX DuPont preservative DIW Deionized water
[0046] Example 1: Waterproof emulsion 1-1
[0047] Preparation of pre-emulsion I: 109 parts of deionized water DIW, 14.2 parts of sodium dodecylbenzene sulfonate SDBS, 45 parts of styrene ST, 16 parts of hydroxyethyl acrylate HEA, and 395 parts of butyl acrylate BA are prepared in pre-emulsification kettle 1 and stirred thoroughly;
[0048] Preparation of pre-emulsion II: 25 parts of deionized water DIW, 5 parts of sodium dodecylbenzene sulfonate SDBS, 105 parts of styrene ST, prepared in pre-emulsification kettle 2 and stirred thoroughly;
[0049] Weigh 1.1 parts of sodium persulfate SPS and dissolve it in 6 parts of deionized water DIW to prepare a first oxidant solution; weigh 1.1 parts of sodium persulfate SPS and dissolve it in 35 parts of deionized water DIW to prepare a second oxidant solution;
[0050] Add 160 parts of deionized water to the reactor, heat to 80-85°C, and add 5.5 parts of allyl propylene oxide COPS-1. Transfer 5wt% of pre-emulsion I seeds from pre-emulsification kettle 1 to the reactor, and add the first oxidant solution. After 15 minutes of reaction, add pre-emulsion I and the second oxidant solution simultaneously, control the reaction temperature at 80-85°C, and when the addition is 120 minutes, add pre-emulsion II to pre-emulsification kettle 1 simultaneously until the liquid level of pre-emulsion kettle 1 is close to 0 at 210 minutes. Continue to add pre-emulsion II to the reactor, and after 30 minutes of addition, all pre-emulsion II and the second oxidant are dripped. After keeping the temperature for 30 minutes, the contents of the reactor were cooled to 60-65°C, and 1.43 parts of tert-butyl hydroperoxide TBHP dissolved in 10 parts of deionized water DIW and 0.83 parts of isoascorbic acid IAA dissolved in 10 parts of deionized water DIW were added dropwise for 30 minutes. The temperature was cooled to below 50°C, 4 parts of NaOH (provided in the form of a 32 wt% aqueous solution) were added for neutralization, and then 3.6 parts of SN5040, 0.5 parts of defoamer Tego-825 and 2.07 parts of preservative Kordek MLX were added. Waterproof emulsion 1-1 was obtained.
[0051] Example 2: Waterproof emulsion 1-2
[0052] Preparation of pre-emulsion I: 109 parts of deionized water DIW, 14.2 parts of sodium dodecylbenzene sulfonate SDBS, 75 parts of styrene ST, 16 parts of hydroxyethyl acrylate HEA, and 395 parts of butyl acrylate BA are prepared in pre-emulsification kettle 1 and stirred thoroughly;
[0053] Preparation of pre-emulsion II: 25 parts of deionized water DIW, 5 parts of sodium dodecylbenzene sulfonate SDBS, 75 parts of styrene ST, prepared in pre-emulsification kettle 2 and stirred thoroughly;
[0054] Weigh 1.1 parts of sodium persulfate SPS and dissolve it with 6 parts of deionized water DIW to prepare a first oxidant solution; weigh 1.1 parts of sodium persulfate SPS and dissolve it with 35 parts of deionized water DIW to prepare a second oxidant solution;
[0055] Add 160 parts of deionized water to the reactor, heat to 80-85°C, and add 5.5 parts of allyl propylene oxide COPS-1. Transfer 5wt% pre-emulsion seeds from pre-emulsification kettle 1 to the reactor, and add the first oxidant solution. After 15 minutes of reaction, simultaneously add pre-emulsion I and the second oxidant solution, control the reaction temperature at 80-85°C, and when the addition is 110 minutes, simultaneously add pre-emulsion II to pre-emulsification kettle 1 until the liquid level of pre-emulsion kettle 1 is close to 0 at 190 minutes. Continue to add pre-emulsion II to the reactor, and after 40 minutes of addition, all pre-emulsion II and the second oxidant are dripped. After keeping the temperature for 30 minutes, the contents in the reactor were cooled to 60-65°C, and 1.43 parts of tert-butyl hydroperoxide TBHP dissolved in 10 parts of deionized water DIW and 0.83 parts of isoascorbic acid IAA dissolved in 10 parts of deionized water DIW were added dropwise for 30 minutes. The temperature was cooled to below 50°C, 4 parts of NaOH (provided in the form of a 32 wt% aqueous solution) were added for neutralization, and then 3.6 parts of SN5040, 0.5 parts of defoamer Tego-825 and 2.07 parts of preservative Kordek MLX were added. Waterproof emulsion 1-2 was obtained.
[0056] Example 3: Waterproof Emulsion 1-3
[0057] Preparation of pre-emulsion I: 109 parts of deionized water DIW, 14.2 parts of sodium dodecylbenzene sulfonate SDBS, 30 parts of styrene ST, 16 parts of hydroxyethyl acrylate HEA, and 395 parts of butyl acrylate BA are prepared in pre-emulsification kettle 1 and stirred thoroughly;
[0058] Preparation of pre-emulsion II: 25 parts of deionized water DIW, 5 parts of sodium dodecylbenzene sulfonate SDBS, 120 parts of styrene ST, prepared in pre-emulsification kettle 2 and stirred thoroughly;
[0059] Weigh 1.1 parts of sodium persulfate SPS and dissolve it with 6 parts of deionized water DIW to prepare a first oxidant solution; weigh 1.1 parts of sodium persulfate SPS and dissolve it with 35 parts of deionized water DIW to prepare a second oxidant solution;
[0060] Add 160 parts of deionized water to the reactor, heat to 80-85°C, and add 5.5 parts of allyl propylene oxide COPS-1. Transfer 5wt% pre-emulsion seeds from pre-emulsification kettle 1 to the reactor and add the first oxidant solution. After 15 minutes of reaction, simultaneously add pre-emulsion I and the second oxidant solution, control the reaction temperature at 80-85°C, and when the addition is 130 minutes, simultaneously add pre-emulsion II to pre-emulsification kettle 1 until the liquid level of pre-emulsion kettle 1 is close to 0 at 230 minutes. Continue to add pre-emulsion II to the reactor, and after 20 minutes of addition, all pre-emulsion II and the second oxidant are dripped. After keeping the temperature for 30 minutes, the contents of the reactor were cooled to 60-65°C, and 1.43 parts of tert-butyl hydroperoxide TBHP dissolved in 10 parts of deionized water DIW and 0.83 parts of isoascorbic acid IAA dissolved in 10 parts of deionized water DIW were added dropwise for 30 minutes. The temperature was cooled to below 50°C, 4 parts of NaOH (provided in the form of a 32 wt% aqueous solution) were added for neutralization, and then 3.6 parts of SN5040, 0.5 parts of defoamer Tego-825 and 2.07 parts of preservative Kordek MLX were added. Waterproof emulsion 1-3 was obtained.
[0061] Comparative Example 1: Waterproof Emulsion 2-1
[0062] Preparation of pre-emulsion: 135 parts of deionized water DIW, 19.2 parts of sodium dodecylbenzene sulfonate SDBS, 150 parts of styrene ST, 16 parts of hydroxyethyl acrylate HEA, and 395 parts of butyl acrylate BA are prepared in pre-emulsification kettle 1 and stirred thoroughly;
[0063] Weigh 1.1 parts of sodium persulfate SPS and dissolve it in 6 parts of deionized water DIW to prepare a first oxidant solution; weigh 1.1 parts of sodium persulfate SPS and dissolve it in 35 parts of deionized water DIW to prepare a second oxidant solution;
[0064] Add 160 parts of deionized water to the reactor, heat to 80-85°C, and add 5.5 parts of allyl propylene oxide COPS-1. Transfer 5wt% pre-emulsion seeds from pre-emulsification reactor 1 to the reactor and add the first oxidant solution. After reacting for 15 minutes, add pre-emulsion I and the second oxidant simultaneously, and control the reaction temperature at 80-85°C. After 240 minutes of dripping, all the pre-emulsion and the second oxidant are dripped. After keeping warm for 30 minutes, the materials in the reactor are then cooled to 60-65°C, and 1.43 parts of tert-butyl hydroperoxide TBHP dissolved in 10 parts of deionized water DIW and 0.83 parts of isoascorbic acid IAA dissolved in 10 parts of deionized water DIW are dripped into the flask, and the dripping time is 30 minutes. The temperature was lowered to below 50° C., 4 parts of NaOH (provided in the form of a 32 wt % aqueous solution) were added for neutralization, and then 3.6 parts of SN5040, 0.5 parts of defoamer Tego-825 and 2.07 parts of preservative Kordek MLX were added to obtain waterproof emulsion 2-1.
[0065] Comparative Example 2: Waterproof Emulsion 2-2
[0066] Preparation of pre-emulsion I: 109 parts of deionized water DIW, 19.2 parts of sodium dodecylbenzene sulfonate SDBS, 45 parts of styrene ST, 16 parts of hydroxyethyl acrylate HEA, and 395 parts of butyl acrylate BA are prepared in pre-emulsification kettle 1 and stirred thoroughly;
[0067] Preparation of pre-emulsion II: 105 parts of styrene ST, prepared in pre-emulsification kettle 2;
[0068] Weigh 1.1 parts of sodium persulfate SPS and dissolve it with 6 parts of deionized water DIW to prepare a first oxidant solution; weigh 1.1 parts of sodium persulfate SPS and dissolve it with 35 parts of deionized water DIW to prepare a second oxidant solution;
[0069] Add 160 parts of deionized water to the reactor, heat to 80-85°C, and 5.5 parts of allyl propylene oxide COPS-1. Transfer 5wt% pre-emulsion seeds from pre-emulsification kettle 1 to the reactor and add the first oxidant solution. After 15 minutes of reaction, simultaneously add pre-emulsion I and the second oxidant, and control the reaction temperature at 80-85°C. After 120 minutes of dripping, simultaneously add pre-emulsion II to pre-emulsification kettle 1 until 220 minutes of dripping, when the addition of pre-emulsion I is finished. Continue to drip pre-emulsion II into the reactor, and after 20 minutes of dripping, all the pre-emulsion and the second oxidant are dripped. After keeping the temperature for 30 minutes, the contents of the reactor were cooled to 60-65°C, and 1.43 parts of tert-butyl hydroperoxide TBHP dissolved in 10 parts of deionized water DIW and 0.83 parts of isoascorbic acid IAA dissolved in 10 parts of deionized water DIW were added dropwise to the flask for 30 minutes. The temperature was lowered to below 50°C, 4 parts of NaOH (provided in the form of a 32 wt% aqueous solution) were added for neutralization, and then 0.5 parts of defoamer Tego-825 and 2.07 parts of preservative Kordek MLX were added. Waterproof emulsion 2-2 was obtained.
[0070] Comparative Example 3: Waterproof Emulsion 2-3
[0071] Preparation of pre-emulsion I: 109 parts of deionized water DIW, 14.2 parts of sodium dodecylbenzene sulfonate SDBS, 150 parts of styrene ST, 16 parts of hydroxyethyl acrylate HEA, and 395 parts of butyl acrylate BA are prepared in pre-emulsification kettle 1 and stirred thoroughly;
[0072] Preparation of pre-emulsion II: 25 parts of deionized water DIW and 5 parts of sodium dodecylbenzene sulfonate SDBS are prepared in pre-emulsification kettle 2 and stirred thoroughly;
[0073] Weigh 1.1 parts of sodium persulfate SPS, dissolve it in 6 parts of deionized water DIW to prepare a first oxidant solution; Weigh 1.1 parts of sodium persulfate SPS, dissolve it in 35 parts of deionized water DIW to prepare a second oxidant solution;
[0074] Add 160 parts of deionized water to the reactor, heat to 80-90°C, and add 5.5 parts of allyl propylene oxide COPS-1. Transfer 5wt% pre-emulsion seeds from pre-emulsification kettle 1 to the reactor and add the first oxidant solution. After 15 minutes of reaction, simultaneously add pre-emulsion I and the second oxidant, and control the reaction temperature at 80-85°C. After 120 minutes of dripping, simultaneously add pre-emulsion II to pre-emulsification kettle 1 until 210 minutes of dripping, when the addition of pre-emulsion I is finished. Continue to drip pre-emulsion II into the reactor, and after 30 minutes of dripping, all the pre-emulsion and the second oxidant are dripped. After keeping the temperature for 30 minutes, the contents of the reactor were cooled to 60-65°C, and 1.43 parts of tert-butyl hydroperoxide TBHP dissolved in 10 parts of deionized water DIW and 0.83 parts of isoascorbic acid IAA dissolved in 10 parts of deionized water DIW were added dropwise to the flask for 30 minutes. The temperature was cooled to below 50°C, 4 parts of NaOH (provided in the form of a 32 wt% aqueous solution) were added for neutralization, and then 0.5 parts of defoamer Tego-825 and 2.07 parts of preservative Kordek MLX were added. Waterproof emulsion 2-3 was obtained.
[0075] The emulsion prepared in the above example is mixed with water, defoamer, preservative, etc. to form the liquid part, and cement, quartz powder, heavy calcium, etc. are used to form the powder part. According to the formula in Table 2, the liquid and powder are mixed and stirred at high speed for 10 minutes. Take the mixed paint and scrape a 1mm film, scrape the second 2mm film 24 hours later, cure at room temperature for 96 hours, cure at 40℃ for 48 hours, and test after cooling.
[0076] Particle size: Malvern ZS90 particle size analyzer, polystyrene latex model, water as the dispersion medium General purpose analysis method.
[0077] Solid content: Weigh about 1.0g of the emulsion and place it on a 5cm diameter aluminum foil. Spread it evenly and place it in a 150°C oven for 20 minutes for determination.
[0078] Process viscosity: measured using Brookfield LV63#30r and 64#60r
[0079] Tensile strength: measured according to GB / T16777-2008 test method;
[0080] Elongation: Determined according to GB / T16777-2008 testing method.
[0081] Table 2 Waterproof coating test formula
[0082]
[0083] Table 3 Comparison of basic indicators of emulsion
[0084]
[0085] It can be seen from Table 3 that the emulsion prepared by this embodiment has a significantly reduced process viscosity, and the mechanical strength and elongation of the emulsion are 28% higher than those of the comparative example 2-1 which does not adopt this technology, and the strength is 0.2 MPa higher, thereby achieving simultaneous performance improvement.
[0086] Finally, it should be noted that the above waterproof emulsion embodiments are only used to describe the preferred embodiments of the present invention, rather than to limit the protection scope of the present invention. Although the present invention is described in detail with reference to the preferred embodiments, those skilled in the art should understand that various modifications and improvements made by modifying or equivalently replacing the technical solution of the present invention should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for preparing a water-based styrene acrylic JS waterproof emulsion, comprising the following steps: (1) Add deionized water to the reaction kettle, raise the temperature to 80-90° C., and add the emulsifier solution at the bottom of the kettle; (2) At 80-90° C., a portion of the pre-emulsion I and the first oxidant solution are added to the reactor for seeding. After 10-20 minutes, the second oxidant solution and the pre-emulsion I are added dropwise for 110-130 minutes; (3) synchronously adding a portion of the pre-emulsion II to the remaining pre-emulsion I, and at the same time, continuing to drop the mixture into the reactor until the pre-emulsion I is completely added; (4) Continue to dropwise add the remaining pre-emulsion II to the reactor for 20-40 min, and then keep warm for 0.5-1.5 hours; (5) cooling to 65-75° C., adding post-treatment oxidant and reductant solutions simultaneously, taking 30-60 min, then cooling to 40-50° C., adding alkali solution for neutralization, adjusting the pH to 7.5-8.5, continuing to add optional auxiliary agents, and filtering the material; The pre-emulsion I comprises the following composition, calculated based on 100 parts of the total amount of the pre-emulsion I: The pre-emulsion II comprises the following composition, calculated based on 100 parts of the total amount of the pre-emulsion II: 65-85 parts by mass of hard monomer; 1-6 parts by mass of the second emulsifier; 10-30 parts by mass of water.
2. The method according to claim 1, It is characterized in that The pre-emulsion I comprises the following composition, calculated based on 100 parts of the total amount of the pre-emulsion I:
3. The method according to claim 1, It is characterized in that The pre-emulsion II comprises the following composition, calculated based on 100 parts of the total amount of the pre-emulsion II: 70-80 parts by weight of hard monomer; 2-5 parts by weight of the second emulsifier; 15-25 parts by mass of water.
4. The method according to claim 1, It is characterized in that The amount of the pre-emulsion I in step (2) is 1-8% of the total amount of the pre-emulsion I.
5. The method according to claim 1, It is characterized in that The amount of a portion of the pre-emulsion I in the step (2) is 2%-7% of the total amount of the pre-emulsion I.
6. The method according to claim 1, It is characterized in that The water-based styrene acrylic JS waterproof emulsion has a solid content of 55%-57% and a particle size of 200-400nm, and comprises the following components:
7. The method according to claim 6, It is characterized in that The water-based styrene acrylic JS waterproof emulsion comprises the following components:
8. The method according to claim 1, It is characterized in that The hard monomer comprises one or more of styrene, methyl methacrylate, and butyl methacrylate.
9. The method according to claim 1, It is characterized in that The soft monomer comprises isooctyl acrylate and / or butyl acrylate.
10. The method according to claim 1, It is characterized in that The functional monomers include acrylamide and / or hydroxypropyl acrylate.
11. The method according to claim 1, It is characterized in that The emulsifier is one or more of tridecyl alcohol polyoxyethylene ether sulfate sodium salt, sodium dodecylbenzene sulfonate, allyl propylene oxide ether, and fatty alcohol polyoxyethylene ether.
Citation Information
Patent Citations
Method for preparing high-solid-content and low-viscosity core-shell structure styrene-acrylic emulsion
CN101838371A
A water-based polyacrylate emulsion and its preparation method
CN106832106B
Ammonia-free waterproof emulsion and preparation method thereof
CN112266439A