A positive electrode slurry, a positive electrode sheet, its preparation method and application

By forming a porous polymer coating layer on the cathode material substrate, the problem of the cathode material not being optimized in the electrode pore formation in the prior art is solved, which achieves the effect of alleviating crystal structure cracks and reducing resistance, and improves discharge capacity.

CN116230909BActive Publication Date: 2026-11-17ZHEJIANG HUAYOU COBALT CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310455149.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-24
Publication Date
2026-11-17
Estimated Expiration
2043-04-24

AI Technical Summary

Technical Problem

Existing electrode pore-forming technology increases ionic conductivity, but does not optimize the cathode material itself. It is difficult to resist the stress caused by volume changes during charging and discharging, which can easily lead to crystal structure cracks, and the cost is high.

Method used

A porous polymer coating layer is formed on a positive electrode material substrate. The positive electrode material and polymer are mixed in a solution system to form a polymer coating layer, and a pore-forming treatment is performed to form a porous structure. A binder and a conductive agent are then combined to prepare a positive electrode slurry.

Benefits of technology

It effectively alleviates crystal structure cracks, reduces resistance, increases discharge capacity, and reduces costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116230909B_ABST
    Figure CN116230909B_ABST
Patent Text Reader

Abstract

This invention discloses a positive electrode slurry, a positive electrode sheet, its preparation method, and its application, belonging to the field of battery technology. During the preparation of the positive electrode slurry, the positive electrode material substrate is modified to form a polymer coating layer with a porous structure. The modified positive electrode material with the porous polymer coating layer is mixed with a binder and a conductive agent to obtain the positive electrode slurry, which can resist the stress caused by volume changes during charging and discharging, effectively alleviate crystal structure cracks, or reduce resistance and increase discharge capacity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of battery technology, and more specifically, to a positive electrode slurry, a positive electrode sheet, a method for preparing the same, and its applications. Background Technology

[0002] Pore ​​formation during the coating process of positive electrode sheets is one of the effective means to reduce interfacial resistance and improve energy density and stability. The pores formed after pore formation can improve the compatibility of the electrode-electrolyte interface and enhance the ion transport capacity inside the electrode sheet. Most of the techniques for electrode pore formation disclosed in papers and patents involve adding a pore-forming agent to the electrode material slurry to prepare the electrode sheet, thereby forming pores in situ within the electrode sheet.

[0003] Most pore-forming methods use citric acid, ammonium bicarbonate, polyvinylpyrrolidone, urea, ammonium carbonate, or ketones as pore-forming agents, which require large quantities and are therefore costly.

[0004] More importantly, current electrode pore-forming technology still has the following problems: electrode pore-forming only increases the ionic conductivity of the electrode, without further optimizing the positive electrode material itself, making it difficult to resist the stress caused by volume changes during charging and discharging, and easily leading to crystal structure cracks.

[0005] In view of this, the present invention is proposed. Summary of the Invention

[0006] The purpose of this invention is to provide a positive electrode slurry, a positive electrode sheet, a method for preparing the same, and its application, which aims to effectively alleviate crystal structure cracks or reduce resistance and increase discharge capacity.

[0007] This invention is implemented as follows:

[0008] In a first aspect, the present invention provides a positive electrode slurry, comprising a solvent and a modified positive electrode material dispersed in the solvent, wherein the modified positive electrode material comprises a positive electrode material substrate and a polymer coating layer coated on the positive electrode material substrate, and the polymer coating layer has a porous structure.

[0009] The preparation process of the positive electrode slurry includes: mixing and coating the positive electrode material substrate and polymer in a solution system and creating pores to form a polymer coating layer, thereby obtaining a second positive electrode material dispersion; mixing the second positive electrode material dispersion with a binder and a conductive agent to obtain the positive electrode slurry.

[0010] In an optional implementation, the positive electrode slurry satisfies at least one of the following conditions (1)-(7):

[0011] (1) The polymer used to prepare the polymer coating layer is selected from at least one of polyimide, polyester, epoxy resin, silicone resin, polyurethane, polyamide, phenolic resin and acrylic resin;

[0012] (2) The polymer coating layer is a mesh;

[0013] (3) The porosity of the polymer coating is 5%-80%;

[0014] (4) The pore diameter of the polymer coating layer is 0.2μm-10μm;

[0015] (5) The mass ratio of the polymer coating layer to the positive electrode material substrate is 0.1-5:100;

[0016] (6) In the positive electrode slurry, the mass fraction of the modified positive electrode material is 80%-98%;

[0017] (7) The cathode material substrate is selected from at least one of lithium cobalt oxide, NC binary cathode material, NM binary cathode material, NCM ternary cathode material and lithium iron phosphate.

[0018] In an optional implementation, the positive electrode slurry satisfies at least one of the following conditions (8)-(11):

[0019] (8) The adhesive is selected from at least one of PVDF, polyacrylic acid, and polyimide;

[0020] (9) The conductive agent is selected from at least one of conductive carbon materials;

[0021] (10) The mass ratio of the modified positive electrode material, binder and conductive agent is 80-98:2-20:2-20;

[0022] (11) The solvent is selected from at least one of NMP, DMAc, DMF and THF.

[0023] In a second aspect, the present invention provides a method for preparing a positive electrode slurry in any of the foregoing embodiments, comprising: mixing and coating a positive electrode material substrate and a polymer in a solution system and creating pores to form a polymer coating layer, thereby obtaining a second positive electrode material dispersion; and mixing the second positive electrode material dispersion with a binder and a conductive agent to obtain a positive electrode slurry.

[0024] In an optional embodiment, a polymer solution, a cathode material substrate, and a solvent are mixed to obtain a first cathode material dispersion having a non-porous polymer coating layer;

[0025] The first cathode material dispersion and the pore-forming agent are mixed and heated to obtain the second cathode material dispersion;

[0026] The second positive electrode material dispersion, binder, and conductive agent are mixed;

[0027] The boiling point of the pore-forming agent is lower than that of the solvent, and the difference between their boiling points is greater than 30°C.

[0028] In an optional embodiment, the process of preparing the first positive electrode material dispersion includes: mixing the positive electrode material substrate, solvent and polymer solution with a solid content of 10%-40%, reacting at a temperature of 60°C-180°C, and reacting for 0.5h-12h.

[0029] Optionally, the mass ratio of the polymer in the polymer solution to the cathode material substrate is 0.1-5:100.

[0030] In an optional embodiment, the pore-forming agent is selected from at least one organic solvent with a boiling point of less than 80°C;

[0031] Optionally, the hole-making process satisfies at least one of the following conditions (12)-(13):

[0032] (12) The pore-forming agent is selected from at least one of methanol, diethyl ether and ethanol;

[0033] (13) During the mixing and heating of the first positive electrode material dispersion and the pore-forming agent, the reaction temperature is controlled at 60℃-180℃ and the reaction time is 0.5h-12h.

[0034] Thirdly, the present invention provides a method for preparing a positive electrode sheet, comprising: coating a positive electrode sheet slurry onto a positive electrode current collector and drying it into a film; wherein the positive electrode sheet slurry is any positive electrode sheet slurry in the foregoing embodiments or a positive electrode sheet slurry prepared by any preparation method in the foregoing embodiments.

[0035] Optionally, the method for preparing the positive electrode sheet satisfies at least one of the following conditions (14)-(15):

[0036] (14) The coating density of the positive electrode slurry is 3 mg / cm³. 2 -20 mg / cm 2 ;

[0037] (15) The positive current collector is selected from at least one of aluminum foil and modified aluminum foil.

[0038] Fourthly, the present invention provides a positive electrode sheet, which is prepared by the preparation method described in the foregoing embodiments.

[0039] Fifthly, the present invention provides a secondary battery, including the positive electrode sheet of the aforementioned embodiments.

[0040] The present invention has the following beneficial effects: by modifying the positive electrode material substrate during the preparation of the positive electrode slurry, a polymer coating layer is formed on the positive electrode material substrate, and the polymer coating layer has a porous structure, which can resist the stress caused by volume change during charging and discharging, effectively alleviate crystal structure cracks, and at the same time reduce resistance and increase discharge capacity. Attached Figure Description

[0041] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation on the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.

[0042] Figure 1 This is a synthetic route diagram for polyimide PTF;

[0043] Figure 2 This is a route diagram for the synthesis of polyester ETT;

[0044] Figure 3 Flowchart of polymer coating pore-forming and pulping process;

[0045] Figure 4 This is a scanning electron microscope (1K) image of the raw material for the cathode material of the present invention;

[0046] Figure 5 This is a scanning electron microscope (3K) image of the raw material for the cathode material of this invention;

[0047] Figure 6 This is a scanning electron microscope (10K) image of the raw material for the cathode material of this invention;

[0048] Figure 7 This is a transmission electron microscope image of the cathode material after pore-forming treatment.

[0049] Figure 8 Cyclic stability test curves of the samples prepared in Example 2 and Comparative Examples 1 and 2;

[0050] Figure 9 The cyclic stability test curves are for the samples prepared in Example 2 and Comparative Examples 1 and 3. Detailed Implementation

[0051] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.

[0052] This invention provides a method for preparing a positive electrode slurry, comprising the following steps:

[0053] S1, Polymer Preparation

[0054] The polymer used to prepare the polymer coating layer is selected from at least one of polyimide, polyester, epoxy resin, silicone resin, polyurethane, polyamide, phenolic resin, and acrylic resin. All of the above polymer types are suitable for use as coating materials. All of the above raw materials can be commercially available or synthesized by conventional methods. Preferably, at least one of polyimide and polyester is selected.

[0055] The synthetic route of polyimide (PTF) is as follows: Figure 1 As shown, a polyimide solution containing one or more functional groups (the type of functional group is not limited) is synthesized from dianhydride, diamine, and monoanhydride as a coating agent, with a solid content of 10% to 40%.

[0056] The synthetic route of polyester (ETT) is as follows: Figure 2 As shown, a polyester solution containing one or more functional groups (the type of functional group is not limited) is synthesized using dianhydride and diol as raw materials as a coating agent, with a solid content of 10% to 40%.

[0057] S2, Formation of polymer coating layer

[0058] Please combine Figure 3 The cathode material substrate and polymer are mixed and coated in a solution system to form a non-porous polymer coating layer. In the slurry preparation, the cathode material substrate and polymer are first added to the solvent, and the non-porous polymer coating layer is formed by controlling the temperature and reaction time.

[0059] In actual operation, the polymer solution, the positive electrode material substrate and the solvent are mixed to obtain the first positive electrode material dispersion with a non-porous polymer coating layer. The reaction temperature is 60℃-180℃ and the reaction time is 0.5h-12h.

[0060] Specifically, the reaction temperature can be 60℃, 80℃, 100℃, 120℃, 140℃, 160℃, 180℃, etc.; the reaction time can be 0.5h, 1.0h, 3.0h, 5.0h, 8.0h, 10.0h, 12.0h, etc.

[0061] In some embodiments, the mass ratio of polymer to cathode material substrate is 0.1-5:100. The polymer is a polymer solution with a solid content of 10%-40% as raw material to ensure that the reaction proceeds fully. The solid content of the polymer solution can be 10%, 20%, 30%, 40%, etc.

[0062] In some embodiments, the cathode material substrate is selected from at least one of lithium cobalt oxide, NC binary cathode material, NM binary cathode material, NCM ternary cathode material and lithium iron phosphate, and can be any of the commonly used cathode material substrates, and also includes the above materials that have been modified by element doping, inorganic coating and other methods.

[0063] In some embodiments, the solvent is selected from at least one of NMP (methylpyrrolidone), DMAc (dimethylacetamide), DMF (dimethylformamide), and THF (tetrahydrofuran), and may be any one or more of the above.

[0064] S3, Hole Formation

[0065] Pore-forming is performed on the unpored polymer coating layer to create a porous structure. The method for creating pores can include adding a pore-forming agent, but is not limited to this. Specifically, the boiling point of the pore-forming agent is lower than that of the solvent, and the difference between their boiling points is greater than 30°C.

[0066] In actual operation, the first positive electrode material dispersion and the pore-forming agent are mixed and heated to obtain the second positive electrode material dispersion. The reaction temperature is controlled at 60℃-180℃ and the reaction time is 0.5h-12h to form a uniform pore structure, so that the coating layer forms a structure similar to a "fishing net".

[0067] Specifically, the reaction temperature can be 60℃, 80℃, 100℃, 120℃, 140℃, 160℃, 180℃, etc.; the reaction time can be 0.5h, 1.0h, 3.0h, 5.0h, 8.0h, 10.0h, 12.0h, etc.

[0068] In some embodiments, the pore-forming agent is selected from at least one organic solvent with a boiling point less than 80°C, and the specific type is not limited, such as at least one of methanol, diethyl ether, and ethanol, or one or more of them. During the reaction, the reaction temperature is controlled to be higher than the boiling point of the pore-forming agent. After the pore-forming agent is vaporized and removed, pores are formed on the material.

[0069] S4. Add binder and conductive agent.

[0070] The second positive electrode material dispersion, binder, and conductive agent are mixed to meet the performance requirements of the positive electrode slurry.

[0071] In some embodiments, the mass ratio of the modified cathode material, binder, and conductive agent is 90:4-6:4-6, such as 90:4:4, 90:5:5, 90:6:6, etc.

[0072] In some embodiments, the adhesive is selected from at least one of PVDF, polyacrylic acid, and polyimide, and can be any one or more of the above. General oil-based adhesives are applicable to the embodiments of the present invention.

[0073] In some embodiments, the conductive agent is selected from at least one of conductive carbon materials, such as Super P Li, conductive graphite, carbon nanotubes, etc.

[0074] This invention provides a positive electrode slurry, comprising a solvent and a modified positive electrode material dispersed in the solvent. The modified positive electrode material includes a positive electrode material substrate and a polymer coating layer coated on the positive electrode material substrate, the polymer coating layer having a porous structure. By modifying the positive electrode material substrate during the preparation of the positive electrode slurry, a polymer coating layer is formed on the positive electrode material substrate, and the polymer coating layer has a porous structure.

[0075] It should be noted that the coating layer possesses excellent mechanical properties, effectively mitigating crystal structure cracks and resisting stress caused by volume changes during charging and discharging. The pore-forming process transforms the coating layer into a "fishing net" structure, allowing partial contact between the electrolyte and the active material, thereby reducing resistance and increasing discharge capacity. Both PTF and ETT coatings (regardless of pore formation) significantly improve cycle stability, and the capacity is also increased after pore formation compared to pure coating. Since most polymers have very low electronic and ionic conductivity, the pore-forming process can reduce the capacity loss caused by polymer coating.

[0076] In some embodiments, the polymer coating layer is a mesh with a porosity of 5%-80% and a pore diameter of 0.2-10 μm. The pore structure is preferably within the above range to effectively alleviate crystal structure cracks.

[0077] In some embodiments, the mass ratio of the polymer coating layer to the positive electrode material substrate is 0.1-5:100, and the content of the polymer coating layer is preferably within the above range, so as to reduce resistance and increase discharge capacity.

[0078] In some embodiments, the modified cathode material has a mass fraction of 80%-98% in the cathode slurry to form a coating with excellent electrochemical performance on the surface of the cathode current collector.

[0079] This invention also provides a method for preparing a positive electrode sheet, comprising: coating a positive electrode sheet slurry onto a positive electrode current collector and drying it into a film; wherein the positive electrode sheet slurry is the positive electrode sheet slurry in the above embodiments.

[0080] Specifically, the method of forming a coating using positive electrode slurry is existing technology and is not limited here. In actual operation, a flatbed coating machine is used to apply the positive electrode slurry to the dry surface of the positive current collector, with a coating density of 3 mg / cm³. 2 -20 mg / cm 2 Afterwards, the electrode is dried at 70°C with forced air until there is no obvious liquid. Then, the electrode is transferred to a vacuum oven and dried under vacuum at 100°C overnight.

[0081] In some embodiments, the positive current collector is selected from at least one of aluminum foil and modified aluminum foil, and can be any one or more of the above.

[0082] This invention provides a positive electrode sheet prepared by the above-described method. The positive electrode sheet can resist the stress caused by volume changes during charging and discharging, effectively alleviate crystal structure cracks, and at the same time reduce resistance and increase discharge capacity.

[0083] This invention also provides a secondary battery, including the above-mentioned positive electrode, and may further include a negative electrode, electrolyte, separator, etc.

[0084] The features and performance of the present invention will be further described in detail below with reference to embodiments.

[0085] Example 1

[0086] This embodiment provides a method for preparing a positive electrode slurry, including the following steps:

[0087] (1) Synthesis of polyimide coating agent PTF

[0088] At room temperature, prepare an acid anhydride mixture of BTDA (3,3,4,4-benzophenone tetracarboxylic acid dianhydride) and PAn (phthalic anhydride) in NMP (N-methylpyrrolidone) solution with a total acid anhydride concentration of 10 wt% and a PAn:BTDA ratio of 2:9. The resulting acid anhydride solution is then set aside for use.

[0089] Prepare a 10 wt% NMP solution of diamine TFDB (2,2'-bis(trifluoromethyl)diaminobiphenyl) to obtain a diamine solution for later use.

[0090] The anhydride solution was slowly added to the diamine solution at a mass ratio of PAn:BTDA:TFDB = 2:9:10. After stirring at room temperature for 1 hour, the mixture was stirred at 120°C for 8 hours to obtain a 10wt% NMP solution of polyimide PTF as the product.

[0091] (2) Covering pore formation

[0092] Under room temperature (25℃) and humidity of 30%, the following process is used to prepare a slurry with a positive electrode material (including coating):PVDF:Super P Li mass ratio of 90:5:5, containing 0.5wt% of coating agent relative to the active material and 2wt% of pore-forming agent relative to the coating agent, and a solid content of 40%:

[0093] Prepare a PVDF solution with a solid content of 5% for later use; use a 10wt% PTF NMP solution as the coating agent.

[0094] 18g of ternary cathode material (Ni90 commercial product) was added to 6mL of NMP, and 0.9g of coating agent solution was added and stirred until homogeneous. The mixture was first stirred in an oil bath at 60℃ for 0.5h at a speed of 700rpm. After the oil bath stirring was completed, the mixture was cooled to room temperature. 1.8mg of pore-forming agent methanol was added and stirred until homogeneous. The mixture was stirred in an oil bath at 80℃ for 40min. After the oil bath stirring was completed, the mixture was cooled to room temperature. 1g of Super PLi conductive agent was added and stirred until homogeneous. Then 20g of PVDF solution was added and stirred until homogeneous. The mixture was stirred at 1500rpm for 1h. Finally, the mixture was transferred to a planetary mixer and stirred at a revolution speed of 7200rpm for 12min to obtain the final slurry.

[0095] This embodiment also provides a method for preparing a positive electrode sheet, which uses the positive electrode sheet slurry in this embodiment to form a coating on an aluminum foil. The specific steps are as follows:

[0096] The slurry was coated onto dry aluminum foil using a flatbed coating machine, with a coating density of 8 mg / cm³. 2 Afterwards, the electrode is dried at 70°C with forced air until there is no obvious liquid. Then, the electrode is transferred to a vacuum oven and dried under vacuum at 100°C overnight.

[0097] Example 2

[0098] This embodiment provides a method for preparing a positive electrode slurry, including the following steps:

[0099] (1) Synthesis of polyester coating agent ETT

[0100] At room temperature, a 10 wt% NMP solution of BTDA (3,3,4,4-benzophenone tetracarboxylic dianhydride) and a 10 wt% NMP solution of triethylene glycol (N-methylpyrrolidone) were prepared. The anhydride solution was slowly added to the triethylene glycol solution at a BTDA:triethylene glycol ratio of 10:11. After stirring at room temperature for 1 hour, the mixture was stirred at 120°C for 8 hours to obtain a 10 wt% NMP solution of ETT as the product.

[0101] (2) Covering pore formation

[0102] Under room temperature (25℃) and humidity of 30%, the following process is used to prepare a slurry with a positive electrode material (including coating):PVDF:Super P Li weight ratio of 90:5:5, containing 0.5wt% of coating agent relative to the active material, 2% of pore-forming agent relative to the coating agent, and a solid content of 40%:

[0103] A PVDF solution with a solid content of 5% was prepared, and the NMP solution with 10 wt% ETT from Example 2 was used as the coating agent solution.

[0104] 18g of ternary cathode material (Ni90 commercial product) was added to 6mL of NMP, and 0.9g of coating agent solution was added and stirred until homogeneous. The mixture was first stirred in an oil bath at 60℃ for 0.5h at a speed of 700rpm. After the oil bath stirring was completed, the mixture was cooled to room temperature. 1.8mg of pore-forming agent methanol was added and stirred until homogeneous. The mixture was stirred in an oil bath at 80℃ for 40min. After the oil bath stirring was completed, the mixture was cooled to room temperature. 1g of Super PLi conductive agent was added and stirred until homogeneous. Then 20g of PVDF solution was added and stirred until homogeneous. The mixture was stirred at 1500rpm for 1h. Finally, the mixture was transferred to a planetary mixer and stirred at a revolution speed of 7200rpm for 12min to obtain the final slurry.

[0105] This embodiment also provides a method for preparing a positive electrode sheet, which uses the positive electrode sheet slurry in this embodiment to form a coating on an aluminum foil. The specific steps are as follows:

[0106] The slurry was coated onto dry aluminum foil using a flatbed coating machine, with a coating density of 8 mg / cm³. 2 Afterwards, the electrode is dried at 70°C with forced air until there is no obvious liquid. Then, the electrode is transferred to a vacuum oven and dried under vacuum at 100°C overnight.

[0107] Example 3

[0108] This embodiment provides a method for preparing a positive electrode slurry, including the following steps:

[0109] (1) Synthesis of polyimide coating agent PTF

[0110] The specific steps are the same as in Example 1, except that the PTF solid content in the product is controlled to be 40%.

[0111] (2) Covering pore formation

[0112] Under room temperature (25℃) and humidity of 30%, the following process is used to prepare a slurry with a positive electrode material (including coating): polyacrylic acid: Super P Li mass ratio of 80:2:2, containing 0.1 wt% of coating agent relative to the active material and 1 wt% of pore-forming agent relative to the coating agent, with a solid content of 40%:

[0113] Prepare a 5% solids polyacrylic acid solution for later use; use a 40 wt% PTF NMP solution as the coating agent solution.

[0114] 18g of ternary cathode material was added to 6mL of NMP, and 0.045g of coating agent solution was added and stirred until homogeneous. The mixture was first stirred in an oil bath at 60℃ for 12h at a speed of 700rpm. After stirring in the oil bath, the mixture was cooled to room temperature. 0.18mg of pore-forming agent ether was added and stirred until homogeneous. The mixture was stirred in an oil bath at 60℃ for 12h. After stirring in the oil bath, the mixture was cooled to room temperature. 0.45g of Super P Li conductive agent was added and stirred until homogeneous. Then, 9g of polyacrylic acid solution was added and stirred until homogeneous. The mixture was stirred at 1500rpm for 1h. Finally, the mixture was transferred to a planetary mixer and stirred at a revolution speed of 7200rpm for 12min to obtain the final slurry.

[0115] This embodiment also provides a method for preparing a positive electrode sheet, which uses the positive electrode sheet slurry in this embodiment to form a coating on an aluminum foil. The specific steps are as follows:

[0116] The slurry was coated onto dry aluminum foil using a flatbed coating machine, with a coating density of 3 mg / cm³. 2 Afterwards, the electrode is dried at 70°C with forced air until there is no obvious liquid. Then, the electrode is transferred to a vacuum oven and dried under vacuum at 100°C overnight.

[0117] Example 4

[0118] This embodiment provides a method for preparing a positive electrode slurry, including the following steps:

[0119] (1) Synthesis of polyimide coating agent PTF

[0120] For specific steps, please refer to Example 1.

[0121] (2) Covering pore formation

[0122] Under room temperature (25℃) and humidity of 30%, the following process is used to prepare a slurry with a positive electrode material (including coating), polyimide, and Super P Li mass ratio of 98:20:20, and a slurry containing 5 wt% of coating agent relative to the active material and 5 wt% of pore-forming agent relative to the coating agent, with a solid content of 40%:

[0123] Prepare a 5% solids content polyimide solution for later use; use a 10 wt% PTF NMP solution as the coating agent solution.

[0124] 18g of ternary cathode material was added to 6mL of NMP, and 9g of coating agent solution was added and stirred until homogeneous. The mixture was first stirred in an oil bath at 180℃ for 0.5h at a speed of 700rpm. After stirring in the oil bath, the mixture was cooled to room temperature. 45mg of pore-forming agent ethanol was added and stirred until homogeneous. The mixture was stirred in an oil bath at 180℃ for 0.5h. After stirring in the oil bath, the mixture was cooled to room temperature. 3.67g of SuperP Li conductive agent was added and stirred until homogeneous. Then 73.47g of polyimide solution was added and stirred until homogeneous. The mixture was stirred at 1500rpm for 1h. Finally, the mixture was transferred to a planetary mixer and stirred at a revolution speed of 7200rpm for 12min to obtain the final slurry.

[0125] This embodiment also provides a method for preparing a positive electrode sheet, which uses the positive electrode sheet slurry in this embodiment to form a coating on an aluminum foil. The specific steps are as follows:

[0126] The slurry was coated onto dry aluminum foil using a flatbed coating machine, with a coating density of 20 mg / cm³. 2 Afterwards, the electrode is dried at 70°C with forced air until there is no obvious liquid. Then, the electrode is transferred to a vacuum oven and dried under vacuum at 100°C overnight.

[0127] Comparative Example 1

[0128] The only difference from Example 1 is that polymer coating and pore formation are not performed.

[0129] Under room temperature (25℃) and humidity of 30%, the following process is used to prepare a slurry with a solid content of 40% at a weight ratio of 90:5:5 for the positive electrode material (excluding coating):PVDF:Super PLi::

[0130] Prepare a PVDF solution with a solid content of 5%. Add the ternary cathode material to NMP, add Super P Li conductive agent and mix well, then add the PVDF solution and mix well. Stir at 1500 rpm for 1 hour, and finally transfer to a centrifuge degasser and stir at 430 rpm revolution speed and 720 rpm rotation speed for 4 minutes, then stir at 1300 rpm revolution speed and 1300 rpm rotation speed for 12 minutes to obtain the final slurry.

[0131] Comparative Example 2

[0132] The only difference from Example 1 is that only polymer coating is performed, and no pore formation is performed.

[0133] Under room temperature (25℃) and humidity of 30%, the following process is used to prepare a slurry with a positive electrode material (including coating, without pore formation):PVDF:Super P Li weight ratio of 90:5:5, and a polymer coating agent of 0.5wt% relative to the active material and a solid content of 40%:

[0134] 18g of ternary cathode material (Chengdu Bamo Ni90 commercial product) was added to 6mL of NMP, and 0.9g of coating agent solution was added and stirred until homogeneous. The mixture was first stirred in an oil bath at 60℃ for 0.5h at a speed of 700rpm. After the oil bath stirring was completed, the mixture was cooled to room temperature. The mixture was stirred until homogeneous, and then stirred in an oil bath at 80℃ for 40min. After the oil bath stirring was completed, the mixture was cooled to room temperature, and 1g of SuperP Li conductive agent was added and stirred until homogeneous. Then, 20g of PVDF solution was added and stirred until homogeneous. The mixture was stirred at 1500rpm for 1h, and finally transferred to a planetary mixer and stirred at a revolution speed of 7200rpm for 12min to obtain the final slurry.

[0135] Comparative Example 3

[0136] The only difference from Example 2 is that only polymer coating is performed, and no pore formation is performed.

[0137] Under room temperature (25℃) and humidity of 30%, the following process is used to prepare a slurry with a positive electrode material (including coating):PVDF:Super P Li weight ratio of 90:5:5, and a polymer coating agent of 0.5wt% relative to the active material and a solid content of 40%:

[0138] A PVDF solution with a solid content of 5% was prepared, and the NMP solution with 10 wt% ETT from Example 2 was used as the coating agent solution.

[0139] 18g of ternary cathode material (Chengdu Bamo Ni90 commercial product) was added to 6mL of NMP, and 0.9g of coating agent solution was added and stirred until homogeneous. The mixture was first stirred in an oil bath at 60℃ for 0.5h at a speed of 700rpm. After the oil bath stirring was completed, the mixture was cooled to room temperature. The mixture was stirred until homogeneous, and then stirred in an oil bath at 80℃ for 40min. After the oil bath stirring was completed, the mixture was cooled to room temperature, and 1g of SuperP Li conductive agent was added and stirred until homogeneous. Then, 20g of PVDF solution was added and stirred until homogeneous. The mixture was stirred at 1500rpm for 1h, and finally transferred to a planetary mixer and stirred at a revolution speed of 7200rpm for 12min to obtain the final slurry.

[0140] Experimental Example 1

[0141] Scanning electron microscopy (SEM) analysis was performed on the positive electrode material in the positive electrode slurry prepared in Example 1. Figure 4 , Figure 5 and Figure 6 The images are electron microscope images at 1, 3, and 10 K, respectively.

[0142] It can be seen that the cathode material exhibits a spherical structure with a particle size of 12 μm.

[0143] The coated and pore-forming cathode material prepared in Example 1 was analyzed by transmission electron microscopy, such as... Figure 7 It can be seen that the coating layer is about 30 nm thick, has a pore size of about 8 nm, and a porosity of about 10%.

[0144] It should be noted that the porosity test method is based on estimation from TEM images, which is the cross-sectional area of ​​the pores divided by the total surface area.

[0145] Experimental Example 2

[0146] The performance of the positive electrode sheets prepared in the test examples and comparative examples is as follows: Figure 8 and Figure 9 .

[0147] The electrochemical test parameters are as follows: After the 2025 coin cell is assembled, it is left at room temperature for 6 hours, activated for 3 cycles at a rate of 0.2C and a voltage of 2.5 to 4.25V, and then subjected to a cycle test at a temperature of 45℃ at a rate of 0.5C and a voltage of 2.5V to 4.25V, maintaining a constant voltage during charging until the current drops to 0.005C.

[0148] In the figure, PTF-coated vias represent Example 1, ETT-coated vias represent Example 2, no coating represents Comparative Example 1, PTF-coated vias represent Comparative Example 2, and ETT-coated vias represent Comparative Example 3. After 50 cycles at 45°C, the cycle retention rate of PTF-coated vias (Example 1) was 94.4%, PTF-coated vias (Comparative Example 2) was 93%, no coating (Comparative Example 1) was 87.5%, ETT-coated vias (Example 2) was 92.9%, and ETT-coated vias (Comparative Example 3) was 92.5%.

[0149] Figure 8 Examples and comparative examples of Ni90 cathode material coated with polyimide PTF. The PTF structure is loose, with almost no loss of capacity. The cycle stability after coating is significantly improved compared to the blank. After coating and pore-forming treatment, the cycle stability is further improved due to the reduction of polarization.

[0150] Figure 9 The results for the polyester ETT coating agent show that, due to the tighter coating of ETT, the capacity is reduced by 15mAh / g after coating, the cycle stability is significantly improved, the advantage is shown after about 50 cycles, and the overall capacity is improved after pore formation.

[0151] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A positive electrode slurry, characterized in that, The invention includes a solvent and a modified cathode material dispersed in the solvent. The modified cathode material includes a cathode material substrate and a polymer coating layer coated on the cathode material substrate. The polymer coating layer has a porous structure. The preparation process of the positive electrode slurry includes: mixing a polymer solution, a positive electrode material substrate, and a solvent to obtain a first positive electrode material dispersion with a non-porous polymer coating layer; mixing the first positive electrode material dispersion and a pore-forming agent and heating to obtain a second positive electrode material dispersion; and mixing the second positive electrode material dispersion with a binder and a conductive agent to obtain the positive electrode slurry. The process of preparing the first positive electrode material dispersion includes: mixing the positive electrode material substrate, solvent and polymer solution with a solid content of 10%-40%, the reaction temperature is 60℃-180℃ and the reaction time is 0.5h-12h; During the mixing and heating process of the first positive electrode material dispersion and the pore-forming agent, the reaction temperature is controlled at 60℃-180℃ and the reaction time is 0.5h-12h. The polymer is selected from polyimide; the boiling point of the pore-forming agent is lower than that of the solvent, and the difference between their boiling points is greater than 30°C.

2. The positive electrode slurry according to claim 1, characterized in that, The positive electrode slurry satisfies at least one of the following conditions (1)-(6): (1) The polymer coating layer is a mesh; (2) The porosity of the polymer coating layer is 5%-80%; (3) The pore diameter of the polymer coating layer is 0.2 μm-10 μm; (4) The mass ratio of the polymer coating layer to the positive electrode material substrate is 0.1-5:100; (5) In the positive electrode slurry, the mass fraction of the modified positive electrode material is 80%-98%; (6) The cathode material substrate is selected from at least one of lithium cobalt oxide, NC binary cathode material, NM binary cathode material, NCM ternary cathode material and lithium iron phosphate.

3. The positive electrode slurry according to claim 1 or 2, characterized in that, The positive electrode slurry satisfies at least one of the following conditions (8)-(11): (8) The adhesive is selected from at least one of PVDF, polyacrylic acid, and polyimide; (9) The conductive agent is selected from at least one of conductive carbon materials; (10) The mass ratio of the modified cathode material, the binder and the conductive agent is 80-98:2-20:2-20; (11) The solvent is selected from at least one of NMP, DMAc, DMF and THF.

4. A method for preparing the positive electrode slurry as described in any one of claims 1-3, characterized in that, include: A polymer solution, a cathode material substrate, and a solvent are mixed to obtain a first cathode material dispersion with a non-porous polymer coating layer. The process of preparing the first positive electrode material dispersion includes: mixing the positive electrode material substrate, solvent and polymer solution with a solid content of 10%-40%, the reaction temperature is 60℃-180℃ and the reaction time is 0.5h-12h; The first positive electrode material dispersion and the pore-forming agent are mixed and heated to obtain the second positive electrode material dispersion; during the mixing and heating of the first positive electrode material dispersion and the pore-forming agent, the reaction temperature is controlled at 60℃-180℃ and the reaction time is 0.5h-12h. The second positive electrode material dispersion is mixed with a binder and a conductive agent to obtain the positive electrode slurry; The polymer used to prepare the polymer coating layer is selected from polyimide; wherein the boiling point of the pore-forming agent is lower than that of the solvent, and the difference between their boiling points is greater than 30°C.

5. The preparation method according to claim 4, characterized in that, The mass ratio of the polymer in the polymer solution to the positive electrode material substrate is 0.1-5:

100.

6. The preparation method according to claim 4, characterized in that, The pore-forming agent is selected from at least one of organic solvents with a boiling point of less than 80°C; Optionally, the pore-forming agent is selected from at least one of methanol, diethyl ether, and ethanol.

7. A method for preparing a positive electrode sheet, characterized in that, include: A positive electrode slurry is coated onto a positive current collector and dried to form a film; wherein the positive electrode slurry is the positive electrode slurry according to any one of claims 1-3 or the positive electrode slurry prepared by any one of claims 4-6; Optionally, the preparation method satisfies at least one of the following conditions (14)-(15): (14) The coating density of the positive electrode slurry is 3 mg / cm³. 2 -20 mg / cm 2 ; (15) The positive current collector is selected from at least one of aluminum foil and modified aluminum foil.

8. A positive electrode sheet, characterized in that, It is prepared by the preparation method described in claim 7.

9. A secondary battery, characterized in that, Includes the positive electrode sheet as described in claim 8.

Citation Information

Patent Citations

  • Flame-retardant porous polymer film and preparation method thereof

    CN101905555A

  • Porous polyimide film and method for producing same

    CN107001681A

  • Preparation method of high-performance positive electrode material for inhibiting dissolution of transition metal ions of lithium ion battery positive electrode material

    CN111200128A