A porous catalyst and its preparation method and application

By mixing γ-alumina with active components such as lanthanide metal salts and titanium dioxide, and using pore-forming agents to increase the specific surface area, a porous catalyst is prepared, which solves the problems of low activity and short life of the existing catalysts and significantly improves the low efficiency Treatment effect and ozone utilization rate of concentrated COD wastewater.

CN116272949BActive Publication Date: 2024-10-25SHANDONG MOTONG ECOLOGICAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310065939.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-06
Publication Date
2024-10-25
Estimated Expiration
2043-02-06

AI Technical Summary

Technical Problem

The existing catalysts have short lifespan, low activity, poor treatment effect on low-concentration COD wastewater, and low ozone utilization rate, resulting in large ozone loss.

Method used

By mixing γ-alumina with active components such as lanthanide metal salts and titanium dioxide, and using pore-forming agents to increase the specific surface area, a porous catalyst is prepared to increase the catalytic activity and ozone contact area.

Benefits of technology

The prepared porous catalyst has high catalytic activity, significantly improves the treatment effect of low-concentration COD wastewater and the utilization rate of ozone, and extends the service life of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116272949B_ABST
    Figure CN116272949B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of catalysts, and provides a method for preparing a porous catalyst. The present invention mixes γ-alumina with an active component to obtain a mixed powder; granulates the mixed powder and a pore-forming agent solution to obtain a catalyst precursor pellet; calcines the catalyst precursor pellet to obtain a porous catalyst; the active component includes a lanthanide metal salt and / or titanium dioxide. The present invention uses γ-alumina as an active carrier and mixes it with a component having a high catalytic activity, and uses a pore-forming agent to increase the specific surface area of ​​the catalyst, thereby preparing a porous catalyst with high catalytic activity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of catalysts, and in particular to a porous catalyst and a preparation method and application thereof. Background Art

[0002] Ozone catalytic oxidation technology is an efficient wastewater deep treatment technology and has been a hot application in the field of wastewater treatment in recent years. Compared with the treatment technology that directly uses ozone as a single oxidant, ozone catalysis refers to the hydroxyl radicals formed by ozone under the action of a catalyst. Hydroxyl radicals have stronger oxidizing properties and can oxidize almost all organic matter. Therefore, the reaction rate with organic matter is higher. At the same time, ozone can directly oxidize organic matter in wastewater into CO under the action of a catalyst. 2 and H 2 O, or oxidize and decompose large molecular organic matter into small molecules, greatly reducing the difficulty of degradation of large molecular organic matter.

[0003] At present, most common catalysts on the market use copper oxide, iron oxide, and manganese dioxide as active components. They have a short lifespan, usually about five years. At the same time, the active components loaded are of a single type, and the loaded carrier has a small specific area, resulting in low catalyst activity and low ozone utilization, resulting in large ozone loss. Existing commercially available catalysts are usually used for front-end high-concentration COD wastewater detoxification treatment in wastewater treatment, but are rarely used for tailwater improvement at the end, and have poor treatment effects on low-concentration COD wastewater. Summary of the invention

[0004] In view of this, the present invention provides a porous catalyst and a preparation method and application thereof. The porous catalyst prepared by the preparation method provided by the present invention has high catalytic activity and has a good treatment effect on low-concentration COD wastewater.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] The present invention provides a method for preparing a porous catalyst, comprising the following steps:

[0007] mixing γ-alumina with active components to obtain mixed powder;

[0008] Granulating the mixed powder and pore-forming agent solution to obtain catalyst precursor pellets;

[0009] calcining the catalyst precursor pellets to obtain a porous catalyst;

[0010] The active component includes lanthanide metal salt and / or titanium dioxide.

[0011] Preferably, the lanthanide metal salt comprises lanthanum nitrate and / or cerium nitrate.

[0012] Preferably, the mesh number of the γ-alumina is 325-400 mesh, and the mass ratio of the γ-alumina to the active component is 10:1-10:3.

[0013] Preferably, the pore-forming agent solution comprises a polyvinyl alcohol aqueous solution, and the mass fraction of the polyvinyl alcohol in the pore-forming agent solution is 1-5%.

[0014] Preferably, the mass ratio of the mixed powder to the pore-forming agent solution is 100:20-40.

[0015] Preferably, the particle size of the catalyst precursor pellets is 3 to 5 mm.

[0016] Preferably, the calcination temperature is 500-600° C., the calcination holding time is 1.5-3 h, and the rate of heating to the calcination temperature is 100-120° C. / h.

[0017] The present invention provides a porous catalyst prepared by the above preparation method, comprising a γ-alumina carrier and an active component loaded on the γ-alumina carrier, wherein the active component is a lanthanide metal oxide, TiO 2 The porous catalyst has a particle size of 3 to 6 mm and a bulk density of 600 to 800 kg / m 3 , specific surface area ≥ 200m 2 / g, and the mass fraction of the active component is 5-25%.

[0018] The present invention provides the use of the porous catalyst in ozone catalytic oxidation of wastewater, wherein the COD content of the wastewater is 500-1500 mg / L.

[0019] The present invention provides a method for preparing a porous catalyst, comprising mixing γ-alumina with an active component to obtain a mixed powder; granulating the mixed powder and a pore-forming agent solution to obtain a catalyst precursor pellet; calcining the catalyst precursor pellet to obtain a porous catalyst; the active component comprises a lanthanide metal salt and / or titanium dioxide. The present invention uses γ-alumina as an active carrier and mixes it with a component having a high catalytic activity, and at the same time uses a pore-forming agent to increase the specific surface area of ​​the catalyst, thereby preparing a porous catalyst with high catalytic activity.

[0020] Furthermore, the present invention controls the mass ratio of active components to γ-alumina, the type of pore-forming solution, the diameter of the pellets obtained after granulation, and the calcination conditions to prepare a porous catalyst with a large specific surface area, high activity, good shape integrity, and appropriate packing density, which is beneficial to increase the contact area with ozone during the ozone catalysis process, improve the catalytic effect on ozone, and thus effectively improve the wastewater treatment effect.

[0021] The present invention also provides a porous catalyst prepared by the preparation method described in the above scheme. The porous catalyst provided by the present invention has a large specific surface area and a suitable stacking density, which is beneficial to having a large reaction area in the process of treating wastewater. At the same time, since the present invention combines the lanthanide metal compound and titanium dioxide with an alumina carrier with a certain activity, the prepared catalyst has a high activity, which is beneficial to improving the catalytic oxidation effect on ozone, and can increase the concentration of ozone catalytic products in low-concentration COD, thereby improving the treatment effect of low-concentration COD wastewater.

[0022] The present invention also provides the use of the porous catalyst described in the above scheme in ozone catalytic oxidation of wastewater. The porous catalyst provided by the present invention has a large specific surface area, high activity, appropriate bulk density, good catalytic oxidation effect on ozone, and is suitable for ozone catalytic oxidation treatment of wastewater. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a comparison chart of the catalytic performance of the commercially available catalyst and the catalyst prepared in Example 1;

[0024] Figure 2 is the COD removal rate of Example 2 and the commercially available catalyst;

[0025] Figure 3 is the COD removal rate of Example 3 and the commercially available catalyst;

[0026] Figure 4 The COD removal rates of Example 4 and commercially available catalysts are shown in FIG. DETAILED DESCRIPTION

[0027] The present invention provides a method for preparing a porous catalyst, comprising the following steps: mixing γ-alumina with an active component to obtain a mixed powder; granulating the mixed powder and a pore-forming agent solution to obtain catalyst precursor pellets; calcining the catalyst precursor pellets to obtain a porous catalyst; the active component comprises a lanthanide metal salt and / or titanium dioxide.

[0028] Unless otherwise specified, the raw materials used in the present invention are all commercially available.

[0029] The present invention mixes γ-alumina with an active component to obtain a mixed powder. In the present invention, the mesh number of the γ-alumina is preferably 325 to 400 meshes, more preferably 350 meshes. The present invention preferably uses the above mesh number of γ-alumina as a carrier. On the one hand, γ-alumina has a higher catalytic activity. On the other hand, the mesh number of the γ-alumina used is easier to granulate, and the cost is low, and the cost will not be multiplied due to the excessive mesh number. In the present invention, the active component includes a lanthanide metal salt and / or titanium dioxide, more preferably a lanthanide metal salt; the lanthanide metal salt is more preferably lanthanum nitrate and / or cerium nitrate, more preferably lanthanum nitrate. In the present invention, the mass ratio of the γ-alumina to the active component is preferably 10:1 to 10:3, more preferably 10:1.5 to 10:2.5, and further preferably 10:2. In the present invention, the mixing method is preferably grinding, the grinding ball-to-material ratio is preferably 8-12:2, more preferably 9-11:2, and more preferably 10:2, the grinding speed is preferably 20-40r / min, more preferably 25-35r / min, and more preferably 30r / min, and the grinding time is preferably 10-20min, more preferably 13-17min, and more preferably 14-15min. The preferred grinding method of the present invention is conducive to making the mixing between the active component and the raw material more uniform.

[0030] After obtaining the mixed powder, the present invention granulates the mixed powder and the pore-forming agent solution to obtain catalyst precursor pellets. In the present invention, the pore-forming agent solution preferably includes a polyvinyl alcohol aqueous solution, and the mass fraction of polyvinyl alcohol in the pore-forming agent solution is preferably 1-5%, and more preferably 2-4%. In the present invention, the polyvinyl alcohol aqueous solution is preferably a polyvinyl alcohol-200 aqueous solution or a polyvinyl alcohol-600 aqueous solution. In the present invention, the preparation method of the polyvinyl alcohol aqueous solution preferably includes the following steps: mixing the polyvinyl alcohol and distilled water to obtain the polyvinyl alcohol aqueous solution, and the mixing temperature is 85-95°C. In the present invention, the mass ratio of the mixed powder and the pore-forming agent solution is preferably 100:20-40, further preferably 100:25-35, and more preferably 100:28-33. In the present invention, the granulation is preferably carried out in a round pot granulator, and the round pot granulator preferably includes a spray device. In the present invention, it is preferred to place the mixed powder in a round pot granulator, and spray the pore-forming agent solution onto the mixed powder through a spray device for rolling granulation. In the present invention, the particle size of the catalyst precursor pellets is preferably 3 to 5 mm, more preferably 3.5 to 4.5 mm, and further preferably 4 mm. In the present invention, the shape of the catalyst precursor pellets is preferably a sphere or spheroid with a smooth surface. The catalyst precursor pellets preferably in the above-mentioned particle size range are conducive to obtaining a catalyst of a suitable particle size after calcination. On the one hand, it prevents the particle size from being too small and causing the catalyst to have an excessively large bulk density, thereby reducing the amount of wastewater treated per unit time. On the other hand, it can prevent the catalyst from having an excessively large particle size, resulting in an excessively small specific surface area of ​​the catalyst, a reduced contact area with ozone, and an adverse effect on the catalytic performance of the catalyst.

[0031] After obtaining the catalyst precursor pellets, the present invention calcines the catalyst precursor pellets to obtain a porous catalyst. In the present invention, the catalyst precursor pellets are preferably dried before calcination, and the drying temperature is preferably 60 to 80°C, more preferably 65 to 75°C, and further preferably 68 to 72°C; the drying time is preferably 4 to 6h, more preferably 4.5 to 5.5h, and further preferably 4.8 to 5.2h. In the present invention, the calcination is preferably carried out in an air atmosphere. In the present invention, the calcination temperature is preferably 500 to 600°C, more preferably 530 to 580°C, and further preferably 540 to 560°C; the calcination holding time is preferably 1.5 to 3h, more preferably 1.6 to 2.5h, and further preferably 1.8 to 2.2h; the rate of rising to the calcination temperature is preferably 100 to 120°C / h. In the present invention, it is preferred to cool down naturally after calcination. In the present invention, the above calcination conditions are preferably used to fully activate the active components and improve the catalytic activity of the catalyst.

[0032] The present invention also provides a porous catalyst prepared by the preparation method of the above scheme, comprising a γ-alumina carrier and an active component loaded on the carrier, wherein the active component is a lanthanide metal oxide and / or TiO 2 The lanthanide metal oxide is preferably La 2 O 3 and / or CeO 2 .

[0033] In the present invention, the particle size of the porous catalyst is 3 to 6 mm, preferably 4 to 5 mm; the bulk density of the porous catalyst is 600 to 800 kg / m 3 , preferably 650~750kg / m 3 ; The specific surface area of ​​the porous catalyst is ≥200m 2 / g, preferably 280 to 360 m 2 / g, more preferably 300 to 350 m 2 / g; the La 2 O 3 and / or TiO 2 Preferably, it is 5-25%, more preferably 10-20%. The porous catalyst prepared by the present invention has a suitable particle size, bulk density and a high specific surface area, which is conducive to improving the catalytic effect on ozone. At the same time, lanthanide metals and titanium as active components can further improve the catalytic effect on ozone.

[0034] The present invention also provides the use of the porous catalyst described in the above scheme in ozone catalytic oxidation wastewater. In the present invention, the COD content in the wastewater is preferably 500-1500 mg / L, more preferably 1000-1500 mg / L, and further preferably 1000-1200 mg / L; the pH value of the wastewater is preferably 8-9, more preferably 8.2-8.8, and further preferably 8.3-8.6. In the present invention, the usage ratio of the porous catalyst to the wastewater is preferably 0.8-1.3 kg 0.9-1.3 L, more preferably 0.8-1.2 kg: 0.9-1.1 L, and further preferably 1-1.2 kg: 0.95-1.05 L.

[0035] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention.

[0036] Example 1

[0037] Weigh 1L of distilled water and heat it to 90°C in a constant temperature water bath, add 10g of polyvinyl alcohol-200 to the distilled water, and stir continuously until the polyvinyl alcohol-200 is dissolved to prepare a 1wt% polyvinyl alcohol aqueous solution pore-forming agent.

[0038] Weigh 325 mesh γ-alumina powder and lanthanum nitrate in a mass ratio of 10:1, grind and mix, the grinding ball-to-material ratio is 10:2, the grinding speed is 20r / min, and the grinding time is 15min to prepare alumina-lanthanum nitrate (La(NO 3 ) 3 ) mixed powder. The mixed powder is then placed in a round pot granulator, and a 1wt% polyvinyl alcohol aqueous solution is sprayed into the granulator for rolling spray granulation. The mass ratio of the mixed powder and the pore-forming agent solution is 10:2. When the mixed powder in the granulator is rolled to form catalyst precursor pellets with a diameter of 3 to 5 mm and a smooth surface, the precursor pellets are taken out and placed in a constant temperature drying oven at 70°C for 5 hours. After drying, the dried precursor pellets are taken out and loaded into a crucible, and the crucible is placed in a box-type resistance furnace and heated to 550°C at a rate of 100°C / h, and then kept at a constant temperature for calcination for 2 hours. After calcination, it is naturally cooled to room temperature and taken out to obtain a porous catalyst. The particle size of the porous catalyst is 4 to 5 mm, and the bulk density is 0.7 kg / m 3 , with a specific surface area of ​​350m 2 / g,La 2 O 3 The mass fraction is 20%.

[0039] Example 2

[0040] Weigh 1L of distilled water and heat it to 90°C in a constant temperature water bath, add 15g of polyvinyl alcohol-200 to the distilled water, and stir continuously until the polyvinyl alcohol-200 is dissolved to prepare a 1.5wt% polyvinyl alcohol aqueous solution pore-forming agent.

[0041] Weigh 325 mesh γ-alumina powder and cerium nitrate in a mass ratio of 10:2, grind and mix, grind the ball-to-material ratio of 10:2, grind at a speed of 30 r / min, and grind for 15 min to prepare alumina-cerium nitrate (Ce(NO 3 ) 3 ) mixed powder. The mixed powder is then placed in a round pot granulator, and a 1.5wt% polyvinyl alcohol aqueous solution is sprayed into the granulator for rolling spray granulation. The mass ratio of the mixed powder and the pore-forming agent solution is 10:2. When the mixed powder in the granulator is rolled to form catalyst precursor pellets with a diameter of 4 to 4.5 mm and a smooth surface, the precursor pellets are taken out and placed in a constant temperature drying oven to dry at 80°C for 4 hours. After drying, the dried precursor pellets are taken out and loaded into a crucible, and the crucible is placed in a box-type resistance furnace and heated to 600°C at a rate of 100°C / h, and then kept at a constant temperature for calcination for 1.5 hours. After calcination, it is naturally cooled to room temperature and taken out to obtain a porous catalyst. The particle size of the porous catalyst is 5 mm, and the bulk density is 630 kg / m 3, with a specific surface area of ​​330m 2 / g,CeO 2 The mass fraction is 10%.

[0042] Example 3

[0043] Weigh 1L of distilled water and heat it to 90°C in a constant temperature water bath, add 15g of polyvinyl alcohol 400 to the distilled water, and stir continuously until the polyvinyl alcohol 400 is dissolved to prepare a 1.5wt% polyvinyl alcohol aqueous solution pore-forming agent.

[0044] Weigh 325 mesh γ-alumina powder and lanthanum nitrate in a mass ratio of 10:3 and grind and mix them. The grinding ball-to-material ratio is 10:3, the grinding speed is 40r / min, and the grinding time is 10min to prepare alumina-lanthanum nitrate (La(NO 3 ) 3 ) mixed powder. The mixed powder is then placed in a round pot granulator, and a 1.5wt% polyvinyl alcohol aqueous solution is sprayed into the granulator for rolling spray granulation. The mass ratio of the mixed powder and the pore-forming agent solution is 100:35. When the mixed powder in the granulator is rolled to form catalyst precursor pellets with a diameter of 3 to 4 mm and a smooth surface, the precursor pellets are taken out and placed in a constant temperature drying oven at 70°C for 5 hours. After drying, the dried precursor pellets are taken out and loaded into a crucible, and the crucible is placed in a box-type resistance furnace and heated to 600°C at a rate of 100°C / h, and then kept at a constant temperature for calcination for 2 hours. After calcination, it is naturally cooled to room temperature and taken out to obtain a porous catalyst. The particle size of the porous catalyst is 4.4 mm, and the bulk density is 570 kg / m 3 , with a specific surface area of ​​350m 2 / g,La 2 O 3 The mass fraction is 15%.

[0045] Example 4

[0046] Weigh 1L of distilled water and heat it to 90°C in a constant temperature water bath, add 15g of polyvinyl alcohol-400 to the distilled water, and stir continuously until the polyvinyl alcohol-400 is dissolved to prepare a 1.5wt% polyvinyl alcohol aqueous solution pore-forming agent.

[0047] Weigh 325 mesh γ-alumina powder, lanthanum nitrate and titanium dioxide for grinding and mixing. The mass ratio of lanthanum nitrate to titanium dioxide is 1:1, the mass ratio of γ-alumina powder to the mixture of lanthanum nitrate and titanium dioxide is 10:2, the grinding ball-to-material ratio is 10:2, the grinding speed is 30r / min, and the grinding time is 15min. Alumina-lanthanum nitrate (La(NO 3 ) 3)-titanium dioxide mixed powder. The mixed powder is then placed in a round pot granulator, and a 1.5wt% polyvinyl alcohol aqueous solution is sprayed into the granulator for rolling spray granulation. The mass ratio of the mixed powder and the pore-forming agent solution is 10:3. When the mixed powder in the granulator is rolled to form catalyst precursor pellets with a diameter of 3.5-4.5mm and a smooth surface, the precursor pellets are taken out and placed in a constant temperature drying oven at 70°C for 5h. After drying, the dried precursor pellets are taken out and loaded into a crucible, and the crucible is placed in a box-type resistance furnace and heated to 550°C at a rate of 100°C / h, and then kept at a constant temperature for calcination for 2.5h. After calcination, it is naturally cooled to room temperature and taken out to obtain a porous catalyst. The particle size of the porous catalyst is 4-5mm, and the bulk density is 600kg / m 3 , with a specific surface area of ​​350m 2 / g,La 2 O 3 and TiO 2 The mass fraction is 15%.

[0048] Application Example 1

[0049] A commercially available catalyst (silicon-aluminum substrate, active components including copper oxide, iron oxide, manganese dioxide, specific surface area> 300m 3 / g) was used as a comparative example and the catalyst prepared in Example 1 of the present application (hereinafter referred to as the homemade catalyst) was tested for performance comparison. The particle sizes of the commercially available catalyst and the homemade catalyst were both 3-5 mm. A target water sample with a COD of 1500 mg / L was prepared using phenol and chlorobenzene distilled water, and the pH value was adjusted to 8.5. 800 mm 3 The catalyst was placed in the same reactor, and 800 mL of the target water sample was poured into each reactor to mix. The ozone generator was turned on, and samples were taken every 30 minutes to detect the COD content in the sample and calculate the COD removal rate. The entire test time lasted for 2 hours, and the test temperature was 120°C. The test results are as follows: Figure 1 As shown, Figure 1 The catalytic performance comparison chart of the commercially available catalyst and the catalyst prepared in Example 1. Figure 1 It can be seen that at 2 hours, the removal rate of COD in the target water sample by the catalyst prepared by the present invention is 13% higher than that of the commercially available catalyst. It can be seen that the catalyst prepared by the present invention has a good catalytic effect.

[0050] The catalytic performance of the catalysts prepared in Examples 2 to 4 is comparable to that of the catalyst prepared in Example 1. The COD removal rate of Example 2 and the commercially available catalyst is as follows: Figure 2 As shown; Example 3 and the COD removal rate of commercially available catalysts are as follows Figure 3 As shown; Example 4 and the COD removal rate of commercially available catalysts are as follows Figure 4 shown.

[0051] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a porous catalyst, characterized in that: The following steps are involved: mixing γ-alumina with active components to obtain mixed powder; Granulating the mixed powder and pore-forming agent solution to obtain catalyst precursor pellets; calcining the catalyst precursor pellets to obtain a porous catalyst; The active component includes lanthanide metal salt and / or titanium dioxide; the lanthanide metal salt includes lanthanum nitrate and / or cerium nitrate; The mesh number of the γ-alumina is 325-400 mesh; the mass ratio of the γ-alumina to the active component is 10:1-10:3; The pore-forming agent solution includes a polyvinyl alcohol aqueous solution, wherein the mass fraction of the polyvinyl alcohol in the pore-forming agent solution is 1 to 5%; the mass ratio of the mixed powder to the pore-forming agent solution is 100:20 to 40; The calcination temperature is 500-600° C., and the calcination holding time is 1.5-2.5 hours.

2. The preparation method according to claim 1, characterized in that: The particle size of the catalyst precursor pellets is 3 to 5 mm.

3. The preparation method according to claim 1, characterized in that: The rate of heating to the calcination temperature is 100-120°C / h.

4. The porous catalyst prepared by the preparation method according to any one of claims 1 to 3, characterized in that: The invention comprises a γ-alumina carrier and an active component loaded on the γ-alumina carrier, wherein the active component is one or more of lanthanide metal oxides and TiO2, the particle size of the porous catalyst is 3 to 6 mm, and the bulk density is 600 to 800 kg / m 3 , specific surface area ≥ 200m 2 / g, and the mass fraction of the active component is 5-25%.

5. Use of the porous catalyst according to claim 4 in ozone catalytic oxidation of wastewater, wherein the COD content of the wastewater is 500 to 1500 mg / L.