In-situ polymethyl methacrylate masterbatch with Rayleigh scattering effect and preparation method thereof

Through the preparation of anatase nanotitanium dioxide and plasma surface treatment, combined with the suspension polymerization process, the problem of uneven distribution of nanoparticles in the light diffusion raw materials is solved, and efficient Rayleigh scattering effect and real blue sky effect are achieved.

CN116284522BActive Publication Date: 2024-12-06KUNSHAN ZHONGYIFENG PHOTOELECTRIC TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310091767.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-10
Publication Date
2024-12-06
Estimated Expiration
2043-02-10

AI Technical Summary

Technical Problem

In the prior art, the direct blending of light diffusion raw materials for preparing light diffusion have problems such as agglomeration and uneven distribution of titanium dioxide nanoparticles, which makes it difficult to feel the real blue sky and sunlight effects.

Method used

Using the preparation of anatase nanotitanium dioxide and plasma surface treatment, a polymethyl methacrylate masterbatch rich in hydrophilic anatase nanotitanium dioxide was prepared through suspension polymerization to ensure nanoscale distribution and uniformity.

Benefits of technology

The nanoscale distribution of the light diffuser in the polymer matrix is ​​realized, and the Rayleigh scattering effect is efficiently realized, the blue sky effect and light transmittance of the light diffuser plate are improved, and the agglomeration phenomenon is avoided.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present application discloses an in-situ polymethyl methacrylate masterbatch with Rayleigh scattering effect and a preparation method thereof. First, a light scattering agent with a particle size of 3 to 4.5 nm is prepared by a sol-gel reaction of a titanate, and after appropriate hydrophilic modification of the surface, it is blended with methyl methacrylate (MMA), and a polymethyl methacrylate-based Rayleigh scattering masterbatch with a narrow particle size distribution and uniform dispersion and a high content of light scattering agent is prepared by suspension polymerization. The preparation method provided by the present invention solves the problems of poor compatibility of light scattering agents such as titanium dioxide with light diffusion base materials, uneven light diffusion, and insufficient scattering effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the preparation of a raw material for a light diffusion plate used to improve indoor environment, and in particular to an in-situ polymethyl methacrylate masterbatch with Rayleigh scattering effect and a preparation method thereof. Background Art

[0002] In recent years, with the improvement of people's material living standards, smart home has entered the vision of thousands of people. The blue sky is no longer the patent of the sky. Artificial indoor blue sky has become a reality, bringing a comfortable indoor environment. With the continuous evolution of lighting technology, people's demand for LED lighting has evolved from the initial brightness and light efficiency to the pursuit of natural light environment and its impact on human physical and mental health. As a result, sky lights that can simulate natural sunlight and blue sky and white clouds began to appear in the public's field of vision and gradually became a rising "star" in the lighting industry. When the white light of the lamp light source passes through a polymer transparent panel with titanium dioxide nanoparticles added, the tiny particles in it will cut off the blue light in the LED, causing it to scatter on the surface, so that the surface of the lamp will eventually present a blue sky effect, and the color temperature of the white light has basically no effect. The panel containing nanoparticles acts like the earth's atmosphere. Sky lights designed based on this principle can make people feel like they are in nature and feel the extremely real blue sky and sunshine.

[0003] However, direct blending in the prior art will cause serious agglomeration problems and uneven distribution of titanium dioxide nanoparticles. At the same time, the titanium dioxide nanoparticles in the prior art such as CN112980125A are too large or too small, and the control of the addition amount will lead to uneven particle distribution, making it difficult to feel the unusually real blue sky and sunshine.

[0004] The technical solution of the present application avoids many deficiencies of the conventional direct blending method for preparing light diffusing raw materials, realizes the nano-scale distribution of the light diffusing agent in the polymer matrix, and efficiently realizes the Rayleigh scattering effect. Summary of the invention

[0005] In view of the problems existing in the above-mentioned prior art, the purpose of this application is to overcome the problems of agglomeration and uneven distribution of titanium dioxide nanoparticles in the prior art, which make it difficult to feel the extremely real blue sky and sunshine, and to provide a method for preparing an in-situ polymethyl methacrylate masterbatch with Rayleigh scattering effect and a preparation method thereof. Methyl methacrylate is referred to as MMA, and polymethyl methacrylate is referred to as PMMA.

[0006] In order to achieve the above objectives, this application adopts the following technical solutions:

[0007] A method for preparing an in-situ polymethyl methacrylate masterbatch with Rayleigh scattering effect comprises the following steps:

[0008] 1) Preparation of anatase nano titanium dioxide: tetrabutyl titanate is mixed with ethanol, acetic acid and deionized water in proportion, and then stirred at room temperature by magnetic high-speed stirring for 30 to 60 minutes, and then placed in an ice water bath, and a certain amount of iron salt aqueous solution is added in proportion. Stirring is stopped after gel appears, and then aged, dried, and calcined at 400 to 450°C to obtain;

[0009] 2) Plasma surface treatment: grinding, ball milling and sieving the anatase nano-titanium dioxide calcined in the previous step, and then treating the anatase nano-titanium dioxide with a size of 3 to 4.5 nm with plasma to impart hydrophilicity to the anatase nano-titanium dioxide, thereby obtaining hydrophilic anatase nano-titanium dioxide;

[0010] 3) The hydrophilic anatase nano-titanium dioxide is prepared into a dispersion liquid, and then MMA, an initiator, and a dispersant are added to prepare a PMMA masterbatch rich in hydrophilic anatase nano-titanium dioxide by a suspension polymerization process.

[0011] Preferably, the reagents involved in the above step 1) are all of chemically pure grade or above;

[0012] Preferably, the above steps 1) to 3) all use primary deionized water;

[0013] Preferably, in the above step 1), the iron salt is one of ferric chloride and ferric nitrate, and the iron content is not higher than 0.05% of the titanium content;

[0014] Preferably, in the above step 3), the initiator is benzoyl peroxide or azobisisobutyronitrile;

[0015] Preferably, in the above step 3), a cationic dispersant is used to disperse titanium dioxide in water.

[0016] Preferably, in the above step 3), a 5 wt% aqueous solution of polyvinyl alcohol 1788 is used as a dispersant for suspension polymerization.

[0017] Preferably, in the above steps, the content of hydrophilic anatase nano-titanium dioxide is 0.005-0.01wt% of the PMMA masterbatch; more preferably 0.008wt%.

[0018] Preferably, in the above steps, the mass of MMA is 10-15wt% of the total reaction system; the total reaction system refers to the reaction system of hydrophilic anatase nano-titanium dioxide dispersion, MMA, initiator and dispersant.

[0019] Preferably, in the suspension polymerization process, the process is as follows: rapid stirring is performed at 40-70°C for 1-3 hours, and after suspended particles appear in the reaction system, the temperature is controlled at 78±2°C, and the reaction is continued for 3-4 hours.

[0020] Preferably, the in-situ polymethyl methacrylate masterbatch obtained in step 3) above needs to be repeatedly precipitated and washed with deionized water for 3 to 5 times, and then filtered and dried.

[0021] Beneficial effects of this application:

[0022] 1. The in-situ polymethyl methacrylate masterbatch with Rayleigh scattering effect provided in the present application improves the affinity between titanium dioxide and polymethyl methacrylate from the source through in-situ polymerization, thereby improving the Rayleigh scattering effect of the subsequent preparation of the light diffusion plate.

[0023] 2. This application uses anatase-type nano-titanium dioxide with a size of 3 to 4.5 nm to perform surface treatment with plasma to impart hydrophilicity to it, thereby obtaining hydrophilic anatase-type nano-titanium dioxide and improving the uniform distribution of titanium dioxide. Anatase-type nano-titanium dioxide with an oversized size will result in its tendency to agglomerate in MMA, limiting the subsequent application of light diffusion plates. Anatase-type nano-titanium dioxide with an undersized size will result in poor hydrophilicity after surface treatment with plasma. The optimal anatase-type nano-titanium dioxide size is 4 nm.

[0024] 3. The hydrophilic anatase nano-titanium dioxide content used in this application is 0.005-0.01wt% of the PMMA masterbatch. Too little hydrophilic anatase nano-titanium dioxide content will lead to poor Rayleigh scattering effect; too much hydrophilic anatase nano-titanium dioxide content will lead to excessively increased light scattering intensity, requiring additional treatment to reduce the generation of agglomeration, and the effect is not good. Even if the agglomeration is eliminated, it is not conducive to presenting a real blue sky effect. The optimal hydrophilic anatase nano-titanium dioxide content is 0.008wt% of the PMMA masterbatch. DETAILED DESCRIPTION

[0025] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art may make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the appended claims of the present application. The specific embodiments are essentially considered to be illustrative and non-restrictive.

[0026] Example 1

[0027] A method for preparing an in-situ polymethyl methacrylate masterbatch with Rayleigh scattering effect comprises the following steps:

[0028] 1) Preparation of anatase nano-titanium dioxide: Tetrabutyl titanate was mixed with ethanol, acetic acid and deionized water in proportion, and then stirred at room temperature for 30 minutes under magnetic high-speed stirring, and then placed in an ice-water bath, and an aqueous solution of ferric chloride with a titanium content of 0.01 wt% was added in proportion. Stirring was stopped after gel appeared, and then aged at room temperature for 6 hours, dried at 80°C for 6 hours, and calcined at 420°C for 1 hour;

[0029] 2) Plasma surface treatment: grinding, ball milling and sieving the anatase-type nano-titanium dioxide calcined in the previous step, and then treating the anatase-type nano-titanium dioxide with a size of 3 nm with plasma to impart hydrophilicity to the anatase-type nano-titanium dioxide, thereby obtaining hydrophilic anatase-type nano-titanium dioxide;

[0030] 3) dispersing titanium dioxide with sodium dodecylbenzene sulfonate to prepare a dispersion, wherein the content of hydrophilic anatase nano-titanium dioxide is 0.005wt% of the PMMA masterbatch, and then adding MMA, benzoyl peroxide as an initiator, and a 5wt% aqueous solution of polyvinyl alcohol 1788 as a dispersant, wherein the mass of MMA is 15wt% of the total reaction system; the rest is deionized water;

[0031] The suspension polymerization process was adopted, with rapid stirring at 40°C for 1h. After suspended particles appeared in the reaction system, the temperature was controlled at 80°C and the reaction was continued for 3h to prepare a PMMA masterbatch rich in hydrophilic rutile nano-titanium dioxide. The mixture was then washed repeatedly with deionized water for 5 times, filtered and dried.

[0032] Example 2

[0033] A method for preparing an in-situ polymethyl methacrylate masterbatch with Rayleigh scattering effect comprises the following steps:

[0034] 1) Preparation of anatase nano-titanium dioxide: Tetrabutyl titanate was mixed with ethanol, acetic acid and deionized water in proportion, and then stirred at room temperature with high-speed magnetic stirring for 50 min, and then placed in an ice-water bath, and an aqueous solution of ferric chloride with a titanium content of 0.02 wt% was added in proportion. Stirring was stopped after gel appeared, and then aged at room temperature for 6 h, dried at 80 ° C for 6 h, and calcined at 450 ° C for 1 h;

[0035] 2) Plasma surface treatment: grinding, ball milling and sieving the anatase-type nano-titanium dioxide calcined in the previous step, and then treating the anatase-type nano-titanium dioxide with a size of 4 nm with plasma to impart hydrophilicity to the anatase-type nano-titanium dioxide, thereby obtaining hydrophilic anatase-type nano-titanium dioxide;

[0036] 3) dispersing titanium dioxide with sodium dodecylbenzene sulfonate to prepare a dispersion, wherein the content of hydrophilic anatase nano-titanium dioxide is 0.01wt% of the PMMA masterbatch, and then adding MMA, benzoyl peroxide as an initiator, and a 5wt% aqueous solution of polyvinyl alcohol 1788 as a dispersant, wherein the mass of MMA is 15wt% of the total reaction system; the rest is deionized water;

[0037] The suspension polymerization process was adopted, with rapid stirring at 60°C for 2 hours. After suspended particles appeared in the reaction system, the temperature was controlled at 78°C and the reaction was continued for 4 hours to prepare a PMMA masterbatch rich in hydrophilic rutile nano-titanium dioxide. The mixture was then washed repeatedly with deionized water for 4 times, filtered and dried.

[0038] Example 3

[0039] A method for preparing an in-situ polymethyl methacrylate masterbatch with Rayleigh scattering effect comprises the following steps:

[0040] 1) Preparation of anatase nano-titanium dioxide: Tetrabutyl titanate was mixed with ethanol, acetic acid and deionized water in proportion, and then stirred at room temperature with high-speed magnetic stirring for 50 min, and then placed in an ice-water bath, and an aqueous solution of ferric chloride with a titanium content of 0.02 wt% was added in proportion. Stirring was stopped after gel appeared, and then aged at room temperature for 6 h, dried at 80 ° C for 6 h, and calcined at 450 ° C for 1 h;

[0041] 2) Plasma surface treatment: grinding, ball milling and sieving the anatase-type nano-titanium dioxide calcined in the previous step, and then treating the anatase-type nano-titanium dioxide with a size of 4 nm with plasma to impart hydrophilicity to the anatase-type nano-titanium dioxide, thereby obtaining hydrophilic anatase-type nano-titanium dioxide;

[0042] 3) dispersing titanium dioxide with sodium dodecylbenzene sulfonate to prepare a dispersion, wherein the content of hydrophilic anatase nano-titanium dioxide is 0.008wt% of the PMMA masterbatch, and then adding MMA, benzoyl peroxide as an initiator, and a 5wt% aqueous solution of polyvinyl alcohol 1788 as a dispersant, wherein the mass of MMA is 15wt% of the total reaction system; the rest is deionized water;

[0043] The suspension polymerization process was adopted, with rapid stirring at 60°C for 2 hours. After suspended particles appeared in the reaction system, the temperature was controlled at 78°C and the reaction was continued for 4 hours to prepare a PMMA masterbatch rich in hydrophilic rutile nano-titanium dioxide. The masterbatch was then washed repeatedly with deionized water for 3 times, filtered and dried.

[0044] Comparative Example 1

[0045] A method for preparing an in-situ polymethyl methacrylate masterbatch with Rayleigh scattering effect comprises the following steps:

[0046] 1) Preparation of anatase nano-titanium dioxide: Tetrabutyl titanate was mixed with ethanol, acetic acid and deionized water in proportion, and then stirred at room temperature for 30 minutes under magnetic high-speed stirring, and then placed in an ice-water bath, and an aqueous solution of ferric chloride with a titanium content of 0.01 wt% was added in proportion. Stirring was stopped after gel appeared, and then aged at room temperature for 6 hours, dried at 80°C for 6 hours, and calcined at 420°C for 1 hour;

[0047] 2) Plasma surface treatment: grinding, ball milling and sieving the anatase nano-titanium dioxide calcined in the previous step, and then treating the anatase nano-titanium dioxide with a size of 30 nm with plasma to impart hydrophilicity to the anatase nano-titanium dioxide, thereby obtaining hydrophilic anatase nano-titanium dioxide;

[0048] 3) dispersing titanium dioxide with sodium dodecylbenzene sulfonate to prepare a dispersion, wherein the content of hydrophilic anatase nano-titanium dioxide is 2wt% of the PMMA masterbatch, and then adding MMA, benzoyl peroxide as an initiator, and a 5wt% aqueous solution of polyvinyl alcohol 1788 as a dispersant, wherein the mass of MMA is 15wt% of the total reaction system; the rest is deionized water;

[0049] The suspension polymerization process was adopted, with rapid stirring at 40°C for 1h. After suspended particles appeared in the reaction system, the temperature was controlled at 80°C and the reaction was continued for 3h to prepare a PMMA masterbatch rich in hydrophilic rutile nano-titanium dioxide. The mixture was then washed repeatedly with deionized water for 5 times, filtered and dried.

[0050] Comparative Example 2

[0051] A method for preparing an in-situ polymethyl methacrylate masterbatch with Rayleigh scattering effect comprises the following steps:

[0052] 1) Preparation of anatase nano-titanium dioxide: Tetrabutyl titanate was mixed with ethanol, acetic acid and deionized water in proportion, and then stirred at room temperature for 30 minutes under magnetic high-speed stirring, and then placed in an ice-water bath, and an aqueous solution of ferric chloride with a titanium content of 0.01 wt% was added in proportion. Stirring was stopped after gel appeared, and then aged at room temperature for 6 hours, dried at 80°C for 6 hours, and calcined at 420°C for 1 hour;

[0053] 2) No plasma surface treatment: The anatase-type nano-titanium dioxide calcined in the previous step was ground, ball-milled, and sieved to obtain anatase-type nano-titanium dioxide with a size of 3 nm; no plasma surface treatment was performed;

[0054] 3) dispersing titanium dioxide with sodium dodecylbenzene sulfonate to prepare a dispersion, wherein the content of anatase nano-titanium dioxide is 0.001wt% of the PMMA masterbatch, and then adding MMA, benzoyl peroxide as an initiator, and a 5wt% aqueous solution of polyvinyl alcohol 1788 as a dispersant, wherein the mass of MMA is 15wt% of the total reaction system; the rest is deionized water;

[0055] The suspension polymerization process was adopted, with rapid stirring at 40°C for 1 hour. After the suspended particles appeared in the reaction system, the temperature was controlled at 80°C and the reaction was continued for 3 hours to prepare a PMMA masterbatch rich in anatase nano-titanium dioxide. The masterbatch was then washed repeatedly with deionized water for 5 times, filtered and dried.

[0056] The PMMA masterbatch prepared in Examples 1 to 3 and Comparative Examples 1 to 2 was prepared into a 10 mm thick light diffuser plate by injection molding and other methods. After testing, the light diffuser plate prepared in Examples 1 to 3 has a real blue sky effect, excellent Rayleigh scattering effect, and the anatase nano titanium dioxide is evenly distributed, and there is no agglomeration phenomenon. The light diffuser plate was tested in the transmittance difference and blueness of the 390-492nm band and the 492-760nm band. The transmittance difference was 36-42%, among which the titanium dioxide distribution uniformity of Example 2 was better than that of Example 1, and the Rayleigh scattering effect was also better than that of Example 1. The transmittance difference of Example 3 was 40-42%, and the titanium dioxide distribution was the most uniform, and the Rayleigh scattering effect was also the best among the examples. However, the transmittance difference of the light diffuser plate prepared in Comparative Example 1 was 3-7%, and that of Comparative Example 2 was 4-9%. The transmittance difference of the light diffuser plate in the comparative example was low, and it was difficult to meet the needs. Correspondingly, in terms of blueness, the light diffuser plates prepared in Examples 1 to 3 have excellent blueness and good blue sky effect, while the plates prepared in Comparative Examples 1 and 2 have lower blueness, agglomeration of titanium dioxide particles, and lower light transmittance.

[0057] The contents explained in the embodiments of the present application should be understood as these embodiments are only used for clearer explanation and are not used to limit the scope of the present application. Without departing from the scope of the present application, all improvements and modifications made should be within the scope of protection of the present application.

Claims

1. A method for preparing an in-situ polymethyl methacrylate masterbatch having Rayleigh scattering effect, comprising the following steps: 1) Preparation of anatase nano titanium dioxide: tetrabutyl titanate is mixed with ethanol, acetic acid and deionized water in proportion, and then stirred at room temperature by magnetic high-speed stirring for 30 to 60 minutes, and then placed in an ice water bath, and a certain amount of iron salt aqueous solution is added in proportion. Stirring is stopped after gel appears, and then aged, dried, and calcined at 400 to 450°C to obtain; 2) Plasma surface treatment: grinding, ball milling and sieving the anatase nano-titanium dioxide calcined in the previous step, and then treating the anatase nano-titanium dioxide with a size of 3 to 4.5 nm with plasma to impart hydrophilicity to the anatase nano-titanium dioxide, thereby obtaining hydrophilic anatase nano-titanium dioxide; 3) The hydrophilic anatase nano-titanium dioxide is prepared into a dispersion liquid, and then MMA, an initiator, and a dispersant are added to prepare a PMMA masterbatch rich in hydrophilic anatase nano-titanium dioxide by a suspension polymerization process.

2. The method for preparing an in-situ polymethyl methacrylate masterbatch having Rayleigh scattering effect according to claim 1, characterized in that: The reagents involved in step 1) are all chemically pure or above.

3. The method for preparing an in-situ polymethyl methacrylate masterbatch having Rayleigh scattering effect according to claim 1 or 2, characterized in that: Steps 1) to 3) all use first-grade deionized water.

4. The method for preparing an in-situ polymethyl methacrylate masterbatch with Rayleigh scattering effect according to claim 1 or 2, characterized in that: The iron salt is one of ferric chloride and ferric nitrate, and the iron content is not higher than 0.05% of the titanium content.

5. The method for preparing an in-situ polymethyl methacrylate masterbatch with Rayleigh scattering effect according to claim 1 or 2, characterized in that: In step 3), the initiator is benzoyl peroxide or azobisisobutyronitrile.

6. The method for preparing an in-situ polymethyl methacrylate masterbatch with Rayleigh scattering effect according to claim 1 or 2, characterized in that: In step 3), titanium dioxide is dispersed in water using a cationic dispersant; the in-situ polymethyl methacrylate masterbatch obtained in step 3) needs to be repeatedly precipitated and washed with deionized water for 3 to 5 times, and then filtered and dried.

7. The method for preparing an in-situ polymethyl methacrylate masterbatch with Rayleigh scattering effect according to claim 1 or 2, characterized in that: In step 3), a 5 wt% aqueous solution of polyvinyl alcohol 1788 is used as a dispersant for suspension polymerization; the mass of MMA is 10-15 wt% of the total reaction system.

8. The method for preparing an in-situ polymethyl methacrylate masterbatch with Rayleigh scattering effect according to claim 1 or 2, characterized in that: The content of hydrophilic anatase nano titanium dioxide is 0.005-0.01wt% of the PMMA masterbatch.

9. The method for preparing an in-situ polymethyl methacrylate masterbatch with Rayleigh scattering effect according to claim 1 or 2, characterized in that: It is characterized in that The content of hydrophilic anatase nano-titanium dioxide is 0.008wt% of the PMMA masterbatch.

10. An in-situ polymethyl methacrylate masterbatch having Rayleigh scattering effect obtained by the preparation method according to any one of claims 1 to 9.