A flame retardant nylon resin composition and preparation method thereof
By combining phosphate ester flame retardant and maleic anhydride grafted PPE in nylon resin, the problem of poor flame retardant performance and compatibility of nylon materials in the existing technology is solved, and excellent flame retardant performance and good compatibility are achieved. Suitable for electronic and electrical components.
Patent Information
- Application Number
- CN202310051550.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-02
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-02-02
AI Technical Summary
When existing halogen-free flame retardant nylon materials reach the UL 94V-0 level of flame retardancy, the material's impact strength and mold corrosion problems are serious, and the poor compatibility between phosphorus-containing flame retardants and nylon resin leads to appearance defects.
Phosphate ester flame retardant and maleic anhydride grafted PPE are combined with polyamide resin, and the flame-retardant nylon resin composition is prepared through mixing and extrusion granulation processes to reduce the amount of aluminum diethyl hypophosphinate and improve the phase. Capacitive and dispersible, reducing precipitation.
It achieves excellent flame retardant properties and good compatibility of the nylon resin composition, reduces the impact strength degradation and mold corrosion problems of the material, and has good market application prospects.
Smart Images

Figure BDA0004058274610000011 
Figure BDA0004058274610000021 
Figure BDA0004058274610000041
Abstract
Description
Technical Field
[0001] The invention belongs to the field of modified plastics, and particularly relates to a flame retardant nylon resin composition and a preparation method thereof. Background Art
[0002] Halogen-free flame-retardant nylon has excellent mechanical properties and processing characteristics, so it has a large number of applications in the field of electronic appliances. The commonly used flame retardant for halogen-free flame-retardant nylon is diethyl aluminum hypophosphite, which is compounded with a small amount of melamine polyphosphate. Diethyl aluminum hypophosphite has good compatibility with nylon and has good flame retardant efficiency. However, it is usually necessary to add a large amount of diethyl aluminum hypophosphite to achieve UL 94V-0 level flame retardancy, which has an adverse effect on the performance of the material. For example: the impact strength of the material deteriorates, and the mold corrosion problem is serious during molding.
[0003] Other phosphorus-containing flame retardants, such as BDP, have little effect on the impact strength of nylon materials and corrosion of molding molds, but they have poor compatibility with nylon resins and are easily precipitated in nylon resins, causing appearance defects, and therefore cannot be used. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a flame retardant nylon resin composition and a preparation method thereof. The nylon resin composition has excellent flame retardant properties. At the same time, the phosphate flame retardant and maleic anhydride grafted PPE used have good compatibility with polyamide resin, less precipitation, and good market application prospects.
[0005] The present invention provides a flame retardant nylon resin composition, comprising the following components in parts by weight:
[0006]
[0007] The maleic anhydride grafted PPE blend comprises 100 parts of PPE resin and 0.5-4 parts of maleic anhydride.
[0008] The polyamide resin is at least one of PA6, PA11, PA12, PA46, PA56, PA66, PA610, PA612, PA6T, PA9T, PA10T, PA1010, and PA1012.
[0009] The maleic anhydride grafted PPE blend is obtained by mixing PPE resin and maleic anhydride at a mixing temperature of 300-350°C.
[0010] Preferably, the particle size of the melamine polyphosphate is 0.5-10 microns.
[0011] Preferably, the mass ratio of the diethyl aluminum hypophosphite, melamine polyphosphate and phosphate flame retardant is (10-15): (2-5): (6-10).
[0012] The phosphate flame retardant is at least one of bisphenol A bis(diphenyl phosphate) BDP, hydroquinone bis(diphenyl phosphate) RDP, and oligomeric phosphate flame retardant PX-220.
[0013] Preferably, the following components are included by weight:
[0014]
[0015] The present invention also provides a method for preparing a flame retardant nylon resin composition, comprising the following steps:
[0016] The raw materials are mixed according to their mass fractions and added into a twin-screw extruder for mixing, melting, homogenization and then extrusion granulation at an extrusion temperature of 250-300° C. to obtain a flame-retardant nylon resin composition.
[0017] The present invention also provides an application of the flame-retardant nylon resin composition in electronic and electrical components, especially relays and connectors.
[0018] The phosphate flame retardant and maleic anhydride grafted PPE in the present invention have excellent compatibility. At the same time, the maleic anhydride group on the PPE molecular chain can be grafted onto the main chain of the polyamide resin, so that the phosphate flame retardant can be well dispersed in the polyamide resin and synergistically act with other original phosphorus-containing flame retardants in the system, thereby reducing the addition amount of diethyl aluminum hypophosphite.
[0019] Beneficial Effects
[0020] The nylon resin composition of the invention has excellent flame retardant performance. The phosphate flame retardant and maleic anhydride grafted PPE used in the invention have good compatibility with the polyamide resin and less precipitation, and has good market application prospects. DETAILED DESCRIPTION
[0021] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0022] Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0023] The raw materials used in the following examples and comparative examples are as follows:
[0024] PA resin 1#: trade name PA66 U4800 NC01, INVISTA.
[0025] PA resin 2#: the product name is PA6 M2400, Xinhui Meida.
[0026] Maleic anhydride grafted PPE blend 1#: 100 parts of PPE resin (PPE LXN040) and 1.5 parts of maleic anhydride (commercially available) were added into a twin-screw extruder and kneaded at 300°C to obtain the blend.
[0027] Maleic anhydride grafted PPE blend 2#: 100 parts of PPE resin (PPE LXN040) and 0.5 parts of maleic anhydride (commercially available) were added into a twin-screw extruder and kneaded at 300°C to obtain the blend.
[0028] Maleic anhydride grafted PPE blend 3#: 100 parts of PPE resin (PPE LXN040) and 4 parts of maleic anhydride (commercially available) were added into a twin-screw extruder and kneaded at 300°C to obtain the blend.
[0029] Maleic anhydride grafted PPE blend 4#: 100 parts of PPE resin (PPE LXN040) and 4.5 parts of maleic anhydride (commercially available) were added into a twin-screw extruder and kneaded at 300°C to obtain the blend.
[0030] PPE resin: The trade name is PPE LXN040, Nantong Xingchen.
[0031] Diethylaluminum hypophosphite: trade name OP 1230, Clariant.
[0032] Melamine polyphosphate: particle size is 8um, trade name is BUDIT 341, Budenheim Company.
[0033] Phosphate flame retardant 1#: bisphenol A bis(diphenyl phosphate), trade name WSFR-BDP-N2, Wansheng Chemical.
[0034] Phosphate flame retardant 2#: oligomeric phosphate flame retardant, trade name WSFR-PX-200, Daba Chemical.
[0035] Non-phosphorus flame retardant: magnesium hydroxide Aitemag 12FD, Jiangsu Aitek Flame Retardant Materials Co., Ltd.
[0036] Glass fiber: model ECS10-03-568H, manufacturer Jushi, diameter 10 microns, short cut length 3 mm.
[0037] The composite materials of each embodiment and comparative example were prepared by the following process:
[0038] The raw materials were mixed according to their mass fractions and added into a twin-screw extruder for mixing, melting, homogenization and then extrusion granulation at an extrusion temperature of 280° C. to obtain a laser-weldable polyamide composite material.
[0039] The embodiments and comparative examples were subjected to the following test methods or test standards:
[0040] Notched impact strength: tested in accordance with ISO 180-2019.
[0041] Vertical burning test: UL94-2018 thickness 0.8mm.
[0042] Mold corrosion test: Evaluate the hot runner needle valve during injection molding. The hot runner temperature is fixed at 285°C, and other process parameters remain unchanged. Each time a new needle valve is replaced, 300 molds are continuously injected to evaluate the corrosion. A represents almost no corrosion, and the weight change of the hot runner needle valve is ≤1%; B represents slight corrosion, and the weight change of the hot runner needle valve is greater than 1% and less than 5%; C represents severe corrosion, and the weight change of the hot runner needle valve is ≥5%.
[0043] Precipitation test: Injection molded high gloss color plate samples, and place them in an 85℃ / 85%RH environment box for 168h, and observe the whitening phenomenon of the surface precipitation. A represents almost no precipitation, B represents slight precipitation, and C represents severe precipitation.
[0044] Table 1 Formula composition and test results of embodiments and comparative examples
[0045]
[0046] From the test results in Table 1, it can be seen that the present invention adopts the compound of phosphate flame retardant and maleic anhydride grafted PPE, not only the vertical flammability can reach V-0, but also the notched impact strength of the material can reach 5.2-8.9KJ / m 2 . It can be seen from Comparative Examples 1 and 2 that when only phosphate flame retardants and maleic anhydride grafted PPE are used, the flame retardant properties do not meet the requirements. It can be seen from Comparative Example 3. When only ordinary PPE resin is used, the material toughness is not good. It can be seen from Comparative Example 5 that when non-phosphorus flame retardants are used in this system, the flame retardant properties also do not meet the requirements. It can be seen from Comparative Example 6 that when the amount of maleic anhydride grafted PPE added is too much, the mold corrosion and precipitation phenomena are worsened. It can be seen from Comparative Examples 6-8 that when the amount of diethyl aluminum hypophosphite, melamine polyphosphate, and phosphate flame retardant 1# added is too much, the toughness of the material declines, and corrosion and precipitation are serious.
[0047] Obviously, the above embodiments of the present invention are only examples for clearly explaining the present invention, and are not intended to limit the implementation methods of the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention shall be included in the protection scope of the claims of the present invention.
Claims
1. A flame retardant nylon resin composition, characterized in that: In parts by weight, it comprises the following components: The maleic anhydride grafted PPE blend is obtained by mixing 100 parts of PPE resin and 0.5-1.5 parts of maleic anhydride; the mass ratio of diethyl aluminum hypophosphite, melamine polyphosphate and phosphate flame retardant is (10-15): (2-5): (6-10).
2. The flame retardant nylon resin composition according to claim 1, characterized in that: The polyamide resin is at least one of PA6, PA11, PA12, PA46, PA56, PA66, PA610, PA612, PA6T, PA9T, PA10T, PA1010, and PA1012.
3. The flame retardant nylon resin composition according to claim 1, characterized in that: The particle size of the melamine polyphosphate is 0.5-10 microns.
4. The flame retardant nylon resin composition according to claim 1, characterized in that: The phosphate flame retardant is at least one of bisphenol A bis(diphenyl phosphate), hydroquinone bis(diphenyl phosphate), and oligomeric phosphate flame retardants.
5. The flame retardant nylon resin composition according to claim 1, characterized in that: In parts by weight, it comprises the following components:
6. A method for preparing the flame retardant nylon resin composition according to any one of claims 1 to 5, comprising the following steps: The raw materials are mixed according to their mass fractions and added into a twin-screw extruder for mixing, melting, homogenization and then extrusion granulation at an extrusion temperature of 250-300° C. to obtain a flame-retardant nylon resin composition.
7. Use of the flame retardant nylon resin composition according to any one of claims 1 to 5 in electronic and electrical components.
Citation Information
Patent Citations
Flame-retardancy-enhanced polyarylidene ether-polyamide composite material, and preparation method and application thereof