A solid polymer electrolyte and a battery preparation method thereof

The solid polymer electrolyte is prepared through cross-linking polymerization of cyclic carbonate monomers and fluorine-substituted phosphate cross-linking agents, and is polymerized in situ in the battery. This solves the problems of insufficient cycle performance and safety of lithium batteries and achieves high performance. Energy density and excellent flame retardancy.

CN116315064BActive Publication Date: 2024-10-01NANKAI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310076371.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-17
Publication Date
2024-10-01
Estimated Expiration
2043-01-17

AI Technical Summary

Technical Problem

Existing lithium batteries have deficiencies in cycle performance and safety. In particular, the oxidation stability window of solid polymer electrolytes is not wide enough to meet high energy density requirements, and it has certain flammability, leading to safety risks.

Method used

The solid polymer electrolyte is prepared through cross-linking polymerization of cyclic carbonate monomers and fluorine-substituted phosphate cross-linking agents, and is polymerized in situ in the battery to achieve close interface contact between the solid electrolyte and the electrode and improve battery performance.

Benefits of technology

It improves the cycle performance and safety of lithium batteries, expands the oxidation stability window, reduces self-ignition time, and enhances the battery's flame retardancy and energy density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004067381470000021
    Figure BDA0004067381470000021
  • Figure BDA0004067381470000031
    Figure BDA0004067381470000031
  • Figure BDA0004067381470000041
    Figure BDA0004067381470000041
Patent Text Reader

Abstract

The present application relates to a method for preparing a solid polymer electrolyte, the method comprising: uniformly mixing a cyclic carbonate monomer, a fluorine-substituted phosphate crosslinking agent, a lithium salt, a solvent and an initiator to obtain a precursor solution; and subjecting the precursor solution to a crosslinking polymerization reaction to obtain the solid polymer electrolyte. The present application also relates to a method for preparing a solid polymer electrolyte, a battery or capacitor containing the solid polymer electrolyte and a method for preparing the same.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of electrochemistry. Specifically, the present application relates to solid polymer electrolytes, methods for preparing the same and uses thereof, in particular uses thereof in batteries or capacitors (e.g., solid lithium metal batteries). The present application also relates to batteries or capacitors comprising the solid polymer electrolytes and methods for preparing the batteries. Background Art

[0002] With the continuous development of society, the demand for high energy density and high safety batteries is increasing. However, the cycle performance and safety of lithium batteries currently used cannot meet the use requirements in various fields, thus hindering the large-scale application of lithium batteries. Electrolyte is an important component of lithium batteries and has a very large impact on the performance of lithium batteries. Compared with liquid electrolytes, solid polymer electrolytes can avoid the leakage of electrolytes and have higher safety, but the development of such batteries still faces some problems. For example, the oxidation stability window of the polymer skeleton is not wide enough to meet the needs of high energy density lithium batteries; solid polymer electrolytes have certain flammability and can also burn when the battery catches fire, causing greater safety problems; and the cycle performance of batteries containing solid polymer electrolytes still needs to be further improved. Summary of the invention

[0003] The present application provides a solid polymer electrolyte, a method for preparing the solid polymer electrolyte, and a battery or capacitor comprising the solid polymer electrolyte. Specifically, the present application obtains a solid polymer electrolyte by cross-linking polymerization of a cyclic carbonate monomer and a fluorine-substituted phosphate cross-linking agent.

[0004] In addition, the present application also provides a method for preparing a solid polymer electrolyte by in-situ polymerization within a battery, thereby achieving close interface contact between the solid electrolyte and the electrode.

[0005] In a first aspect, the present application provides a method for preparing a solid polymer electrolyte, the method comprising:

[0006] uniformly mixing a cyclic carbonate monomer, a fluorine-substituted phosphate crosslinking agent, a lithium salt, a solvent and an initiator to obtain a precursor solution; and

[0007] subjecting the precursor solution to a cross-linking polymerization reaction to obtain the solid polymer electrolyte,

[0008] The cyclic carbonate monomer is a compound represented by Formula 1, a compound represented by Formula 2, or a combination thereof.

[0009]

[0010] In Formula 1 and Formula 2, R1, R2 and R3 are each independently selected from a hydrogen atom, a deuterium atom, a halogen atom, a substituted or unsubstituted C1-C 12 Alkyl, or substituted or unsubstituted C2-C 12 Alkenyl,

[0011] The fluorine-substituted phosphate crosslinking agent is a fluorine-substituted phosphate compound containing two or three polymerizable functional groups,

[0012] Based on the mass of the precursor solution, the content of the cyclic carbonate monomer is 5wt% to 80wt%,

[0013] Based on the mass of the precursor solution, the content of the fluorine-substituted phosphate crosslinking agent is 1wt% to 50wt%,

[0014] The content of the lithium salt is 1 wt % to 40 wt % based on the mass of the precursor solution.

[0015] In a second aspect, the present application provides a method for preparing a battery, the method comprising:

[0016] The cyclic carbonate monomer, the fluorine-substituted phosphate crosslinking agent, the lithium salt, the solvent and the initiator are uniformly mixed to obtain a precursor solution;

[0017] subjecting the precursor solution to a cross-linking polymerization reaction to obtain the solid polymer electrolyte; and

[0018] Assembling the solid polymer electrolyte with the positive electrode and the negative electrode into a battery,

[0019] The cyclic carbonate monomer is a compound represented by Formula 1, a compound represented by Formula 2, or a combination thereof.

[0020]

[0021] In Formula 1 and Formula 2, R1, R2 and R3 are each independently selected from a hydrogen atom, a deuterium atom, a halogen atom, a substituted or unsubstituted C1-C 12 Alkyl, or substituted or unsubstituted C2-C 12 Alkenyl,

[0022] The fluorine-substituted phosphate crosslinking agent is a fluorine-substituted phosphate compound containing two or three polymerizable functional groups,

[0023] Based on the mass of the precursor solution, the content of the cyclic carbonate monomer is 5wt% to 80wt%,

[0024] Based on the mass of the precursor solution, the content of the fluorine-substituted phosphate crosslinking agent is 1wt% to 50wt%,

[0025] The content of the lithium salt is 1 wt % to 40 wt % based on the mass of the precursor solution.

[0026] In a third aspect, the present application provides a method for preparing a battery, the method comprising:

[0027] The cyclic carbonate monomer, the fluorine-substituted phosphate crosslinking agent, the lithium salt, the solvent and the initiator are uniformly mixed to obtain a precursor solution;

[0028] adding the precursor solution to a battery housing including a positive electrode, a negative electrode and a separator; and

[0029] subjecting the precursor solution to a cross-linking polymerization reaction to obtain a battery comprising a solid polymer electrolyte,

[0030] The cyclic carbonate monomer is a compound represented by Formula 1, a compound represented by Formula 2, or a combination thereof.

[0031]

[0032] In Formula 1 and Formula 2, R1, R2 and R3 are each independently selected from a hydrogen atom, a deuterium atom, a halogen atom, a substituted or unsubstituted C1-C 12 Alkyl, or substituted or unsubstituted C2-C 12 Alkenyl,

[0033] The fluorine-substituted phosphate crosslinking agent is a fluorine-substituted phosphate compound containing two or three polymerizable functional groups,

[0034] Based on the mass of the precursor solution, the content of the cyclic carbonate monomer is 5wt% to 80wt%,

[0035] Based on the mass of the precursor solution, the content of the fluorine-substituted phosphate crosslinking agent is 1wt% to 50wt%,

[0036] The content of the lithium salt is 1 wt % to 40 wt % based on the mass of the precursor solution.

[0037] In some embodiments, the fluorine-substituted phosphate crosslinker can be selected from the following

[0038] One or more of the compounds represented by Formula 3 and Formula 4:

[0039]

[0040] Wherein in Formula 3 and Formula 4, m, n, l, o and p are each independently a natural number from 1 to 12, and R4 is independently selected from a hydrogen atom, a deuterium atom, a hydroxyl group, a substituted or unsubstituted C1-C 12Alkyl, substituted or unsubstituted C1-C 12 Alkoxy, substituted or unsubstituted C2-C 12 Unsaturated alkoxy, substituted or unsubstituted C2-C 12 Alkenyl.

[0041] In some embodiments, the lithium salt can be selected from lithium hexafluorophosphate, lithium difluorophosphate, lithium bistrifluoromethylsulfonyl imide, lithium bisfluoromethanesulfonate, lithium perchlorate, lithium tetrafluoroborate, lithium trifluoromethylsulfonate, lithium bistrifluoromethylsulfonamide, lithium bisoxalatoborate, lithium difluorooxalatoborate, or any combination thereof.

[0042] In some embodiments, the solvent can be selected from ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, dimethoxy carbonate, dimethyl carbonate, dioxolane, ethylene glycol dimethyl ether, fluoroethylene carbonate, trifluoroethyl methyl carbonate, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether or 2,2,2-trifluoroethyl-1,1,2,2-tetrafluoroethyl ether or any combination thereof.

[0043] In some embodiments, the initiator may include one or more of azobisisoheptylnitrile, azobisisobutyronitrile, benzoyl peroxide, dibenzoyl peroxide, di-o-toluoyl peroxide, acetylisobutyryl peroxide, and diisopropyl peroxydicarbonate.

[0044] In some embodiments, the positive electrode comprises one or more of lithium iron phosphate, lithium nickel oxide, lithium manganese oxide, lithium cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, and lithium-rich manganese positive electrode materials.

[0045] In some embodiments, the negative electrode includes metallic lithium.

[0046] In some embodiments, the cross-linking polymerization reaction may be performed at a temperature of 0°C to 100°C.

[0047] In some embodiments, the cross-linking polymerization reaction may last from 0.5 hours to 72 hours.

[0048] In some embodiments, the content of the solvent is 10 wt % to 90 wt % based on the mass of the precursor solution.

[0049] In some embodiments, the content of the initiator is 0.01 wt % to 20 wt % of the cyclic carbonate monomer based on the mass of the precursor solution.

[0050] In a fourth aspect, the present application provides a solid polymer electrolyte.

[0051] In a fifth aspect, the present application provides a battery obtained by a battery preparation method.

[0052] In a sixth aspect, the present application provides a battery or a capacitor, wherein the battery or the capacitor comprises a solid polymer electrolyte.

[0053] In a seventh aspect, the present application provides the use of a solid polymer electrolyte in the preparation of a battery or a capacitor. BRIEF DESCRIPTION OF THE DRAWINGS

[0054] Figure 1 This is a graph showing the oxidation stability test of the solid polymer electrolyte according to Example 1.

[0055] Figure 2 This is a cycle diagram of the battery containing the solid polymer electrolyte in Example 5 at 0.5C.

[0056] Figure 3 : is a cycle diagram of the liquid battery according to Comparative Example 1 at 0.5C. Specific implementation plan

[0057] The following definitions and methods are provided to better define this application and guide those of ordinary skill in the art in the practice of this application. Unless otherwise specified, terms are understood according to the conventional usage of those of ordinary skill in the relevant field. All patent documents, academic papers and other publications cited herein are incorporated herein by reference in their entirety.

[0058] As used herein, the term "optional" or "optionally" means that the subsequently described event or circumstance can, but does not have to, occur, and the description includes instances where said event or circumstance occurs and instances where they do not occur.

[0059] As used herein, the term "about" (eg, in the parameters of component amounts) refers to any value within ±5% of a given value, for example, about X can represent any value in the range of 95%X to 105%X.

[0060] Wherever a numerical range is given herein, that range includes its endpoints, and all individual integers and fractions within that range, and also includes each narrower range formed by all possible combinations of those endpoints and internal integers and fractions therein to form subgroups of the larger numerical group within that range to the same extent as if each of those narrower ranges were expressly stated. For example, the cross-linking polymerization reaction is carried out at a temperature of 0°C to 100°C, which means that the temperature of the cross-linking polymerization reaction can be 0°C, 100°C, and any temperature in the range of 0°C to 100°C, such as 0°C, 1°C, 2°C, 3°C, 4°C, 5°C, 6°C, 7°C, 8°C, 9°C, 10°C, 11°C, 12°C, 13°C, 14°C, 15°C, 16°C, 17°C, 18°C, 19°C, 20°C, 21°C, 22°C, 23°C, 24°C, 25°C, 26°C, 27°C, 28°C, 29°C, 30°C, 31°C, 32°C, 33°C, 34°C, 35°C, 36°C, 37°C, 38°C, 39°C, 40°C, 41°C, 42°C, 43°C, 44°C, 45°C, 46°C, 47°C, 48°C, 49°C, 50°C, 51°C, 52°C, 53°C, 54°C, 55°C, 56°C, 57°C, 58°C, 59°C, 60°C, 61°C, 62°C, 63°C, 64°C, 65°C, 66°C, 67°C, 68°C, 69°C, 70°C, 71°C, 72°C, 73°C, 74°C, 75°C, 76°C, 77°C, 78°C, 79°C, 80°C, 81°C, 82°C, 83°C, 84°C, 85°C, 86°C, 87°C, 88°C, 89°C, 90°C, 91°C, 92°C, 93°C, 94°C, 95°C, 96°C, 97°C, 98°C, 99°C or 100°C and ranges formed thereby.

[0061] In the specification, examples of the halogen atom may include a fluorine atom, a chlorine atom, a bromine atom or an iodine atom.

[0062] In this context, an alkyl group may be linear, branched or cyclic. 12Examples of the alkyl group may include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, a tert-butyl group, an isobutyl group, a 2-ethylbutyl group, a 3,3-dimethylbutyl group, an n-pentyl group, an isopentyl group, a neopentyl group, a tert-pentyl group, a cyclopentyl group, a 1-methylpentyl group, a 3-methylpentyl group, a 2-ethylpentyl group, a 4-methyl-2-pentyl group, an n-hexyl group, a 1-methylhexyl group, a 2-ethyl Hexyl group, 2-butylhexyl group, cyclohexyl group, 4-methylcyclohexyl group, 4-tert-butylcyclohexyl group, n-heptyl group, 1-methylheptyl group, 2,2-dimethylheptyl group, 2-ethylheptyl group, 2-butylheptyl group, n-octyl group, tert-octyl group, 2-ethyloctyl group, 3,7-dimethyloctyl group, cyclooctyl group, n-nonyl group, n-decyl group, n-undecyl group, n-dodecyl group and the like, but the embodiment is not limited thereto.

[0063] In this paper, C2-C 12 The alkenyl group may be a hydrocarbon group containing one or more carbon-carbon double bonds in the middle or at the end of an alkyl group having 2 or more carbon atoms. The alkenyl group may be straight or branched. Examples of alkenyl groups may include vinyl groups, 1-butenyl groups, 1-pentenyl groups, 1,3-butadienyl groups, styryl groups, styryl vinyl groups, etc., but embodiments are not limited thereto.

[0064] In this article, the term "substituted or unsubstituted" may mean a group substituted or unsubstituted by at least one substituent selected from the group consisting of a deuterium atom, a halogen atom, a cyano group, a nitro group, an amino group, a silyl group, a hydroxyl group, a sulfenyl group, a sulfinyl group, a sulfonyl group, a carbonyl group, a boron group, a phosphine oxide group, a phosphine sulfide group, an alkyl group, an alkenyl group, an alkynyl group, an alkoxy group, a hydrocarbon ring group, an aryl group and a heterocyclic group. Each of the substituents listed above may itself be substituted or unsubstituted.

[0065] The term "high voltage cathode" refers to an anode with a charge termination voltage greater than 4V, such as LiNi 0.6 Co 0.2 Mn 0.2 O2 positive electrode, lithium cobalt oxide positive electrode, etc.

[0066] As used herein, the term "in-situ prepared battery" means that the preparation of the electrolyte is carried out in the battery casing, thereby obtaining the electrolyte and the battery simultaneously.

[0067] In this article, the term "battery prepared ex situ" refers to a battery obtained by first obtaining an electrolyte and then assembling the electrolyte with positive and negative electrode materials and a battery casing.

[0068] As used herein, the term "polymerizable functional group" refers to a double bond or a triple bond, such as an alkene group or an alkynyl group.

[0069] In some embodiments, the present application provides a solid polymer electrolyte, which can be obtained by a cross-linking polymerization reaction of a solid polymer electrolyte precursor solution, wherein the solid polymer electrolyte precursor solution may contain: a cyclic carbonate monomer, a fluorine-substituted phosphate cross-linker, a lithium salt, a solvent and an initiator.

[0070] In some embodiments, the present application provides a method for preparing a solid polymer electrolyte, which may include: uniformly mixing a cyclic carbonate monomer, a fluorine-substituted phosphate crosslinker, a lithium salt, a solvent, and an initiator to obtain a precursor solution; and subjecting the reacted precursor solution to a crosslinking polymerization reaction to obtain the solid polymer electrolyte.

[0071] In some embodiments, the present application provides a method for preparing a battery, which may include: uniformly mixing a cyclic carbonate monomer, a fluorine-substituted phosphate cross-linking agent, a lithium salt, a solvent, and an initiator to obtain a precursor solution; subjecting the precursor solution to a cross-linking polymerization reaction to obtain the solid polymer electrolyte; and assembling the solid polymer electrolyte with a positive electrode and a negative electrode into a battery.

[0072] In some embodiments, the present application also provides a method for preparing a battery, which may include: uniformly mixing a cyclic carbonate monomer, a fluorine-substituted phosphate cross-linking agent, a lithium salt, a solvent, and an initiator to obtain a precursor solution; adding the precursor solution to a battery casing including a positive electrode, a negative electrode, and a separator; and subjecting the precursor solution to a cross-linking polymerization reaction to obtain a battery comprising a solid polymer electrolyte.

[0073] In some embodiments, the present application also provides a battery or a capacitor comprising a solid polymer electrolyte.

[0074] In some embodiments, the precursor solution may further include an additive. In some embodiments, the additive may be a film former, an overcharge protection agent, a flame retardant, or a combination thereof.

[0075] In some embodiments, the cyclic carbonate-based monomer may be a compound represented by Formula 1, a compound represented by Formula 2, or a combination thereof,

[0076]

[0077] In Formula 1 and Formula 2, R1, R2 and R3 can be each independently selected from a hydrogen atom, a deuterium atom, -F, -Cl, -Br, -I, a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, a tert-butyl group, an isobutyl group, a 2-ethylbutyl group, a 3,3-dimethylbutyl group, an n-pentyl group, an isopentyl group, a neopentyl group, a tert-pentyl group, a cyclopentyl group, a 1-methylpentyl group, a 3-methylpentyl group, a 2-ethylpentyl group, a 4-methyl-2-pentyl group, an n-hexyl group, a 1-methylhexyl group, a 2-ethylhexyl group, The invention also includes but is not limited to cyclopentyl group, cyclohexyl group, 4-methylcyclohexyl group, 4-tert-butylcyclohexyl group, n-heptyl group, 1-methylheptyl group, 2,2-dimethylheptyl group, 2-ethylheptyl group, 2-butylheptyl group, n-octyl group, tert-octyl group, 2-ethyloctyl group, 3,7-dimethyloctyl group, cyclooctyl group, n-nonyl group, n-decyl group, n-undecyl group, n-dodecyl group, vinyl group, 1-butenyl group, 1-pentenyl group, 1,3-butadienyl group, styryl group and styrylvinyl group, etc.

[0078] In some embodiments, the compound represented by Formula 1 may include vinylene carbonate and derivatives thereof.

[0079] In some embodiments, the compound represented by Formula 2 may include vinyl ethylene carbonate and derivatives thereof.

[0080] In some embodiments, the fluorine-substituted phosphate crosslinker is a fluorine-substituted phosphate compound containing two or three polymerizable functional groups.

[0081] In some embodiments, the fluorine-substituted phosphate crosslinker may be selected from one or more of the compounds represented by the following Formula 3 and Formula 4:

[0082]

[0083] In Formula 3 and Formula 4, m, n, l, o and p are each independently a natural number of 1 to 12, for example, m, n and l can each independently be 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11 or 12. R4 is independently selected from a hydrogen atom, a deuterium atom, a hydroxyl group, a substituted or unsubstituted C1-C 12 Alkyl, substituted or unsubstituted C1-C 12 Alkoxy, substituted or unsubstituted C2-C 12 Unsaturated alkoxy, substituted or unsubstituted C2-C 12 Alkenyl.

[0084] Wherein in Formula 3, m, n and l can each independently be a natural number from 1 to 12, for example, m, n and l can each independently be 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11 or 12. In this article, the compound represented by Formula 3 can be named TFP-lmn, wherein 1, m and n represent specific natural numbers within the above range, for example, TFP-1-1-1 represents a compound in which 1, m and n in Formula 3 are each 1; the compound represented by Formula 4 can be named DFP-R4-op, wherein o and p represent specific natural numbers within the above range, for example, DFP-methoxy-1-1 represents a compound in which R4 in Formula 4 is a methoxy group, and o and p are each 1.

[0085] In some embodiments, the cross-linking polymerization reaction can be completed by maintaining the reaction at a certain temperature for a period of time. In some embodiments, the temperature of the cross-linking polymerization reaction can be 0°C to 100°C, preferably 20°C to 80°C, and more preferably 40°C to 60°C. For example, the temperature of the cross-linking polymerization reaction can be 0°C, 2°C, 5°C, 8°C, 10°C, 12°C, 15°C, 18°C, 20°C, 22°C, 25°C, 28°C, 30°C, 31°C, 32°C, 33°C, 34°C, 35°C, 36°C, 37°C, 38°C, 39°C, 40°C, 41°C, 42°C, 43°C, 44°C, 45°C, 46°C, 47°C, 48°C, 49°C, 50°C, 51°C, 52°C, 53°C, 54°C, 55°C, 56°C, 57°C, 58°C, 59°C, 60°C, 61°C, 62°C, 63°C, 64°C, 65°C, 66°C, 67°C, 68°C, 69°C, 70°C, 71°C, 72°C, 73°C, 74°C, 75°C, 76°C, 77°C, 78°C, 79°C, 80°C, 81°C, 82°C, 83°C 2℃, 53℃, 54℃, 55℃, 56℃, 57℃, 58℃, 59℃, 60℃, 61℃, 62℃, 63℃, 64℃, 65℃, 66℃, 67℃, 68℃, 69℃, 70℃, 71℃, 72℃, 73℃, 74℃, 75℃, 76℃, 77℃, 78℃, 79℃, 80℃, 82℃, 85℃, 88℃, 90℃, 92℃, 95℃, 98℃ or 100℃, etc.

[0086] In some embodiments, the reaction time of the cross-linking polymerization reaction can be 0.5 hour, 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 11 hours, 12 hours, 13 hours, 14 hours, 15 hours, 16 hours, 17 hours, 18 hours, 19 hours, 20 hours, 21 hours, 22 hours, 23 hours, 24 hours, 25 hours, 26 hours, 27 hours, 28 hours, 29 hours, 30 hours, 31 hours, 32 hours, 33 hours, 34 hours, 35 hours, 36 hours, 37 hours, 38 hours, 39 hours, 40 hours, 41 hours, 42 hours, 43 hours, 44 hours, 45 hours, 46 hours, 47 hours, 48 ​​hours, 50 hours, 52 hours, 55 hours, 58 hours, 60 hours, 62 hours, 65 hours, 68 hours, 70 hours or 72 hours, etc.

[0087] In some embodiments, the lithium salt can be selected from lithium hexafluorophosphate, lithium difluorophosphate, lithium bistrifluoromethylsulfonyl imide, lithium bisfluoromethanesulfonate, lithium perchlorate, lithium tetrafluoroborate, lithium trifluoromethylsulfonate, lithium bistrifluoromethylsulfonamide, lithium bisoxalate borate, lithium difluorooxalate borate, or any combination thereof. In a preferred embodiment, the lithium salt can be selected from lithium hexafluorophosphate, lithium difluorooxalate borate, lithium bisfluoromethanesulfonate, lithium bistrifluoromethylsulfonamide, or any combination thereof.

[0088] In some embodiments, the solvent can be selected from ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, dimethoxy carbonate, dimethyl carbonate, dioxolane, ethylene glycol dimethyl ether, fluoroethylene carbonate, trifluoroethyl methyl carbonate, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether or 2,2,2-trifluoroethyl-1,1,2,2-tetrafluoroethyl ether or any combination thereof.

[0089] In some embodiments, the initiator may include one or more of azobisisoheptylnitrile, azobisisobutyronitrile, benzoyl peroxide, dibenzoyl peroxide, di-o-toluoyl peroxide, acetylisobutyryl peroxide, and diisopropyl peroxydicarbonate.

[0090] In some embodiments, the positive electrode comprises one or more of lithium iron phosphate, lithium nickel oxide, lithium manganese oxide, lithium cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, and lithium-rich manganese positive electrode materials.

[0091] In some embodiments, the negative electrode includes at least one of Li, Ag, Mg, Cu, Al, Pt, Pd, Au, Ni, Nd, Ir, Cr, Ca, Mo, Ti, W, In, Sn, Zn, their oxides, their compounds, or mixtures thereof.

[0092] In some embodiments, the membrane comprises a material selected from polyethylene film, polypropylene film, nylon nonwoven membrane, alginate fiber nonwoven membrane, cellulose membrane, bacterial cellulose membrane, glass fiber membrane, polyethylene terephthalate membrane, polyimide nonwoven membrane, polyamide membrane, spandex membrane, aramid membrane or any combination thereof.

[0093] In some embodiments, the battery is a lithium battery.

[0094] In some embodiments, based on the mass of the precursor solution, the content of the cyclic carbonate monomer is 5wt% to 80wt%, for example, 10wt% to 75wt%, 20wt% to 70wt%, 30wt% to 60wt%, or 40wt% to 50wt%, for example, 5wt%, 10wt%, 15wt%, 20wt%, 25wt%, 30wt%, 35wt%, 40wt%, 45wt%, 50wt%, 55wt%, 60wt%, 65wt%, 70wt%, 75wt%, or 80wt%. When the content of the cyclic carbonate monomer is less than 5wt%, it is difficult to form a solid polymer electrolyte; when the content of the cyclic carbonate monomer is greater than 80wt%, the ionic conductivity is low.

[0095] In some embodiments, based on the mass of the precursor solution, the content of the fluorine-substituted phosphate crosslinker is 1 wt% to 50 wt%, for example, 5 wt% to 45 wt%, 10 wt% to 40 wt%, or 20 wt% to 30 wt%, for example, 1 wt%, 2 wt%, 4 wt%, 6 wt%, 8 wt%, 10 wt%, 15 wt%, 20 wt%, 25 wt%, 30 wt%, 35 wt%, 40 wt%, 45 wt%, or 50 wt%. When the content of the fluorine-substituted phosphate crosslinker is less than 1 wt%, the polymer skeleton obtained is easily destroyed; when the content of the fluorine-substituted phosphate crosslinker is greater than 50 wt%, the crosslinking degree is too large, affecting the ion transport rate in the solid polymer electrolyte.

[0096] In some embodiments, based on the mass of the precursor solution, the content of the lithium salt is 1 wt% to 40 wt%, such as 5 wt% to 35 wt%, 10 wt% to 30 wt%, or 15 wt% to 25 wt%, such as 1 wt%, 2 wt%, 4 wt%, 6 wt%, 8 wt%, 10 wt%, 15 wt%, 20 wt%, 25 wt%, 30 wt%, 35 wt%, or 40 wt%. When the content of the lithium salt is less than 1 wt%, the ionic conductivity is low; when the content of the lithium salt is greater than 40 wt%, the lithium salt is easily precipitated in the electrolyte.

[0097] In some embodiments, based on the mass of the precursor solution, the content of the solvent is 10wt% to 90wt%, for example, 15wt% to 90wt%, 20wt% to 90wt%, 30wt% to 70wt%, or 40wt% to 60wt%, for example, 10wt%, 15wt%, 20wt%, 25wt%, 30wt%, 35wt%, 40wt%, 45wt%, 50wt%, 55wt%, 60wt%, 65wt%, 70wt%, 75wt%, 80wt%, 85wt%, 90wt%. Adding too little will result in lower ionic conductivity, and adding too much will make it difficult to form a solid polymer electrolyte.

[0098] In some embodiments, based on the mass of the precursor solution, the content of the initiator is 0.01wt%-20wt% of the cyclic carbonate monomer, for example, 1wt% to 18wt%, 2wt% to 15wt%, 5wt% to 12wt%, or 8wt% to 10wt%, for example, 0.01wt%, 0.1wt%, 1wt%, 2wt%, 4wt%, 5wt%, 8wt%, 10wt%, 12wt%, 15wt%, 18wt% or 20wt%.

[0099] In some embodiments, the content of the additive is 0wt% to 20wt%, for example, 1wt% to 18wt%, 2wt% to 15wt%, 5wt% to 12wt%, or 8wt% to 10wt%, for example, 0wt%, 1wt%, 2wt%, 4wt%, 5wt%, 8wt%, 10wt%, 12wt%, 15wt%, 18wt% or 20wt%, based on the mass of the precursor solution.

[0100] In some embodiments, the conductivity of the solid polymer electrolyte is 0.1 mS / cm to 10 mS / cm, for example, 1 mS / cm to 10 mS / cm, 2 mS / cm to 8 mS / cm, or 4 mS / cm to 6 mS / cm, for example 0.1 mS / cm, 1 mS / cm, 2 mS / cm, 4 mS / cm, 6 mS / cm, 8 mS / cm, or 10 mS / cm.

[0101] In some embodiments, the solid polymer electrolyte has an oxidative stability potential of 4.0V to 6.0V, e.g., 4.3V to 6.0V, 4.5V to 5.5V, or 4.6V to 5.0V, e.g., 4.0V, 4.2V, 4.4V, 4.6V, 4.8V, 5.0V, 5.2V, 5.4V, 5.6V, 5.8V, or 6.0V.

[0102] In some embodiments, the solid polymer electrolyte cannot be ignited. In some embodiments, the self-extinguishing time of the solid polymer electrolyte is 0.01s to 30s, for example, 0.1s to 25s, 1s to 20s, 2s to 15s, 4s to 10s, or 5s to 8s, for example 0.01s, 0.1s, 1s, 2s, 3s, 4s, 5s, 6s, 7s, 8s, 9s, 10s, 15s, 20s, 25s, or 30s.

[0103] In some embodiments, the capacity retention rate of the in situ or ex situ prepared battery after 300 cycles at 0.5C is 20% to 100%, for example, 30% to 90%, 35% to 85%, 40% to 80%, 45% to 75%, 50% to 70%, or 55% to 65%, for example 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, or 100%.

[0104] In some embodiments, the discharge specific capacity of the in situ and ex situ prepared batteries at 0.5C is each independently 100 mAh / g to 300 mAh / g, for example, 120 mAh / g to 280 mAh / g, 140 mAh / g to 260 mAh / g, 160 mAh / g to 240 mAh / g, or 180 mAh / g to 220 mAh / g, for example, 100 mAh / g, 110 mAh / g, 120 mAh / g, 130 mAh / g, 140 mAh / g, 150 mAh / g, 160 mAh / g, 170 mAh / g, 180 mAh / g, 190 mAh / g, 200 mAh / g, 220 mAh / g, 240 mAh / g, 250 mAh / g, 280 mAh / g, or 300 mAh / g.

[0105] In some embodiments, the solid polymer electrolyte according to the present application has a high solvent loading. In some embodiments, the solid polymer electrolyte according to the present application has a high ionic conductivity. In some embodiments, the solid polymer electrolyte according to the present application has an excellent cross-linked network structure. In some embodiments, the solid polymer electrolyte according to the present application has excellent mechanical properties. In some embodiments, the solid polymer electrolyte according to the present application has a wide oxidation stability window. In some embodiments, the solid polymer electrolyte according to the present application has excellent interfacial stability to the negative electrode and the high-voltage positive electrode. In some embodiments, the solid polymer electrolyte according to the present application has a short self-extinguishing time when ignited. In some embodiments, the solid polymer electrolyte according to the present application cannot be ignited. In some embodiments, the solid polymer electrolyte according to the present application has excellent flame retardancy. In some embodiments, the solid polymer electrolyte according to the present application has high solvent loading, high ionic conductivity, excellent cross-linked network structure, excellent mechanical properties, high flame retardancy, wide oxidation stability window, excellent interfacial stability to the negative electrode and the high-voltage positive electrode, short self-extinguishing time, excellent flame retardancy and other one or more properties.

[0106] In some embodiments, the battery comprising a solid polymer electrolyte has a high specific capacity. In some embodiments, the battery comprising a solid polymer electrolyte has high safety. In some embodiments, the battery comprising a solid polymer electrolyte has a high energy density. In some embodiments, the battery comprising a solid polymer electrolyte has excellent cycle stability. In some embodiments, the battery comprising a solid polymer electrolyte has an extended cycle life. In some embodiments, the battery comprising a solid polymer electrolyte has excellent rate performance. In some embodiments, the battery comprising a solid polymer electrolyte has excellent flame retardancy, so that safety can be ensured. In some embodiments, the battery comprising a solid polymer electrolyte has one or more properties such as high specific capacity, high energy density, excellent cycle stability, extended cycle life, excellent rate performance, excellent flame retardancy, and high safety.

[0107] Example

[0108] The following examples are for illustration purposes only and are not intended to limit the scope of this application.

[0109] Example 1

[0110] Under an argon atmosphere, ethylene carbonate, diethyl carbonate, and ethyl methyl carbonate were mixed uniformly in a volume ratio of 1:1:1 to obtain a mixed solvent. Then, lithium difluorooxalatoborate (LiDFOB) was added to the mixed solvent to form a solution LE-1, in which LiDFOB 12.25wt%, ethylene carbonate 35.80wt%, diethyl carbonate 25.47wt%, and ethyl methyl carbonate 26.48wt%.

[0111] Under an argon atmosphere, 0.80 g of vinylene carbonate, 0.04 g of TFP-1-1-1, and 8 mg of azobisisoheptanenitrile were added to 1.00 g of the solution LE-1, and stirred to obtain a precursor solution.

[0112] The precursor solution was allowed to stand at 60° C. for 24 hours to obtain a solid polymer electrolyte.

[0113] Example 2

[0114] Under an argon atmosphere, ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate were mixed uniformly in a volume ratio of 1:1:1 to obtain a mixed solvent. Then, lithium hexafluorophosphate (LiPF6) was added to the mixed solvent to form a solution LE-2, in which LiPF6 was 12.24 wt %, ethylene carbonate was 34.82 wt %, dimethyl carbonate was 27.19 wt %, and ethyl methyl carbonate was 25.75 wt %.

[0115] Under an argon atmosphere, 0.50 g of vinylene carbonate, 0.10 g of TFP-1-1-1, 5 mg of azobisisoheptanenitrile, and 0.03 g of LiDFOB were added to 1.50 g of the solution LE-2, and stirred to obtain a precursor solution.

[0116] The precursor solution was allowed to stand at 60° C. for 24 hours to obtain a solid polymer electrolyte.

[0117] Example 3

[0118] Under an argon atmosphere, fluoroethylene carbonate and trifluoroethyl methyl carbonate were mixed in a volume ratio of 3:7 to obtain a mixed solvent. Then, lithium hexafluorophosphate (LiPF6) was added to the mixed solvent to form a solution LE-3, in which LiPF6 was 10.11 wt %, fluoroethylene carbonate was 29.01 wt %, and trifluoroethyl methyl carbonate was 60.88 wt %.

[0119] Under an argon atmosphere, 0.50 g of vinylene carbonate, 0.10 g of TFP-1-1-1, 5 mg of azobisisoheptanenitrile, and 0.03 g of LiDFOB were added to 1.50 g of the solution LE-3, and stirred to obtain a precursor solution.

[0120] The precursor solution was allowed to stand at 60° C. for 24 hours to obtain a solid polymer electrolyte.

[0121] Example 4

[0122] Under an argon atmosphere, ethylene carbonate, diethyl carbonate, and ethyl methyl carbonate were mixed uniformly in a volume ratio of 1:1:1 to obtain a mixed solvent. Then, lithium difluorooxalatoborate (LiDFOB) was added to the mixed solvent to form a solution LE-1, in which LiDFOB 12.25wt%, ethylene carbonate 35.80wt%, diethyl carbonate 25.47wt%, and ethyl methyl carbonate 26.48wt%.

[0123] Under an argon atmosphere, 0.80 g of vinylene carbonate, 0.08 g of DFP-methoxy-1-1, and 8 mg of azobisisoheptanenitrile were added to 1.00 g of the solution LE-1, and stirred to obtain a precursor solution.

[0124] The precursor solution was allowed to stand at 60° C. for 24 hours to obtain a solid polymer electrolyte.

[0125] Example 5

[0126] Under an argon atmosphere, ethylene carbonate, diethyl carbonate, and ethyl methyl carbonate were mixed uniformly in a volume ratio of 1:1:1 to obtain a mixed solvent. Then, lithium difluorooxalatoborate (LiDFOB) was added to the mixed solvent to form a solution LE-1, in which LiDFOB 12.25wt%, ethylene carbonate 35.80wt%, diethyl carbonate 25.47wt%, and ethyl methyl carbonate 26.48wt%.

[0127] Under an argon atmosphere, 0.80 g of vinylene carbonate, 0.04 g of TFP-1-1-1, and 8 mg of azobisisoheptanenitrile were added to 1.00 g of the above LE-1, and stirred uniformly to obtain a precursor solution.

[0128] The above precursor solution is added to the LiNi 0.6 Co 0.2 Mn 0.2 The solid polymer electrolyte and the battery containing the solid polymer electrolyte were prepared by placing the solid polymer electrolyte in a battery housing with O2 as the positive electrode, lithium metal as the negative electrode and polypropylene as the separator. The solid polymer electrolyte was then placed at 60°C for 24 hours to obtain a solid polymer electrolyte and a battery containing the solid polymer electrolyte.

[0129] Example 6

[0130] Under an argon atmosphere, ethylene carbonate, diethyl carbonate, and ethyl methyl carbonate were mixed uniformly in a volume ratio of 1:1:1 to obtain a mixed solvent. Then, lithium difluorooxalatoborate (LiDFOB) was added to the mixed solvent to form a solution LE-1, in which LiDFOB 12.25wt%, ethylene carbonate 35.80wt%, diethyl carbonate 25.47wt%, and ethyl methyl carbonate 26.48wt%.

[0131] Under an argon atmosphere, 0.80 g of vinylene carbonate, 0.04 g of TFP-1-1-1, and 8 mg of azobisisoheptanenitrile were added to 1.00 g of the solution LE-1, and stirred to obtain a precursor solution.

[0132] The precursor solution was added to a battery housing with LiCoO2 as a positive electrode, lithium metal as a negative electrode, and polypropylene as a separator, and then allowed to stand at 60° C. for 24 hours to obtain a solid polymer electrolyte and a battery containing the solid polymer electrolyte.

[0133] Example 7

[0134] Under an argon atmosphere, ethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate were mixed uniformly in a volume ratio of 1:1:1 to obtain a mixed solvent. Then, lithium hexafluorophosphate (LiPF6) was added to the mixed solvent to form a solution LE-2, in which LiPF6 was 12.24 wt %, ethylene carbonate was 34.82 wt %, dimethyl carbonate was 27.19 wt %, and ethyl methyl carbonate was 25.75 wt %.

[0135] Under an argon atmosphere, 0.50 g of vinylene carbonate, 0.10 g of TFP-1-1-1, 5 mg of azobisisoheptanenitrile, and 0.03 g of LiDFOB were added to 1.50 g of the solution LE-2, and stirred to obtain a precursor solution.

[0136] The above precursor solution is added to the LiNi 0.6 Co 0.2 Mn 0.2 The solid polymer electrolyte and the battery containing the solid polymer electrolyte were prepared by placing the solid polymer electrolyte in a battery housing with O2 as the positive electrode, lithium metal as the negative electrode and polypropylene as the separator, and then left to stand at 60° C. for 24 hours to obtain a solid polymer electrolyte and a battery containing the solid polymer electrolyte.

[0137] Example 8

[0138] Under an argon atmosphere, fluoroethylene carbonate and trifluoroethyl methyl carbonate were mixed in a volume ratio of 3:7 to obtain a mixed solvent. Then, lithium hexafluorophosphate (LiPF6) was added to the mixed solvent to form a solution LE-3, in which LiPF6 was 10.11 wt %, fluoroethylene carbonate was 29.01 wt %, and trifluoroethyl methyl carbonate was 60.88 wt %.

[0139] Under an argon atmosphere, 0.50 g of vinylene carbonate, 0.10 g of TFP-1-1-1, 5 mg of azobisisoheptanenitrile, and 0.03 g of LiDFOB were added to 1.50 g of the solution LE-3, and stirred to obtain a precursor solution.

[0140] The above precursor solution is added to the LiNi 0.6 Co 0.2 Mn 0.2 The solid polymer electrolyte and the battery comprising the solid polymer electrolyte are prepared by placing the solid polymer electrolyte in a battery casing with O2 as the positive electrode, lithium metal as the negative electrode and polypropylene as the separator, and then leaving it to stand at 60° C. for 24 hours to obtain a solid polymer electrolyte and a battery comprising the solid polymer electrolyte.

[0141] Example 9

[0142] Under an argon atmosphere, ethylene carbonate, diethyl carbonate, and ethyl methyl carbonate were mixed uniformly in a volume ratio of 1:1:1 to obtain a mixed solvent. Then, lithium difluorooxalatoborate (LiDFOB) was added to the mixed solvent to form a solution LE-1. In the solution LE-1, LiDFOB 12.25wt%, ethylene carbonate 35.80wt%, diethyl carbonate 25.47wt%, and ethyl methyl carbonate 26.48wt%.

[0143] Under an argon atmosphere, 0.80 g of vinylene carbonate, 0.08 g of DFP-methoxy-1-1, and 8 mg of azobisisoheptanenitrile were added to 1.00 g of the solution LE-1, and stirred to obtain a precursor solution.

[0144] The above precursor solution is added to the LiNi 0.6 Co 0.2 Mn 0.2 The solid polymer electrolyte and the battery comprising the solid polymer electrolyte are prepared by placing the solid polymer electrolyte in a battery casing with O2 as the positive electrode, lithium metal as the negative electrode and polypropylene as the separator, and then leaving it to stand at 60° C. for 24 hours to obtain a solid polymer electrolyte and a battery comprising the solid polymer electrolyte.

[0145] Example 10

[0146] The solid polymer electrolyte obtained in Example 1 was mixed with LiNi 0.6 Co 0.2 Mn 0.2The O2 positive electrode and the lithium metal negative electrode are assembled together to form a battery.

[0147] Embodiment 11

[0148] The solid polymer electrolyte obtained in Example 2 was mixed with LiNi 0.6 Co 0.2 Mn 0.2 The O2 positive electrode and the lithium metal negative electrode are assembled together to form a battery.

[0149] Example 12

[0150] The solid polymer electrolyte obtained in Example 3 was mixed with LiNi 0.6 Co 0.2 Mn 0.2 The O2 positive electrode and the lithium metal negative electrode are assembled together to form a battery.

[0151] Example 13

[0152] The solid polymer electrolyte obtained in Example 4 was mixed with LiNi 0.6 Co 0.2 Mn 0.2 The O2 positive electrode and the lithium metal negative electrode are assembled together to form a battery.

[0153] Comparative Example 1

[0154] Under an argon atmosphere, ethylene carbonate, diethyl carbonate, and ethyl methyl carbonate were mixed in a volume ratio of 1:1:1 to obtain a mixed solvent. Then, lithium difluorooxalatoborate (LiDFOB) was added to the mixed solvent to form a solution LE-1, wherein LiDFOB was 12.25 wt %, ethylene carbonate was 35.80 wt %, diethyl carbonate was 25.47 wt %, and ethyl methyl carbonate was 26.48 wt %.

[0155] Add LE-1 to LiNi 0.6 Co 0.2 Mn 0.2 The liquid battery was prepared by placing the liquid battery in a battery housing with O2 as the positive electrode, lithium metal as the negative electrode and polypropylene as the separator. The liquid battery was then placed at 60°C for 24 hours.

[0156] Comparative Example 2

[0157] Under an argon atmosphere, ethylene carbonate, diethyl carbonate, and ethyl methyl carbonate were mixed uniformly in a volume ratio of 1:1:1 to obtain a mixed solvent. Then, lithium difluorooxalatoborate (LiDFOB) was added to the mixed solvent to form a solution LE-1, in which LiDFOB 12.25wt%, ethylene carbonate 35.80wt%, diethyl carbonate 25.47wt%, and ethyl methyl carbonate 26.48wt%.

[0158] Under an argon atmosphere, 0.80 g of vinylene carbonate and 8 mg of azobisisoheptanenitrile were added to 1.00 g of the above LE-1, and stirred uniformly to obtain a precursor solution.

[0159] The precursor solution was allowed to stand at 60° C. for 24 hours to obtain a solid polymer electrolyte.

[0160] Comparative Example 3

[0161] Under an argon atmosphere, ethylene carbonate, diethyl carbonate, and ethyl methyl carbonate were mixed in a volume ratio of 1:1:1 to obtain a mixed solvent. Then, lithium difluorooxalatoborate (LiDFOB) was added to the mixed solvent to form a solution LE-1, in which LiDFOB 12.25wt%, ethylene carbonate 35.80wt%, diethyl carbonate 25.47wt%, and ethyl methyl carbonate 26.48wt%.

[0162] Under an argon atmosphere, 0.80 g of vinylene carbonate and 8 mg of azobisisoheptanenitrile were added to 1.00 g of the above solution LE-1, and stirred uniformly to obtain a precursor solution.

[0163] The precursor solution was added to a battery housing with LiCoO2 as a positive electrode, lithium metal as a negative electrode, and polypropylene as a separator, and allowed to stand at 60° C. for 24 hours to obtain a solid polymer electrolyte and a battery containing the solid polymer electrolyte.

[0164] Comparative Example 4

[0165] The electrolyte obtained in Comparative Example 2 was assembled into a battery together with a LiCoO2 positive electrode and a lithium metal negative electrode.

[0166] Performance Testing

[0167] (1) Test of electrochemical performance

[0168] The batteries in the examples and comparative examples were activated by cycling for 3 cycles at 0.1C, and then cycled at 0.5C to test the cycle performance of the batteries.

[0169] The ion conductivity and oxidation stability potential of the electrolytes of Examples and Comparative Examples are shown in Table 1 below.

[0170] Table 1

[0171]

[0172] As shown in Table 1, the ionic conductivity of the solid polymer electrolyte in Example 1 at room temperature reaches 3.1×10 - 3mS / cm. The higher room-temperature ionic conductivity can ensure that the solid-state battery has a sufficiently high discharge specific capacity at room temperature. The oxidation stability potential at room temperature is as high as 5.9V, which can withstand high operating voltages, achieve higher energy density, and have great application prospects.

[0173] (2) The discharge specific capacity at 0.5 C, the capacity retention rate after 300 cycles at 0.5 C, and the coulombic efficiency after 300 cycles at 0.5 C of the batteries of the examples and comparative examples are shown in Table 2 below.

[0174] Table 2

[0175]

[0176] (3) Flame retardancy test

[0177] The solid polymer electrolyte of the present application and the liquid electrolyte as a reference were ignited, and the ignition time from the start of ignition to the ignition of the electrolyte was measured, and the self-extinguishing time from the ignition of the ignited electrolyte to the automatic extinguishing was measured. The results are shown in Table 3.

[0178] Table 3

[0179]

[0180]

[0181] It can be seen from Table 3 that the solid polymer electrolytes of Examples 1 and 2 can self-extinguish after a short burning time, and the solid polymer electrolyte of Example 3 cannot even be ignited, while the liquid electrolyte LE-1 in Comparative Example 1 cannot self-extinguish, and the solid electrolyte in Comparative Example 2 that does not use a fluorophosphate crosslinking agent needs a long time to self-extinguish. Therefore, the solid polymer electrolyte of the present application can improve the flame retardancy of the battery, thereby improving the safety of the battery.

[0182] It can be seen from Table 2 and Table 3 that the solid polymer electrolyte of the present application can exhibit excellent electrical properties and excellent flame retardancy.

[0183] in addition, Figure 2 The solid polymer electrolyte in Example 5 is LiNi 0.6 Co 0.2 Mn 0.2 The cycle diagram of the battery with O2 as the positive electrode and lithium metal as the negative electrode in the charge and discharge voltage range of 2.8-4.3V and the charge and discharge rate of 0.5C. After 3 cycles of activation at a rate of 0.1C, the solid-state battery showed a high discharge specific capacity of 168.6mAh / g at 0.5C, and the capacity retention rate was 71.9% after 300 cycles. Figure 2It can be seen that the battery containing the solid polymer electrolyte in Example 5 has excellent cycle stability. Figure 3 This is a cycle diagram of the liquid battery using liquid electrolyte in Comparative Example 1 at 0.5C. Figure 2 and Figure 3 It can be seen that, under the same conditions, the cycle performance of the liquid battery is worse than that of the battery with the solid polymer electrolyte of Example 5, which indicates that the solid polymer electrolyte of Example 5 improves the cycle performance of the battery.

[0184] The present application has been described in detail above with general descriptions and specific implementation schemes, but those skilled in the art can make some modifications or improvements based on the above descriptions and make any combination as needed. Therefore, these modifications, improvements and combinations made without departing from the spirit of the present application all fall within the scope of protection claimed by the present application.

Claims

1. A method for preparing a solid polymer electrolyte, comprising: The cyclic carbonate monomer, the fluorine-substituted phosphate crosslinking agent, the lithium salt, the solvent and the initiator are uniformly mixed to obtain a precursor solution; as well as subjecting the precursor solution to a cross-linking polymerization reaction to obtain the solid polymer electrolyte, The cyclic carbonate monomer is a compound represented by Formula 1, a compound represented by Formula 2, or a combination thereof. In Formula 1 and Formula 2, R1, R2 and R3 are each independently selected from a hydrogen atom, a deuterium atom, a halogen atom, a substituted or unsubstituted C1-C 12 Alkyl, or substituted or unsubstituted C2-C 12 Alkenyl, Based on the mass of the precursor solution, the content of the cyclic carbonate monomer is 5wt% to 80wt%, Based on the mass of the precursor solution, the content of the fluorine-substituted phosphate crosslinking agent is 1wt% to 50wt%, Based on the mass of the precursor solution, the content of the lithium salt is 1wt% to 40wt%, The fluorine-substituted phosphate cross-linking agent is selected from one or more compounds represented by the following formula 3 and formula 4: Wherein in Formula 3 and Formula 4, m, n, l, o and p are each independently a natural number from 1 to 12, and R4 is independently selected from a hydrogen atom, a deuterium atom, a hydroxyl group, a substituted or unsubstituted C1-C 12 Alkyl, substituted or unsubstituted C1-C 12 Alkoxy, substituted or unsubstituted C2-C 12 Unsaturated alkoxy, substituted or unsubstituted C2-C 12 Alkenyl.

2. A method for preparing a battery, comprising: The cyclic carbonate monomer, the fluorine-substituted phosphate crosslinking agent, the lithium salt, the solvent and the initiator are uniformly mixed to obtain a precursor solution; subjecting the precursor solution to a cross-linking polymerization reaction to obtain the solid polymer electrolyte; and Assembling the solid polymer electrolyte with the positive electrode and the negative electrode into a battery, The cyclic carbonate monomer is a compound represented by Formula 1, a compound represented by Formula 2, or a combination thereof. In Formula 1 and Formula 2, R1, R2 and R3 are each independently selected from a hydrogen atom, a deuterium atom, a halogen atom, a substituted or unsubstituted C1-C 12 Alkyl, or substituted or unsubstituted C2-C 12 Alkenyl, Based on the mass of the precursor solution, the content of the cyclic carbonate monomer is 5wt% to 80wt%, Based on the mass of the precursor solution, the content of the fluorine-substituted phosphate crosslinking agent is 1wt% to 50wt%, Based on the mass of the precursor solution, the content of the lithium salt is 1wt% to 40wt%, The fluorine-substituted phosphate crosslinking agent is selected from one or more compounds represented by the following formula 3 and formula 4: Wherein in Formula 3 and Formula 4, m, n, l, o and p are each independently a natural number from 1 to 12, and R4 is independently selected from a hydrogen atom, a deuterium atom, a hydroxyl group, a substituted or unsubstituted C1-C 12 Alkyl, substituted or unsubstituted C1-C 12 Alkoxy, substituted or unsubstituted C2-C 12 Unsaturated alkoxy, substituted or unsubstituted C2-C 12 Alkenyl.

3. A method for preparing a battery, comprising: The cyclic carbonate monomer, the fluorine-substituted phosphate crosslinking agent, the lithium salt, the solvent and the initiator are uniformly mixed to obtain a precursor solution; adding the precursor solution to a battery housing including a positive electrode, a negative electrode and a separator; and subjecting the precursor solution to a cross-linking polymerization reaction to obtain a battery comprising a solid polymer electrolyte, The cyclic carbonate monomer is a compound represented by Formula 1, a compound represented by Formula 2, or a combination thereof. In Formula 1 and Formula 2, R1, R2 and R3 are each independently selected from a hydrogen atom, a deuterium atom, a halogen atom, a substituted or unsubstituted C1-C 12 Alkyl, or substituted or unsubstituted C2-C 12 Alkenyl, Based on the mass of the precursor solution, the content of the cyclic carbonate monomer is 5wt% to 80wt%, Based on the mass of the precursor solution, the content of the fluorine-substituted phosphate crosslinking agent is 1wt% to 50wt%, Based on the mass of the precursor solution, the content of the lithium salt is 1wt% to 40wt%, The fluorine-substituted phosphate crosslinking agent is selected from one or more compounds represented by the following formula 3 and formula 4: Wherein in Formula 3 and Formula 4, m, n, l, o and p are each independently a natural number from 1 to 12, and R4 is independently selected from a hydrogen atom, a deuterium atom, a hydroxyl group, a substituted or unsubstituted C1-C 12 Alkyl, substituted or unsubstituted C1-C 12 Alkoxy, substituted or unsubstituted C2-C 12 Unsaturated alkoxy, substituted or unsubstituted C2-C 12 Alkenyl.

4. The method according to any one of claims 1 to 3, wherein The lithium salt is selected from lithium hexafluorophosphate, lithium difluorophosphate, lithium bis(trifluoromethylsulfonyl imide), lithium bis(fluoromethanesulfonate), lithium perchlorate, lithium tetrafluoroborate, lithium trifluoromethylsulfonate, lithium bis(trifluoromethylsulfonamide), lithium bis(oxalatoborate), lithium difluorooxalatoborate or any combination thereof.

5. The method according to any one of claims 1 to 3, wherein The solvent is selected from ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, dimethoxy carbonate, dimethyl carbonate, dioxolane, ethylene glycol dimethyl ether, fluoroethylene carbonate, trifluoroethyl methyl carbonate, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether or 2,2,2-trifluoroethyl-1,1,2,2-tetrafluoroethyl ether or any combination thereof.

6. The method according to any one of claims 1 to 3, wherein The initiator includes one or more of azobisisoheptylnitrile, azobisisobutyronitrile, benzoyl peroxide, dibenzoyl peroxide, di-o-methylbenzoyl peroxide, acetylisobutyryl peroxide, and diisopropyl peroxydicarbonate.

7. The method according to claim 2 or 3, wherein the positive electrode comprises one or more of lithium iron phosphate, lithium nickel oxide, lithium manganese oxide, lithium cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, and lithium-rich manganese positive electrode materials.

8. The method of claim 2 or 3, wherein the negative electrode comprises metallic lithium.

9. The method according to claim 2 or 3, wherein the cross-linking polymerization reaction is carried out at a temperature of 0°C to 100°C.

10. The method of claim 2 or 3, wherein the cross-linking polymerization reaction lasts for 0.5 to 72 hours.

11. The method according to any one of claims 1 to 3, wherein Based on the mass of the precursor solution, the content of the solvent is 10 wt % to 90 wt %.

12. The method of any one of claims 1 to 3, wherein Based on the mass of the precursor solution, the content of the initiator is 0.01 wt % to 20 wt % of the cyclic carbonate monomer.

13. A solid polymer electrolyte prepared by the method of claim 1.

14. A battery prepared by the method of claim 2 or 3, or comprising a solid polymer electrolyte prepared by the method of claim 1.