Base coating composition and coated article

Through a solvent-based coating composition with high solid content, including pigments, hydroxyl-containing acrylic resin and blocked isocyanate compounds, the problem of high energy consumption of water-based coatings is solved, and excellent adhesion of the coating film is achieved in multi-layer coating. and water resistance, meeting the dual requirements of environment and appearance design.

CN116323013BActive Publication Date: 2024-10-18NIPPON PAINT AUTOMOTIVE COATINGS
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202180067975.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-04
Publication Date
2024-10-18
Estimated Expiration
2041-10-04

AI Technical Summary

Technical Problem

Existing water-based basic coating compositions require a large amount of energy during drying and curing, resulting in heavy equipment load and difficulty in finding a balance between environment and appearance design. Existing solvent-based coatings are energy-saving but difficult to control in multi-layer curing methods. The adhesion and water resistance of the coating film.

Method used

It uses a solvent-based paint with high solid content, including pigments, hydroxyl-containing acrylic resin, blocked isocyanate compounds and polymer cross-linked particles. Through a specific combination of viscosity recovery rate and molecular weight, an excellent base coating film is formed to ensure the durability of bright pigments. Uniformity and film adhesion.

Benefits of technology

It shortens the drying time, optimizes the appearance design, improves the adhesion and water resistance of the coating film, reduces the unevenness and defects of the coating film, and meets the dual requirements of environment and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004159196640000201
    Figure BDA0004159196640000201
  • Figure BDA0004159196640000211
    Figure BDA0004159196640000211
  • Figure BDA0004159196640000251
    Figure BDA0004159196640000251
Patent Text Reader

Abstract

The present invention provides a base coating composition and a coated article obtained therefrom, wherein the base coating composition can form a base coating film having excellent appearance design (unevenness of bright pigment), adhesion and water resistance while satisfying environmental considerations such as shortening the drying time. The present invention provides a coating composition containing a pigment (A), a hydroxyl-containing acrylic resin (B), a blocked isocyanate compound (C), a polymer crosslinked microparticle (D) that is insoluble and stably dispersed in the aforementioned hydroxyl-containing acrylic resin (B) solution, and an acrylic resin (E) having a weight average molecular weight different from that of the hydroxyl-containing acrylic resin (B), wherein a specific hydroxyl-containing acrylic resin (B) is used and the viscosity recovery rate is adjusted. The present invention also provides a coated article formed using the base coating composition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to base coating compositions and coated articles. Background Art

[0002] For example, on a coated object such as a substrate constituting an automobile, a base coating and a clear coating thereon are usually provided for the purpose of imparting a design and durability. The base coating composition forming such a base coating is a basic coating that affects the design of the coated object, but various requirements must be met in consideration of the environment and the ease of coating operations. For example, the base coating composition is disclosed in Patent Documents 1 and 2.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2008-138179

[0006] Patent Document 2: Japanese Patent Application Publication No. 2010-82529 Summary of the invention

[0007] Problems to be solved by the invention

[0008] In consideration of the environment, water-based base coating compositions rather than solvent-based ones have been studied, and a water-based base coating composition is disclosed in Patent Document 1. However, water-based base coating compositions require energy in any case in order to evaporate water during drying and curing, and thus impose a large load on equipment.

[0009] Patent Document 2 does not use a water-based base coating composition but a solvent-based base coating composition. However, a 3-coat 1-bake method is adopted in which 3 layers (middle layer, base layer and clear layer) are applied and then cured at one time. This saves energy, improves the burden on equipment, and meets environmental considerations.

[0010] However, the base coating composition is the most important coating that determines the appearance of the coated object, and there are coatings above and below the base coating, which requires high control. In addition, it is very difficult to take environmental considerations into account, which may not be achieved by the coatings of the prior art.

[0011] The present invention is made in view of the above situation. In the present invention, a solvent-based paint with a high solid content (also called "highsolid") is used to provide a base coating composition and a coated article obtained therefrom that can form a base coating film with excellent appearance design (making the unevenness of bright pigments), adhesion and water resistance while satisfying environmental considerations such as shortening the drying time.

[0012] Means of solving problems

[0013] The present invention provides the following aspects.

[0014] [1] A base coating composition comprising a pigment (A), a hydroxyl-containing acrylic resin (B), a blocked isocyanate compound (C), polymer crosslinked fine particles (D) which are insoluble in a solution of the hydroxyl-containing acrylic resin (B) and are stably dispersed, and an acrylic resin (E) having a weight average molecular weight different from that of the hydroxyl-containing acrylic resin (B),

[0015] The solid content is 35% by mass or more,

[0016] The viscosity V1 was measured at 23°C using a cone-plate viscometer at a shear rate of 0.1 / sec, and then the shear rate was changed from 0.1 / sec to 25000 / sec for 30 seconds.

[0017] Then, the shearing is restored to 0.1 / sec, and when the viscosity V2 after 1 second of shearing is measured, the viscosity recovery rate V2 / V1, which is the ratio of V2 to V1, is 90% or more.

[0018] The pigment (A) contains at least one selected from coloring pigments and flaky pigments,

[0019] The hydroxyl-containing acrylic resin (B) is a polymer containing one or more monomers of a hydroxyl-containing monomer (b), wherein the hydroxyl-containing monomer (b) is a lactone-modified monoester compound of (meth)acrylic acid and a diol having 2 to 8 carbon atoms, and the hydroxyl-containing acrylic resin (B) has a weight average molecular weight of 10,000 to 20,000, a glass transition temperature of 10° C. to 40° C., and a hydroxyl value of 10 mgKOH / g to 50 mgKOH / g.

[0020] The weight average molecular weight of the acrylic resin (E) is 3,000 or more and 7,500 or less.

[0021] [2] The base coating composition described in [1], wherein the hydroxyl-containing acrylic resin (B) is a polymer of the hydroxyl-containing monomer (b) and a monomer other than the hydroxyl-containing monomer (b),

[0022] The hydroxyl group-containing monomer (b) accounts for 5% by mass or more and 20% by mass or less of the total of the hydroxyl group-containing monomer (b) and the other monomers.

[0023] [3] A coated article comprising an article to be coated and a base coating film formed from the base coating composition according to [1] or [2].

[0024] [4] The coated article according to [3], comprising a multilayer coating film, wherein the multilayer coating film comprises a base coating film provided on the coated object and a clear coating film provided on the base coating film.

[0025] [5] The coated article described in [3] comprises a multilayer coating film, wherein the multilayer coating film comprises a base coating film provided on the aforementioned object to be coated having a middle coating film or a primer coating film provided in advance, and a clear coating film provided on the aforementioned base coating film.

[0026] Effects of the Invention

[0027] The present invention provides a base coating composition, which is a base coating composition of a hydroxyl-containing acrylic resin crosslinked with a blocked isocyanate compound, and by mixing an acrylic resin with a low weight average molecular weight different from the above-mentioned hydroxyl-containing acrylic resin and polymer crosslinked microparticles, and specifying the shear viscosity of the obtained composition, even the pigment (especially bright pigment) mixed with a high solid content is excellent in orientation, and the adhesion with the upper and lower coating films of the base coating film is excellent. Since the base coating composition of the present invention has a high solid content, it has excellent drying properties during coating, and does not disturb the mixing of the mixed bright pigment, so that a coating film with excellent appearance is formed.

[0028] The base coating composition of the present invention provides a coating film having excellent adhesion to the coating films above and below the coating film and having excellent design properties with few defects such as coating film peeling, etc., to the coated object. DETAILED DESCRIPTION

[0029] The base coating composition of the present invention is characterized in that it contains a pigment (A), a hydroxyl-containing acrylic resin (B), a blocked isocyanate compound (C), polymer crosslinked fine particles (D) that are insoluble in the above-mentioned hydroxyl-containing acrylic resin (B) and stably dispersed, and an acrylic resin (E) having a weight average molecular weight different from that of the hydroxyl-containing acrylic resin (B), wherein the solid content is a high solid content of 35% by mass or more, and when the viscosity V1 is measured at a shear rate of 0.1 / sec at 23°C using a cone and plate viscometer, the shear rate is changed from 0.1 / sec to 25000 / sec for 30 seconds, and then the shear is restored to 0.1 / sec, and when the viscosity V2 after shearing for 1 second is measured, the ratio of V2 to V1, that is, the viscosity recovery rate V2 / V1, is 90% or more. Furthermore, the pigment (A) contains at least one selected from a coloring pigment and a flaky pigment, the hydroxyl-containing acrylic resin (B) is a polymer of at least one monomer containing a hydroxyl-containing monomer (b), the hydroxyl-containing monomer (b) is a lactone-modified monoester compound of (meth)acrylic acid and a diol having 2 to 8 carbon atoms, the hydroxyl-containing acrylic resin (B) has a weight average molecular weight of 10,000 to 20,000, a glass transition temperature of 10° C. to 40° C., and a hydroxyl value of 10 mgKOH / g to 50 mgKOH / g, and the acrylic resin (E) needs to have a weight average molecular weight of 3,000 to 7,500.

[0030] By using the base coating composition having such requirements, it is possible to obtain a base coating film having excellent adhesion and water resistance and having little unevenness in the coating film with high design even if the base coating composition has a high solid content.

[0031] Hereinafter, the base coating composition and the coated article according to the embodiment of the present invention will be described in detail.

[0032] [Base coating composition]

[0033] The base coating composition according to an embodiment of the present invention contains a pigment (A), a hydroxyl-containing acrylic resin (B), a blocked isocyanate compound (C), polymer crosslinked fine particles (D) that are insoluble in the hydroxyl-containing acrylic resin (B) and stably dispersed, and an acrylic resin (E) having a weight average molecular weight different from that of the hydroxyl-containing acrylic resin (B).

[0034] (1) Pigment (A)

[0035] The pigment (A) contains one or more selected from the group consisting of coloring pigments and flaky pigments.

[0036] Examples of the coloring pigment include organic azo chelate pigments, insoluble azo pigments, condensed azo pigments, diketopyrrolopyrrole pigments, benzimidazolone pigments, phthalocyanine pigments, indigo pigments, perylene pigments, perylene pigments, dioxane pigments, quinacridone pigments, isoindolinone pigments, and metal complex pigments. Examples of the inorganic pigments include chrome yellow, yellow iron oxide, red iron oxide, carbon black, and titanium dioxide.

[0037] Examples of flaky pigments include metal flakes, metal oxide flakes, pearlescent pigments, and mica. Examples of metal flakes include aluminum, chromium, gold, silver, copper, brass, titanium, nickel, nickel-chromium, and stainless steel. Examples of metal oxide flakes include oxides of metal flakes, such as aluminum oxide and chromium oxide.

[0038] In the case where the base coating composition contains a flaky pigment, a metallic luster can be imparted to the base coating film. As described later, the color tone changes more significantly depending on the angle at which the base coating film is observed, that is, a base coating film with high flip-flop properties (hereinafter sometimes referred to as "FF properties") can be formed.

[0039] In order to easily prevent the metal sheet, metal oxide sheet, pearlescent pigment, etc. from reacting with water to generate gas, a metal film, such as a film of a metal compound such as molybdic acid, chromic acid, yttrium, and rare earth metals, or an organic polymer film, such as an organic polymer film obtained using a polymerizable monomer, may be formed on the metal sheet, metal oxide sheet, and pearlescent pigment. For example, the metal sheet, metal oxide sheet, and pearlescent pigment may have a film containing silicon dioxide, zirconium oxide, aluminum oxide, chromium oxide, polymerized synthetic resin, vanadium oxide, molybdenum oxide and / or molybdenum peroxide, phosphate, phosphite, borate, chromate, or a mixture or combination thereof. It should be noted that, for example, in the case of using chromium oxide, the toxicity can be removed by using a substance that makes it chemically inert.

[0040] The flaky pigment may contain a vapor-deposited metal pigment. Such flaky pigments are usually obtained by vapor-depositing a metal film (metal oxide film) on a base film, peeling off the base film, and then crushing the vapor-deposited metal film to make a metal sheet (metal oxide sheet). As the vapor-deposited metal material, for example, the materials described above for the metal sheet and the metal oxide sheet can be used. In this method, the flaky pigment is preferably a vapor-deposited aluminum pigment, a vapor-deposited chromium pigment, a vapor-deposited aluminum oxide pigment or a vapor-deposited chromium oxide pigment. For the vapor-deposited metal pigment, the above-mentioned film can also be formed on its surface as needed.

[0041] Examples of commercially available flaky pigments include METALURE (registered trademark) series, SILVERSHINE (registered trademark) series, HYDROSHINE (registered trademark) series, LiquidBlack (registered trademark), PLISMATIC (registered trademark) series manufactured by ECKART, FD series, GX series, and BS series manufactured by Asahi Kasei Chemicals, and 46 series and 63 series manufactured by Toyo Aluminum. Two or more pigments (A) may be used in combination.

[0042] The content of the pigment (A) is not particularly limited, and for example, the pigment concentration of the pigment (A), that is, the mass ratio of the pigment (A) to the resin solid content of the base coating composition, may be 1% by mass or more and 20% by mass or less. The resin solid content of the base coating composition refers to the resin component, the blocked isocyanate compound (C) and other curing agents that may be included.

[0043] The base coating composition may contain an extender pigment. Examples of the extender pigment include calcium carbonate, barium sulfate, clay, and talc.

[0044] When using an extender pigment, one may be used alone or two or more may be used in combination. When the base coating composition contains an extender pigment, the content of the extender pigment, for example, the mass ratio of the extender pigment to the resin solid content of the base coating composition may be 0.1% by mass or more and 20% by mass or less.

[0045] (2) Hydroxyl-containing acrylic resin (B)

[0046] The hydroxyl-containing acrylic resin (B) is a polymer containing one or more monomers of a hydroxyl-containing monomer (b), wherein the hydroxyl-containing monomer (b) is a lactone-modified monoester compound of (meth)acrylic acid and a divalent alcohol having a carbon number of 2 to 8. In addition, the hydroxyl-containing acrylic resin (B) has a weight average molecular weight of 10,000 to 20,000, a glass transition temperature of 10° C. to 40° C., and a hydroxyl value of 10 mgKOH / g to 50 mgKOH / g.

[0047] By containing a hydroxyl-containing acrylic resin (B), even if the solid content of the base coating composition is as high as 35% by mass or more, the coating viscosity will not be too high, so the unevenness of the coating film can be reduced. Furthermore, when the base coating composition contains flaky pigments, the orientation of the flaky pigments becomes less likely to be disordered, so that excellent FF properties (mutation: the property of the light and dark of the coating surface changing according to the observation angle) can be obtained. The upper limit of the solid content of the base coating composition is not particularly limited, for example, it can be 60% by mass.

[0048] Furthermore, the hydroxy-containing acrylic resin (B) is polymerized with a lactone modified body of a monoester compound of (meth) acrylic acid and a diol having a carbon number of 2 to 8, i.e., a hydroxy-containing monomer (b), and thus has a long chain structure in the side chain, and the long chain structure has a hydroxyl group. Thus, the reactivity with the isocyanate compound (C) as a curing agent can be improved, and the adhesion between the object to be coated and the base coating film, or the adhesion between the middle coating film or the bottom coating film provided on the object to be coated and the base coating film can be improved. For example, in the case where the object to be coated is made of plastic, the base coating composition of an embodiment of the present invention can form a base coating film having good adhesion to the object to be coated even if a bottom coating film is not provided on the object to be coated.

[0049] The hydroxyl-containing acrylic resin (B) is obtained by polymerizing one or more monomers including a hydroxyl-containing monomer (b) according to a conventional method.

[0050] Examples of the hydroxyl group-containing monomer (b) include lactone-modified products obtained by modifying monoesters of (meth)acrylic acid such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate with a diol having 2 to 8 carbon atoms with a lactone such as ε-caprolactone.

[0051] The "(meth)acrylic acid" in this specification means both acrylic acid and methacrylic acid.

[0052] The hydroxyl-containing acrylic resin (B) may be a polymer of a hydroxyl-containing monomer (b) and other monomers other than the hydroxyl-containing monomer (b). In this embodiment, the hydroxyl-containing acrylic resin (B) is obtained by polymerizing a monomer mixture of the hydroxyl-containing monomer (b) and the above-mentioned other monomers. In the total of the hydroxyl-containing monomer (b) and the other monomers, the hydroxyl-containing monomer (b) is preferably 5% by mass or more and 20% by mass or less.

[0053] Examples of other monomers other than the hydroxyl group-containing monomer (b) include acid group-containing monomers such as acrylic acid, methacrylic acid, acrylic acid dimer, crotonic acid, 2-acryloyloxyethyl phthalate, 2-acryloyloxyethyl succinate, ω-carboxy-polycaprolactone mono(meth)acrylate, isocrotonic acid, α-hydro-ω-(((1-oxo-2-propenyl)oxy)poly(oxy(1-oxo-1,6-hexanediyl)), maleic acid, fumaric acid, itaconic acid, 3-vinylsalicylic acid, 3-vinyl acetylsalicylic acid, 2-acryloyloxyethyl acid phosphate, and 2-acrylamido-2-methylpropanesulfonic acid.

[0054] In addition, examples of other monomers other than the hydroxyl-containing monomer (b) include (meth)acrylates (e.g., methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl methacrylate, phenyl acrylate, isobornyl (meth)acrylate, cyclohexyl methacrylate, tert-butylcyclohexyl (meth)acrylate, dicyclopentadienyl (meth)acrylate, dihydrodicyclopentadienyl (meth)acrylate, etc.), polymerizable aromatic compounds (e.g., styrene, α-methylstyrene, vinyl ketone, tert-butylstyrene, p-chlorostyrene, vinylnaphthalene, etc.), polymerizable nitriles (e.g., acrylonitrile, methacrylonitrile, etc.), α-olefins (e.g., ethylene, propylene, etc.), vinyl esters (e.g., vinyl acetate, vinyl propionate, etc.), dienes (e.g., butadiene, isoprene, etc.), etc. From the viewpoint of improving water resistance, styrene is preferably used.

[0055] Furthermore, examples of other monomers other than the hydroxyl group-containing monomer (b) include hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, allyl alcohol, and methallyl alcohol.

[0056] The hydroxyl group-containing monomer (b) may be used alone or in combination of two or more thereof. In addition, monomers other than the hydroxyl group-containing monomer (b) may be used alone or in combination of two or more thereof.

[0057] The weight average molecular weight of the hydroxyl group-containing acrylic resin (B) may be, for example, 10,000 or more and 20,000 or less.

[0058] The weight average molecular weight can be determined, for example, by gel permeation chromatography (GPC) using polystyrene as a standard.

[0059] The glass transition temperature of the hydroxyl group-containing acrylic resin (B) may be, for example, 10° C. or higher and 40° C. or lower.

[0060] The glass transition temperature can be measured or calculated by a known method. For example, the glass transition temperature can be measured using a differential scanning calorimeter (DSC) according to JIS K 7121.

[0061] The hydroxyl value of the hydroxyl-containing acrylic resin (B) may be, for example, 10 mgKOH / g or more and 50 mgKOH / g or less. Also, the acid value of the hydroxyl-containing acrylic resin (B) may be, for example, 0.2 mgKOH / g or more and 20 mgKOH / g or less.

[0062] The hydroxyl value and the acid value can be measured or calculated by a known method. For example, the hydroxyl value and the acid value can be measured according to JISK 0070:1992.

[0063] Two or more hydroxyl-containing acrylic resins (B) may be used in combination. The content of the hydroxyl-containing acrylic resin (B) in the base coating composition is not particularly limited, and for example, may be 30% by mass or more and 70% by mass or less, 40% by mass or more and 60% by mass or less in the resin solid content of the base coating composition.

[0064] (3) Blocked isocyanate compound (C)

[0065] By using the blocked isocyanate compound (C) together with the hydroxyl-containing acrylic resin (B), the adhesion between the object to be coated and the base coating film, or the adhesion between the intermediate coating film or the bottom coating film provided on the object to be coated and the base coating film can be improved. In addition, by crosslinking the base coating film, the coating film physical properties are improved, and the water resistance is improved.

[0066] The blocked isocyanate compound (C) can be prepared by blocking polyisocyanate with a blocking agent.

[0067] Examples of the polyisocyanate include aliphatic diisocyanates such as hexamethylene diisocyanate (including trimers), pentamethylene diisocyanate, tetramethylene diisocyanate, and trimethylhexamethylene diisocyanate; alicyclic polyisocyanates such as isophorone diisocyanate and 4,4'-methylenebis(cyclohexyl isocyanate); aromatic diisocyanates such as 4,4'-diphenylmethane diisocyanate, toluene diisocyanate, and xylylene diisocyanate; and modified products of these diisocyanates (carbamate-modified products, carbodiimides, uretdiones, uretonimines, biuret and / or isocyanurate-modified products, etc.).

[0068] As the end-capping agent, there can be mentioned, for example, monovalent alkyl (or aromatic) alcohols such as n-butanol, n-hexanol, 2-ethylhexanol, lauryl alcohol, phenol methanol, methyl phenyl methanol, etc.; cellosolves such as ethylene glycol monohexyl ether and ethylene glycol mono-2-ethylhexyl ether; polyether-type two-terminal diols such as polyethylene glycol, polypropylene glycol, polytetramethylene ether glycol phenol; polyester-type two-terminal polyols obtained from diols such as ethylene glycol, propylene glycol, 1,4-butanediol and dicarboxylic acids such as oxalic acid, succinic acid, adipic acid, suberic acid, sebacic acid; phenols such as p-tert-butylphenol and cresol; oximes such as dimethyl ketoxime, methyl ethyl ketoxime, methyl isobutyl ketoxime, methyl amyl ketoxime, cyclohexanone oxime; and lactams represented by ε-caprolactam and γ-butyrolactam. As the blocking agent, methyl diketone, methyl ketoester and methyl diester compounds, which are active hydrogen compounds, such as alkyl esters such as acetylacetone, ethyl acetoacetate and diethyl malonate can be used. In addition, blocked isocyanates formed using imidazole compounds and pyrazole compounds can also be used.

[0069] The blocking ratio of the blocked isocyanate compound (C) is preferably 100%, which advantageously improves the storage stability of the base coating composition.

[0070] The blocked isocyanate compound (C) may be used in combination of two or more types.

[0071] The content of the blocked isocyanate compound (C) is not particularly limited. From the viewpoint of more appropriately promoting the curing reaction, the ratio of the number of moles of isocyanate groups in the blocked isocyanate compound (C) to the number of moles of hydroxyl groups in the hydroxyl-containing acrylic resin (B) (NCO / OH) can be 0.2 / 1.0 to 0.6 / 1.0, preferably 0.3 / 1.0 to 0.5 / 1.0.

[0072] The base coating composition may contain other curing agents such as amino resins such as melamine resins, guanamine resins, and urea resins as curing agents other than the isocyanate compound (C). When other curing agents other than the isocyanate compound (C) are contained, the content of the other curing agent is, for example, 10 parts by mass or more and 30 parts by mass or less relative to 100 parts by mass of the resin solid content of the base coating composition.

[0073] (4) Polymer cross-linked microparticles (D)

[0074] The polymer cross-linked microparticles (D) are added as a viscosity modifier to contribute to the adjustment of viscosity described later. Usually, the coating is reduced in viscosity due to the shear force applied during coating, so the viscosity just after coating is lower than the viscosity before coating. Therefore, if the viscosity after coating is low, the coating sags downward, becoming the cause of uneven coating. The base coating composition of an embodiment of the present invention, by containing polymer cross-linked microparticles (D), can recover early and improve the viscosity of reduced viscosity during coating, can suppress the base coating composition applied on the coated object from sagging, and can reduce the unevenness of coating.

[0075] The polymer crosslinked microparticles (D) can be prepared by polymerizing a monomer mixture. The polymerization method may be any polymerization method as long as crosslinked microparticles can be obtained, and multi-stage polymerization may be used. More specifically, emulsion polymerization is preferably used.

[0076] Polymer cross-linked microparticles obtained by emulsion polymerization (D)

[0077] The polymer crosslinked microparticles (D) used in the present invention are prepared by emulsion polymerization of ethylenically unsaturated monomers and crosslinkable comonomers in an aqueous medium by a known method to form an emulsion containing crosslinked polymer microparticles, and removing water by solvent replacement, azeotropy, centrifugal separation, filtration, drying, etc. The emulsion polymerization can be carried out using a known emulsifier and / or dispersant, but it is preferred to use an emulsifier having a zwitterionic group. When the polymer crosslinked microparticles (D) are added to the coating composition, it is important to obtain a uniform particle size because the particle size and structural viscosity are different, but by using an emulsifier having a zwitterionic group, it is easy to obtain polymer crosslinked microparticles with a uniform particle size.

[0078] As the ethylenically unsaturated monomer used in the preparation of the polymer crosslinked microparticles (D), there are alkyl esters of acrylic acid or methacrylic acid such as methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, or other monomers having an ethylenically unsaturated bond copolymerizable therewith, such as styrene, α-methylstyrene, vinyltoluene, tert-butylstyrene, ethylene, propylene, vinyl acetate, vinyl propionate, acrylonitrile, methacrylonitrile, dimethylaminoethyl (meth)acrylate, etc. Two or more of these monomers may be used.

[0079] The crosslinkable comonomer includes a monomer having two or more free-radically polymerizable ethylenically unsaturated bonds in the molecule and / or two types of ethylenically unsaturated group-containing monomers each carrying a group that can react with each other.

[0080] Examples of monomers having two or more free-radically polymerizable ethylenically unsaturated groups in the molecule include polymerizable unsaturated monocarboxylic acid esters of polyhydric alcohols, polymerizable unsaturated alcohol esters of polybasic acids, and aromatic compounds substituted with two or more vinyl groups. Examples thereof include the following compounds.

[0081] Ethylene glycol diacrylate, ethylene glycol dimethacrylate, triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, 1,3-butylene glycol dimethacrylate, trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, 1,4-butylene glycol diacrylate, neopentyl glycol diacrylate, 1,6-hexanediol diacrylate, pentaerythritol diacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, pentaerythritol dimethacrylate, pentaerythritol trimethacrylate, pentaerythritol tetramethacrylate, glycerol dimethacrylate, glycerol diacrylate, glycerol acryloxy dimethacrylate Esters, 1,1,1-trihydroxymethylethane diacrylate, 1,1,1-trihydroxymethylethane triacrylate, 1,1,1-trihydroxymethylethane dimethacrylate, 1,1,1-trihydroxymethylethane trimethacrylate, 1,1,1-trihydroxymethylpropane diacrylate, 1,1,1-trihydroxymethylpropane triacrylate, 1,1,1-trihydroxymethylpropane dimethacrylate, 1,1,1-trihydroxymethylpropane trimethacrylate, triallyl cyanurate, triallyl isocyanurate, triallyl trimellitate, diallyl terephthalate, diallyl phthalate and divinylbenzene.

[0082] In addition, as a crosslinking purpose monomer, it is also possible to replace a monomer having more than two ethylenically unsaturated groups that can be free radically polymerized in the molecule, or to use two monomers with ethylenically unsaturated groups that carry groups that can react with each other as needed. For example, ethylenically unsaturated monomers containing glycidyl groups such as glycidyl methacrylate and glycidyl acrylate and ethylenically unsaturated monomers containing carboxyl groups such as acrylic acid, methacrylic acid, and crotonic acid can be cited; 2-hydroxyethyl acrylate, hydroxypropyl acrylate, 2-hydroxyethyl methacrylate, hydroxypropyl methacrylate, hydroxybutyl acrylate, hydroxybutyl methacrylate, allyl alcohol, methylallyl alcohol and ethylenically unsaturated monomers containing hydroxy groups such as vinyl isocyanate and isopropenyl isocyanate have isocyanate groups, etc. Unsaturated monomers. However, in addition to this, two ethylenically unsaturated monomers carrying any combination of groups that can react with each other can also be used.

[0083] The monomers constituting the polymer cross-linked particles (D) may contain monomers having functional groups capable of reacting with a cross-linking agent, examples of which include carboxyl-containing monomers such as acrylic acid, methacrylic acid, crotonic acid, itaconic acid, maleic acid, fumaric acid, and the like, hydroxyl-containing monomers such as 2-hydroxyethyl acrylate, hydroxypropyl acrylate, 2-hydroxyethyl methacrylate, hydroxypropyl methacrylate, hydroxybutyl acrylate, hydroxybutyl methacrylate, allyl alcohol, methallyl alcohol, nitrogen-containing acrylamide, methacrylamide, and the like.

[0084] Polymerizable crosslinked particles (D) obtained by non-aqueous dispersion polymerization

[0085] The monomer mixture used in the preparation of the polymer crosslinked microparticles (D) contains a free radical polymerizable monomer. The above-mentioned monomer mixture may contain: a free radical polymerizable unsaturated monomer having a side chain containing a higher unsaturated aliphatic group. The monomer mixture contains a free radical polymerizable unsaturated monomer having a side chain containing a higher unsaturated aliphatic group, which has the advantage that the polymer crosslinked microparticles can be appropriately prepared.

[0086] As the above-mentioned free radical polymerizable unsaturated monomer with a side chain containing a high-level unsaturated aliphatic group, for example, a monomer obtained by the reaction of a high-level unsaturated fatty acid with an ethylenically unsaturated glycidyl ester can be cited. As the above-mentioned high-level unsaturated fatty acid, myristoleic acid, palmitoleic acid, oleic acid, linoleic acid, linolenic acid, ricinoleic acid, etc. can be used. In addition, linseed oil fatty acid, safflower oil fatty acid, soybean oil fatty acid, rice bran oil fatty acid, sesame oil fatty acid, castor oil fatty acid, dehydrated castor oil fatty acid, perilla oil fatty acid, hemp seed oil fatty acid, cottonseed oil fatty acid, tall oil fatty acid, etc. can be used. Dry oils, semi-drying oil fatty acids, etc. contain unsaturated fatty acids such as oleic acid, linoleic acid, linolenic acid, eleostearic acid or ricinoleic acid. The average carbon number of the high-level unsaturated aliphatic group is preferably 13 or more and 23 or less. In addition, fatty acids with conjugated double bonds such as tung oil fatty acids can also be used in combination with an amount of 30% by mass or less relative to all saturated fatty acids. In addition, as the above-mentioned ethylenically unsaturated glycidyl ester, glycidyl acrylate, glycidyl methacrylate, methyl glycidyl acrylate, methyl glycidyl methacrylate, allyl glycidyl ether, methyl allyl glycidyl ether, etc. can be used. Among these, it is particularly preferred that the substance obtained by the reaction of at least one selected from oleic acid, linoleic acid, linolenic acid, safflower oil fatty acid, soybean oil fatty acid, castor oil fatty acid, dehydrated castor oil fatty acid, and tall oil fatty acid with glycidyl acrylate and / or glycidyl methacrylate. In addition, as the above-mentioned free radical polymerizable unsaturated monomer, the iodine value is preferably 60 or more and 180 or less, and particularly preferably 70 or more and 150 or less.

[0087] Examples of other radically polymerizable unsaturated monomers other than the radically polymerizable unsaturated monomer having a side chain containing a higher unsaturated aliphatic group contained in the monomer mixture include:

[0088] Acrylate monomers such as methyl acrylate, ethyl acrylate, n-propyl acrylate, n-butyl acrylate, isobutyl acrylate, tert-butyl acrylate, n-hexyl acrylate, n-octyl acrylate, isooctyl acrylate, 2-ethylhexyl acrylate, isononyl acrylate, stearyl acrylate, cyclohexyl acrylate, benzyl acrylate, etc.;

[0089] Methacrylate monomers such as methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, tert-butyl methacrylate, n-hexyl methacrylate, n-octyl methacrylate, isooctyl methacrylate, 2-ethylhexyl methacrylate, isononyl methacrylate, n-dodecyl methacrylate, isododecyl methacrylate, stearyl methacrylate, cyclohexyl methacrylate, benzyl methacrylate, etc.;

[0090] Aromatic vinyl monomers such as styrene, vinyl toluene, ethyl vinyl benzene, etc.

[0091] Carboxyl-containing monomers such as acrylic acid, methacrylic acid, itaconic acid, maleic acid, maleic anhydride, fumaric acid, crotonic acid, and citraconic acid;

[0092] Acrylamide, methacrylamide, N,N-dimethylacrylamide, N-methylacrylamide, N-n-butoxymethylacrylamide and other monomers containing amide groups or substituted amide groups;

[0093] Hydroxyl-containing monomers such as 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, allyl alcohol, and methallyl alcohol;

[0094] Aminoethyl acrylate, N,N-dimethylaminoethyl acrylate, N,N-diethylaminoethyl acrylate, N,N-dimethylaminoethyl methacrylate, N,N-diethylaminoethyl methacrylate and other amino group-containing or substituted amino group-containing monomers;

[0095] Epoxy-containing monomers such as glycidyl methacrylate, glycidyl acrylate, glycidyl allyl ether, glycidyl methyl allyl ether, and glycidyl vinyl ether;

[0096] Monomers containing thiol groups, such as vinyl mercaptan and allyl mercaptan;

[0097] Monomers having two or more free radical polymerizable unsaturated groups in one molecule, such as (poly)ethylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, allyl (meth)acrylate, triallyl cyanurate, triallyl isocyanurate, diallyl phthalate, and divinylbenzene; etc.

[0098] Among the above-mentioned other free radical polymerizable unsaturated monomers, it is preferred to contain one or more selected from, for example, acrylate monomers (preferably ethyl acrylate, n-butyl acrylate, etc.), methacrylate monomers (preferably methyl methacrylate, n-butyl methacrylate, etc.), carboxyl group-containing monomers (preferably acrylic acid, methacrylic acid, ω-carboxyl-polycaprolactone monoacrylate, etc.), and substituted amino group-containing monomers (preferably N,N-dimethylaminoethyl acrylate, N,N-diethylaminoethyl methacrylate, etc. N,N-di-lower alkylamino-lower alkyl (meth)acrylates, etc.).

[0099] Relative to the total amount of 100 parts by mass of the monomer mixture, the amount of the free radical polymerizable unsaturated monomer having a side chain containing a higher unsaturated aliphatic group contained in the above-mentioned monomer mixture is preferably in the range of 0.5 parts by mass to 30 parts by mass, and more preferably in the range of 5 parts by mass to 15 parts by mass. In addition, relative to the total amount of 100 parts by mass of the monomer mixture, the total amount of the acrylate monomer and the methacrylate monomer contained in the above-mentioned monomer mixture is preferably in the range of 50 parts by mass to 90 parts by mass. In addition, the amount of the carboxyl group-containing monomer contained in the above-mentioned monomer mixture is preferably in the range of 10 parts by mass or less. Furthermore, the amount of the substituted amino group-containing monomer contained in the above-mentioned monomer mixture is preferably in the range of 10 parts by mass or less. It should be noted that when the preparation of the polymer crosslinked microparticles (D) of the present invention is carried out by multistage polymerization, the amount of the monomer contained in the above-mentioned monomer mixture is the total amount of the monomers used in each polymerization.

[0100] The polymerization conditions for preparing the polymer crosslinked microparticles (D) can be appropriately selected according to the type and amount of the monomers used, and the polymerization conditions commonly used by those skilled in the art can be carried out. For example, it is preferred to use an appropriate polymerization initiator and a chain transfer agent used as needed, and heat the reaction for several hours while stirring in a nitrogen stream or at the reflux temperature of an organic solvent to polymerize the above-mentioned monomer mixture to reach the range of the weight average molecular weight described below. The polymerization temperature is generally 30°C to 180°C, preferably 60°C to 150°C.

[0101] Examples of the organic solvent used in the polymerization include:

[0102] Cyclohexane, methylcyclohexane, cycloheptane, methylcycloheptane, "Lowes", "Mineral Spirit EC", "Shellsol 71", "VM&P Naphtha", "Shell TS28 Solvent" [all manufactured by Shell Moss], "Isopar C", "Isopar E", "Isopar G", "Isopar H", "Isopar M", "Naphtha No. 3", "Naphtha No. 5", "Naphtha No. 6", "Solvent 7" (all manufactured by Exxon Chemical), "IP Solvent 1016", "IPSolvent 1620", "IP Solvent 2028", "IP Solvent 2835" [all manufactured by Idemitsu Kosan Co., Ltd.], "White Sol" [manufactured by Japan Energy Co., Ltd.], "Mitsubishi Mineral Turpen", "Diamond Solvent", "PEGASOL AN-45", "PEGASOL 3040" [all manufactured by JXTG Energy Co., Ltd.] and other aliphatic or alicyclic hydrocarbon solvents;

[0103] Aromatic hydrocarbon organic solvents such as benzene, toluene, ethylbenzene, propylbenzene, tert-butylbenzene, o-xylene, m-xylene, p-xylene, tetralin, decalin, "SOLVESSO 100" (manufactured by Exxon Chemical Co.), and "SOLVESSO 150" (manufactured by Exxon Chemical Co.);

[0104] Ketone organic solvents such as acetone, acetylacetone, methyl ethyl ketone, methyl isobutyl ketone, methyl amyl ketone, and cyclohexanone;

[0105] Ester organic solvents such as methyl acetate, ethyl acetate, n-butyl acetate, and amyl acetate;

[0106] Cellosolve organic solvents such as methyl cellosolve, ethyl cellosolve, n-propyl cellosolve, isopropyl cellosolve, n-butyl cellosolve, isobutyl cellosolve, isopentyl cellosolve, phenyl cellosolve, and benzyl cellosolve;

[0107] Carbitol organic solvents such as methyl carbitol, ethyl carbitol, n-propyl carbitol, isopropyl carbitol, n-butyl carbitol, isobutyl carbitol, isopentyl carbitol, phenyl carbitol, and benzyl carbitol; etc.

[0108] As the above-mentioned polymerization initiator, for example, organic peroxides such as benzoyl peroxide, lauroyl peroxide, caproyl peroxide, diisopropyl peroxydicarbonate, di-2-ethylhexyl peroxydicarbonate, and tert-butyl peroxypivalate can be cited; azo compounds such as 2,2'-azobisisobutyronitrile, 2,2'-azobis-2,4-dimethylvaleronitrile, 2,2'-azobis-4-methoxy-2,4-dimethylvaleronitrile, etc. can be used alone or in combination of two or more. The usage amount of the above-mentioned polymerization initiator is generally preferably 0.5 mass parts or less and 15 mass parts or less, and more preferably 2 mass parts or less and 8 mass parts or less relative to 100 mass parts of the total monomer amount.

[0109] When the polymer crosslinked fine particles (D) of the present invention are prepared by multi-stage polymerization, the above-mentioned preferred range of the amount of the polymerization initiator used can be applied to each polymerization.

[0110] In the preparation of the polymer crosslinked microparticles (D), when the monomer mixture is subjected to a two-stage polymerization, in the initial polymerization stage, a monomer mixture containing a radically polymerizable unsaturated monomer having a side chain containing a higher unsaturated aliphatic group may be copolymerized to form a soluble portion, and then a monomer mixture not containing a radically polymerizable unsaturated monomer having a side chain containing a higher unsaturated aliphatic group or a monomer mixture containing a radically polymerizable unsaturated monomer having a side chain containing a higher unsaturated aliphatic group may be copolymerized to form a particle portion.

[0111] When the polymer crosslinked fine particles (D) have a soluble part and a particle part, for example, the weight average molecular weight of the soluble part may be 15,000 to 100,000, and the particle part is preferably crosslinked by a monomer having two or more polymerizable unsaturated groups.

[0112] The weight average molecular weight can be determined, for example, by gel permeation chromatography (GPC) using polystyrene as a standard.

[0113] When the polymer crosslinked fine particles (D) have a soluble portion and a granular portion, the mass ratio of the soluble portion to the granular portion is preferably in the range of soluble portion:granular portion = 20:80 to 80:20, more preferably in the range of 30:70 to 70:30.

[0114] As another example of the preparation of the polymer crosslinked microparticles (D), a monomer mixture containing no radical polymerizable unsaturated monomer having a side chain containing a higher unsaturated aliphatic group is polymerized to introduce a side chain containing a higher unsaturated aliphatic group into the obtained copolymer. Specifically, for example, a side chain containing a higher unsaturated aliphatic group can be introduced by polymerizing a monomer mixture containing an alkylene group-containing monomer and then reacting a carboxyl group of a higher unsaturated fatty acid with an alkylene group contained in the obtained copolymer.

[0115] The amount of the polymer crosslinked microparticles (D) in the base coating composition is usually 5 to 40 parts by mass, preferably 10 to 30 parts by mass, relative to 100 parts by mass of the total solid content of the hydroxyl-containing acrylic resin (B), the blocked isocyanate compound (C) and the acrylic resin (E). If the amount of the polymer crosslinked microparticles (D) is too small, the base coating composition has a large penetration into the underlying coating composition in the case of easy dripping and wet-on-wet coating, and the initial purpose cannot be achieved. On the other hand, when the amount is too large, the coating performance is reduced, the smoothness of the film is impaired, and a high finished appearance cannot be obtained.

[0116] Examples of commercially available products of the polymer crosslinked fine particles (D) include Setalux 1 801, 1850, SA-50, and 53 (manufactured by Allnex Corporation).

[0117] (5) Acrylic resin (E)

[0118] The base coating composition contains an acrylic resin (E) having a weight average molecular weight of 3000 to 7500. This makes it easier to adjust the viscosity of the base coating composition.

[0119] The acrylic resin (E) can be obtained by polymerizing an α,β-ethylenically unsaturated monomer. For example, the above-mentioned α,β-ethylenically unsaturated monomers can be used as the hydroxyl-containing acrylic resin (B).

[0120] The weight average molecular weight of the acrylic resin (E) is preferably 3500 or more, more preferably 4000 or more, and is preferably 6500 or less, further preferably 5500 or less.

[0121] The weight average molecular weight can be determined, for example, by gel permeation chromatography (GPC) using polystyrene as a standard.

[0122] The hydroxyl value of the acrylic resin (E) may be, for example, 40 mgKOH / g or more. Also, the acid value of the acrylic resin (E) may be, for example, 0.1 mgKOH / g or more and 20 mgKOH / g or less.

[0123] The hydroxyl value and the acid value can be measured or calculated by a known method. For example, the hydroxyl value and the acid value can be measured according to JIS K0070:1992.

[0124] The acrylic resin (E) may be used in combination of two or more types.

[0125] When an acrylic resin (E) is contained, the content of the acrylic resin (E) is not particularly limited, and can be, for example, 10% by mass or more and 50% by mass or less in the resin solid content of the base coating composition. If the amount of the acrylic resin (E) is too small, the viscosity of the coating becomes high, causing disadvantages during coating. If the amount of the acrylic resin (E) is too large, the viscosity decreases, but the physical properties of the coating film decrease, and the adhesion and water resistance performance decrease.

[0126] (6) Base coating composition

[0127] The base coating composition may contain an organic solvent.

[0128] Examples of such organic solvents include ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and methyl amyl ketone; esters such as ethyl acetate, butyl acetate, amyl acetate, methyl benzoate, ethyl ethoxypropionate, ethyl propionate, and methyl propionate; ethers such as tetrahydrofuran, dioxane, and dimethoxyethane; glycol ethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, and 3-methoxybutyl acetate; aromatic hydrocarbons, aliphatic hydrocarbons, and the like.

[0129] The base coating composition of the present invention may contain a curing catalyst, a viscosity modifier other than the polymer crosslinked fine particles (D), a defoamer, an ultraviolet absorber, a light stabilizer (such as a hindered amine), an antioxidant, a surface modifier, a film-forming aid, a rust inhibitor, and the like.

[0130] The method for producing the base coating composition is not particularly limited, and a method known in the art such as stirring, kneading or dispersing the above-mentioned materials using a dispenser, homogenizer, roll, sand mill or kneader can be used.

[0131] The base coating composition of the present invention is characterized in that, after measuring the viscosity V1 at 0.1 / sec shearing at 23°C using a cone-plate viscometer, the viscosity V2 is measured after shearing for 30 seconds from 0.1 / sec to 25,000 / sec, and then restored to 0.1 / sec after shearing for 1 second, the ratio of V2 to V1, i.e., the viscosity recovery rate V2 / V1, is 90% or more. The higher the viscosity recovery rate V2 / V1, the better. The viscosity recovery rate indicates the ratio of the viscosity at the moment of weak shearing to the viscosity at the moment of strong shearing, and a high viscosity recovery indicates that the viscosity is immediately recovered even after coating. The viscosity of the base coating composition of the present invention will recover rapidly even after coating.

[0132] [Painted items]

[0133] The coated article according to the embodiment of the present invention includes an object to be coated and a base coating film formed from the base coating composition according to the embodiment of the present invention.

[0134] The coated article according to the embodiment of the present invention may include a multilayer coating film including a middle coating film or a primer coating film provided on the coated object, a base coating film provided on the middle coating film or the primer coating film, and a clear coating film provided on the base coating film.

[0135] In a certain embodiment, the coated article of the embodiment of the present invention may not have a middle coating film or a bottom coating film, and a base coating film is provided on the coated object. That is, in this mode, the coated article of the embodiment of the present invention may include a multilayer coating film, and the multilayer coating film includes a base coating film provided on the coated object and a clear coating film provided on the base coating film.

[0136] For example, when the object to be coated is made of plastic, the base coating composition according to the embodiment of the present invention can form a base coating film having good adhesion to the object to be coated even without providing a primer coating film on the object to be coated.

[0137] (1) Object to be coated

[0138] The object to be coated is not particularly limited, and examples thereof include metal substrates, plastic substrates, and foams thereof.

[0139] As the metal substrate, for example, metals such as iron, steel, copper, aluminum, tin, zinc and alloys containing these metals can be cited. As the metal substrate, specifically, automobile bodies such as cars, trucks, motorcycles, buses and parts for automobile bodies can be cited. Such metal substrates are preferably preformed with electrodeposition coatings. In addition, before forming the electrodeposition coating, chemical conversion treatment (such as zinc phosphate chemical conversion treatment, zirconium chemical conversion treatment, etc.) can be carried out as needed.

[0140] Examples of the plastic substrate include polypropylene resin, polycarbonate resin, polyurethane resin, polyester resin, polystyrene resin, ABS resin, vinyl chloride resin, polyamide resin, etc. Specifically, examples of the plastic substrate include automotive parts such as spoilers, bumpers, mirror covers, grilles, and door handles. These plastic substrates are preferably degreased with a solvent such as petroleum light distillate oil or isopropyl alcohol or washed with pure water and / or a neutral detergent.

[0141] (2) Middle coating and bottom coating

[0142] When the object to be coated is a metal substrate, a middle coating film can be provided on the metal substrate on which the electrodeposition coating is formed. In addition, when the object to be coated is a plastic substrate, a base coating film can be provided on the plastic substrate.

[0143] The intermediate coating film and the primer coating film are not particularly limited, and can be formed using, for example, an intermediate coating composition or a primer coating composition containing a coating film-forming resin and, if necessary, a curing agent, etc., respectively.

[0144] (3) Transparent coating

[0145] A clear coating film may be provided on the base coating film. The clear coating film is not particularly limited and may be formed using a clear coating composition containing a coating film forming resin and a curing agent as required. In addition, the clear coating film may contain a coloring component. The form of the clear coating composition is not particularly limited, but preferably a solvent-based one.

[0146] As a preferred example of a solvent-based clear coating composition, from the perspective of transparency or acid etching resistance, a combination of acrylic resin and / or polyester resin and amino resin and / or isocyanate, or acrylic resin and / or polyester resin having a carboxylic acid / epoxy curing system as a coating film forming resin can be cited. Furthermore, a two-component clear coating with isocyanate as a crosslinking agent is more preferred. In particular, a transparent isocyanate is infiltrated into the colored base coating layer and cured, thereby forming a multilayer coating film with excellent water resistance.

[0147] Examples of water-based clear coating compositions include those containing a resin made water-based by neutralizing the coating film-forming resin contained in the examples of solvent-based clear coating compositions with a base. The neutralization can be performed by adding a tertiary amine such as dimethylethanolamine and triethylamine before or after polymerization.

[0148] The clear coating composition may contain a viscosity control agent. Examples of the viscosity control agent include crosslinked or non-crosslinked resin particles, swollen dispersions of fatty acid amides, polyamide-based substances such as amide fatty acids and phosphates of long-chain polyaminoamides, polyethylene-based substances such as colloidal swollen dispersions of oxidized polyethylene, and organic acid smectite clays, organic bentonite-based substances such as montmorillonite, and the like.

[0149] The method for producing the coated article is not particularly limited, and the coated article can be produced, for example, by the method for producing a coated article according to the embodiment of the present invention described below.

[0150] [Method for producing coated article]

[0151] The base coating composition of the present invention is applied to the object to be coated by the same coating method as the usual base coating. The base coating composition is applied to the object to be coated with a middle coating film or a base coating film. In addition, a clear coating is applied on the base coating film to form a clear coating film. The coating film forming method may be a commonly used method, or a spray coater may be used to form an uncured coating film called a so-called wet on wet, and then 2 to 3 layers are cured at the same time.

[0152] There is no particular limitation on the coating method of the middle coating composition, the primer composition, the basic water-based coating composition, and the clear coating composition. Depending on the type of the object to be coated, for example, a coating method commonly used in the coating field such as air spray coating, electrostatic bell coating, multi-stage coating or single-stage coating based on air electrostatic spray coating, or a coating method combining air electrostatic spray coating and a rotary atomization electrostatic coating machine called an automatic metal electrostatic bell (metallic bell) can be used.

[0153] As the heating device for heat curing the uncured coating film, for example, a drying oven utilizing a heating source such as hot air, electricity, gas, infrared rays, etc. can be enumerated. In addition, if a drying oven using two or more of these heating sources in combination is used, the drying time is shortened, so it is preferred.

[0154] The coated article of the embodiment of the present invention can also be manufactured by heat-curing the coating film each time each coating composition is applied, and the coating film of the upper layer is formed in sequence. In addition, the coated article of the embodiment of the present invention can omit the process of forming the middle layer coating film and the bottom layer coating film, and is manufactured in a manner that does not include the middle layer coating film and the bottom layer coating film.

[0155] Example

[0156] Hereinafter, the present invention will be described in more detail using examples, but the present invention is not limited by the examples. In the examples, "parts" and "%" are all based on mass unless otherwise specified.

[0157] (Manufacturing Example 1) Manufacture of Hydroxyl-Containing Acrylic Resin (B-1)

[0158] 57 parts of butyl acetate were added to a reaction apparatus equipped with a stirring blade, a thermometer, a dropping device, a temperature control device, a nitrogen inlet and a condenser, and the temperature was raised to 120°C while introducing nitrogen. Next, a mixture of 0.5 parts of methacrylic acid, 53.1 parts of 2-ethylhexyl methacrylate, 18.1 parts of methyl methacrylate, 15.0 parts of styrene, 13.3 parts of lactone-modified 2-hydroxyethyl methacrylate and a solution obtained by dissolving 2.0 parts of tert-butyl peroxy-2-ethylhexanoate in 5 parts of butyl acetate were added dropwise to the reaction apparatus over 3 hours. After the addition was completed, the mixture was aged for 1 hour, and then a solution obtained by dissolving 0.2 parts of tert-butyl peroxy-2-ethylhexanoate in 5 parts of butyl acetate was added dropwise to the reaction apparatus over 1 hour, and aged for 2 hours while maintaining the temperature at 120°C to complete the reaction. The non-volatile content of the obtained hydroxy-containing resin was 60%, and the weight average molecular weight was 14500. In addition, the glass transition temperature is 20°C and the hydroxyl value is 30 mgKOH / g. Table 1 shows the blended monomer components, property values, the first and second stage amounts of the polymerization initiator (tert-butyl peroxy-2-ethylhexanoate), and the type of hydroxyl group (lactone modified or not).

[0159] (Manufacturing Examples 2 to 10) Manufacture of Hydroxyl-Containing Acrylic Resins (B-2 to B-10)

[0160] In the same reaction apparatus as in Preparation Example B-1, the hydroxyl-containing acrylic resins of Preparation Examples B-2 to B-10 were obtained by the same operation with the formulations shown in Table 1. In Table 1, the property values ​​and the like of the obtained hydroxyl-containing acrylic resins (B-2 to B-10) are also described.

[0161] [Table 1]

[0162]

[0163] (Manufacturing Examples 11 to 13) Manufacture of Acrylic Resins (E-1 to E-3)

[0164] In the same reaction apparatus as in the above-mentioned Production Example B-1, acrylic resins (E-1 to E-3) were obtained by the same operation with the formulation described in Table 2, and their characteristic values ​​(weight average molecular weight, heating residue, first-stage and second-stage polymerization initiator amounts) are recorded in Table 2.

[0165] [Table 2]

[0166]

[0167] Reference Example 1

[0168] Method for producing polyester resin having zwitterionic groups

[0169] In a 2Q flask equipped with a stirrer, a nitrogen inlet tube, a temperature control device, a condenser, and a decanter, 134 parts of bishydroxyethyltaurine, 130 parts of neopentyl glycol, 236 parts of azelaic acid, 186 parts of phthalic anhydride, and 27 parts of xylene were added and the temperature was raised. The water generated by the reaction was removed azeotropically with xylene. The temperature was brought to 190°C after about 2 hours from the start of reflux, and stirring and dehydration were continued until the acid value equivalent to carboxylic acid reached 145, and then cooled to 140°C.

[0170] Next, while maintaining the temperature at 140°C, 314 parts of "CARDURA E10" (tertiary carboxylic acid glycidyl ester manufactured by Shell) was added dropwise over 30 minutes, and then stirring was continued for 2 hours to terminate the reaction. The obtained polyester resin had an acid value of 59, a hydroxyl value of 90, and a Mn of 1,054.

[0171] (Production Example 14) Production Example of Polymer Crosslinked Microparticles D-1

[0172] 281 parts of deionized water, 30 parts of the polyester resin obtained in the above-mentioned Reference Example 1 and 3 parts of dimethylethanolamine were added to a 1L reaction container equipped with a stirrer, a condenser and a temperature control device, and dissolved while maintaining the stirring temperature at 80°C. A liquid obtained by dissolving 1.0 part of azobiscyanovaleric acid in 45 parts of deionized water and 0.9 parts of dimethylethanolamine was added thereto. Next, a mixed solution of 30 parts of n-butyl acrylate, 70 parts of styrene and 60 parts of ethylene glycol dimethacrylate was added dropwise over 60 minutes. After the dropwise addition, a substance obtained by dissolving 0.5 parts of azobiscyanovaleric acid in 15 parts of deionized water and 0.4 parts of dimethylethanolamine was further added, and stirring was continued at 80°C for 2 hours to obtain an emulsion with a non-volatile content of 40% and a particle size of 0.12μ. The emulsion was spray-dried to obtain polymer crosslinked microparticles.

[0173] The polymer crosslinked fine particles were dispersed in a solvent prepared by mixing methyl amyl ketone and xylene at a weight ratio of 1:1 using an ultrasonic disperser, and the heating residue was adjusted to 40% to obtain a stable dispersion solution of the polymer crosslinked particles.

[0174] (Production Example 15) Production Example of Polymer Crosslinked Microparticles D-2

[0175] An emulsion having a particle size of 0.20 μ was obtained by the same operation method as in the above-mentioned preparation example except that 5 parts of sodium di(2-ethylhexyl)sulfosuccinate was used instead of the polyester resin obtained in Reference Example 1. Similarly, the emulsion was spray-dried and ultrasonically dispersed in a mixed solvent, and the heating residue was adjusted to 50%.

[0176] <Examples 1 to 5 and Comparative Examples 1 to 12>

[0177] The base coating compositions of Examples 1 to 5 and Comparative Examples 1 to 12 were obtained by mixing and stirring the raw materials according to the compositions described in Tables 3 and 4 below (mixed with a colored base coating). It should be noted that the units of the compositions in the tables are parts by mass and are the solid content conversion amounts excluding the organic solvent. The amount of the polymer crosslinked fine particles (D) is expressed relative to 100 parts by mass of the total of the hydroxyl-containing acrylic resin (B), the blocked isocyanate compound (C) and the acrylic resin (E).

[0178] (Preparation of coating material)

[0179] The coatings of Examples 1 to 5 and Comparative Examples 1 to 12 were adjusted to a viscosity of 13 seconds in Ford Cup No. 4 at a coating temperature of 20° C. using methyl amyl ketone / Solvesso 100 = 1 / 1 (weight ratio) as a diluent. At this time, coatings with a non-volatile content of less than 35% were evaluated as ×, and those with a non-volatile content of more than 35% were evaluated as ○. In Tables 3 and 4, a column for solid content during coating was provided, and ○ and × were recorded. No other evaluation items were performed on coatings with a non-volatile content of less than 35%.

[0180] (Production of painted items)

[0181] The base coating of Example 1 was spray-coated (dry film thickness 25 μm) on the surface of an ABS resin substrate (70 mm×150 mm×3 mm) wiped with isopropyl alcohol under an environment of 25°C / 70% relative humidity (RH) using a spray gun "Wieda-71" (manufactured by Atestop Iwata Co., Ltd.) and left at room temperature for 5 minutes. On top of it, a clear coating composition (a mixture of R-2550-1 and hardener H-250 produced by NIPPON PAINT AUTOMOTIVE COATINGS CO., LTD.) was spray-coated (dry film thickness 25 μm) using ROBOBEL951 under coating conditions (gun distance: 200 mm, gun speed: 700 mm / s, rotation speed: 2500 rpm, shaping air pressure: 0.07 MPa). Then, after leaving for 10 minutes, it was dried at 80°C for 30 minutes to produce a coated article of Example 1.

[0182] Coated articles of Examples 2 to 5 and Comparative Examples 1 to 12 were obtained in the same manner as in Example 1 except that the base coating compositions of Examples 2 to 5 and Comparative Examples 1 to 12 shown in Tables 3 and 4 were used.

[0183] The obtained base coating composition and coated articles were used to evaluate unevenness (unevenness of coating film), adhesion, water resistance, coating film hardness, viscosity recovery rate and sudden change (FF property) according to the following procedures. The results are shown in Tables 3 and 4.

[0184] (Uneven coating)

[0185] The test panel obtained under the above conditions was observed by visually observing from the front at an angle of 25 degrees and from an angle of 75 degrees, and the orientation of the pigment was observed.

[0186] The evaluation criteria are as follows: ○ represents pass and × represents fail.

[0187] ○: Uniform orientation is observed at any angle.

[0188] ×: Orientation at two or any one angle appears uneven.

[0189] (Adhesion)

[0190] The coating film of the test piece obtained from the coated article was subjected to a cellotape (registered trademark) peeling test in accordance with JIS K5600-5-6: 1999. 100 2 mm square cells were prepared and subjected to the cellotape peeling test, and the number of cells that were not peeled was counted.

[0191] The evaluation criteria are as follows: ○ represents pass and × represents fail.

[0192] ○: 0 / 100 (no peeling)

[0193] ×: 1 / 100~100 / 100 (with peeling)

[0194] [Water resistance]

[0195] The test piece obtained from the coated article was immersed in a water-resistant tank at 40°C for 240 hours. After the immersion, the coating film of the test piece taken out from the water-resistant tank was subjected to a checkerboard Cellotape (registered trademark) peeling test and appearance observation according to JIS K5600-5-6: 1999 within 1 hour after taking out. Prepare 100 checkerboards of 2 mm square, perform the cellotape peeling test, and count the number of checkerboards that were not peeled off. In addition, confirm whether there are abnormalities such as bubbles in the appearance.

[0196] The evaluation criteria are as follows: ○ represents pass and × represents fail.

[0197] ○: 0 / 100 (no peeling), no abnormal appearance

[0198] Δ: 0 / 100 (no peeling), abnormal appearance

[0199] ×: 1 / 100 to 100 / 100 (peeling occurred), not related to abnormal appearance

[0200] (Coating film hardness)

[0201] After the coated plate obtained above is placed at room temperature for 5 days, the pencil scratch hardness is measured. The pencil used is Mitsubishi UNI pencil scratch value test. In the measurement operation, the coated plate is placed and fixed on a horizontal table, and the pencil is held in a manner that the angle between the coated plate and the pencil with the core exposed on the cylinder is 45 degrees. The coated plate is pressed as hard as possible at a speed of about 1 cm / second without breaking the core, and the coated surface is pushed forward to scratch it. This operation is performed 5 times with a pencil of the same concentration. For two pencils with adjacent concentration marks, find a group with more than 2 and less than 2 scratches or breaks, and the concentration mark of the pencil with less than 2 scratches is used as the pencil hardness of the coating.

[0202] The judging criteria are as follows.

[0203] HB or above○(good)

[0204] B or below × (not included)

[0205] (Viscosity recovery rate (%))

[0206] Using a cone-plate viscometer "DHR-3" manufactured by TA Instruments, the viscosity V1 was measured at 0.1 / sec shear at 23°C, then the shear was changed from 0.1 / sec to 25000 / sec, sheared for 30 seconds, then the shear was restored to 0.1 / sec, and the viscosity V2 after 1 second of shear was measured. Based on the obtained V1 and V2, the viscosity recovery rate V2 / V1〔%〕 was calculated.

[0207] The evaluation criteria are as follows: ○ represents pass and × represents fail.

[0208] ○: Viscosity recovery rate is more than 90%

[0209] ×: Viscosity recovery rate is less than 90%

[0210] (mutation (FF))

[0211] The L value was measured at measurement angles of 25 degrees and 75 degrees using "CM-512m3" (variable chromatic aberration meter manufactured by Konica Minolta Co., Ltd.), and the FF value (L value at 25 degrees / L value at 75 degrees) was calculated.

[0212] The evaluation criteria are as follows: ○ represents pass and × represents fail.

[0213] ○: FF value is 2.2 or more

[0214] ×: FF value is less than 2.2

[0215] [Table 3]

[0216]

[0217] [Table 4]

[0218]

[0219] The raw materials in Tables 3 and 4 (excluding Preparation Examples 1 to 17) are described below.

[0220] Blocked isocyanate compound (C): manufactured by Asahi Kasei Chemicals Corporation, trade name: DURANATE MF-K60B

[0221] Pigment (A): Aluminum (flake pigment), manufactured by Toyo Aluminum Co., Ltd., trade name: ALPHA ST 07-0674

[0222] Organic solvent: methyl amyl ketone, SOLVESSO 100 (manufactured by ExxonMobil Corporation)

[0223] The coated articles of Examples 1 to 5 that meet the requirements specified in the embodiment of the present invention have a base coating film with excellent adhesion and water resistance and less uneven coating. In addition, the mutation (FF property) based on the flaky pigment is also excellent. In Comparative Example 1, the weight average molecular weight of the hydroxyl-containing acrylic resin (B) exceeds 20,000, and the non-volatile component when adjusted to the specified viscosity is less than 35%, so it is not a high-solid content type coating, and no other evaluation tests are performed. In Comparative Example 2, in contrast to Comparative Example 1, the weight average molecular weight of the hydroxyl-containing acrylic resin (B) is less than 10,000, and there are problems with the water resistance and hardness of the coating. In Comparative Example 3, the glass transition temperature Tg of the hydroxyl-containing acrylic resin (B) is as low as -10°C, and the hardness of the coating is insufficient. In Comparative Example 4, in contrast to Comparative Example 3, the glass transition temperature Tg is as high as 45°C, and there are problems with the water resistance of the coating. The hydroxyl value of the hydroxyl-containing acrylic resin (B) in Comparative Examples 5 and 6 is less than 10 mgKOH / g (Comparative Example 5) and greater than 50 mgKOH / g (Comparative Example 6). Comparative Example 5 has problems with adhesion and water resistance, and Comparative Example 6 has insufficient water resistance. Comparative Example 7 is not a lactone-modified methacrylate of the hydroxyl-containing acrylic resin (B), so water resistance is insufficient. In Comparative Examples 8 and 9, the weight average molecular weight of the second acrylic resin (E) is as low as 2000 in Comparative Example 8 and as high as 9500 in Comparative Example 9. In Comparative Example 8, the coating performance is insufficient in many items. In Comparative Example 9, the non-volatile component when adjusted to a specified viscosity is less than 35%, so it is not a high solid content type coating, and other evaluation tests were not performed. Comparative Example 10 does not contain a blocked isocyanate compound and is not cross-linked, so the water resistance and hardness of the coating performance are insufficient. Comparative Example 11 did not contain the second acrylic resin (E), and the non-volatile content when adjusted to a predetermined viscosity was less than 35%, so it was not a high-solid content type coating, and no other evaluation tests were performed. Comparative Example 12 did not contain the polymer crosslinked fine particles (D), and the non-volatile content when adjusted to a predetermined viscosity was less than 35%, so it was not a high-solid content type coating, and no other evaluation tests were performed.

Claims

1. A base coating composition comprising a pigment (A), a hydroxyl-containing acrylic resin (B), a blocked isocyanate compound (C), polymer crosslinked fine particles (D) which are insoluble in a solution of the hydroxyl-containing acrylic resin (B) and are stably dispersed, and an acrylic resin (E) having a weight average molecular weight different from that of the hydroxyl-containing acrylic resin (B), wherein: The solid content is 35% by mass or more and 60% by mass or less, The viscosity V1 was measured at 23°C using a cone-plate viscometer at a shear rate of 0.1 / sec, and then the shear rate was changed from 0.1 / sec to 25000 / sec for 30 seconds. Then, the shearing is restored to 0.1 / sec, and when the viscosity V2 after 1 second of shearing is measured, the viscosity recovery rate V2 / V1, which is the ratio of V2 to V1, is 90% or more. The aforementioned pigment (A) is a flaky pigment, The hydroxyl-containing acrylic resin (B) is a polymer containing one or more monomers of a hydroxyl-containing monomer (b), wherein the hydroxyl-containing monomer (b) is a lactone-modified monoester compound of (meth)acrylic acid and a diol having 2 to 8 carbon atoms, and the hydroxyl-containing acrylic resin (B) has a weight average molecular weight of 10,000 to 20,000, a glass transition temperature of 10° C. to 40° C., and a hydroxyl value of 10 mgKOH / g to 50 mgKOH / g. The weight average molecular weight of the acrylic resin (E) is 3000 or more and 7500 or less, The amount of the polymer crosslinked fine particles (D) in the base coating composition is 5 to 40 parts by mass based on 100 parts by mass of the total solid content of the hydroxyl-containing acrylic resin (B), the blocked isocyanate compound (C) and the acrylic resin (E).

2. The base coating composition according to claim 1, wherein The hydroxyl-containing acrylic resin (B) is a polymer of the hydroxyl-containing monomer (b) and a monomer other than the hydroxyl-containing monomer (b). The hydroxyl group-containing monomer (b) accounts for 5% by mass or more and 20% by mass or less of the total of the hydroxyl group-containing monomer (b) and the other monomers.

3. A coated article comprising an object to be coated and a base coating film formed from the base coating composition according to claim 1 or 2. 4 . The coated article according to claim 3 , comprising a multilayer coating film, the multilayer coating film comprising a base coating film provided on the coated object and a clear coating film provided on the base coating film.

5. The coated article according to claim 3, comprising a multilayer coating film, the multilayer coating film comprising a base coating film provided on the coated object provided with a mid-layer coating film or a primer coating film in advance, and a clear coating film provided on the base coating film.

Citation Information

Patent Citations

  • Water-based coating composition

    JP2008138179A

  • Method for forming multilayer coating film and coated article

    JP2010082529A

  • Coating composition

    CN105518091A

  • Method of forming coating film to carbon fiber-reinforced plastics

    JP2010260014A