Low-viscosity alkoxy-rich hyperbranched organic silicon resin as well as preparation method and application thereof
By using controlled hydrolysis and polycondensation reaction of trifunctional siloxane monomer containing alkyl/aryl group and difunctional siloxane monomer in the preparation of alkoxy silicone resin, the complex reaction routes in the prior art are solved. Environmental protection issues, low viscosity alkoxy-rich hyperbranched silicone resin was prepared, achieving high-performance high-temperature and low-dielectric coatings, suitable for industrial production and special material applications.
Patent Information
- Application Number
- CN202411278837.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-09-12
AI Technical Summary
The existing preparation methods of alkoxy silicone resins have complex reaction routes, are not economical and environmentally friendly, and are difficult to prepare in batches. The high temperature stability and dielectric properties of the coating are unclear, which limits its in the fields of semiconductor packaging and high-frequency communications. application.
By selecting a trifunctional siloxane monomer containing alkyl/aromatic group and a difunctional siloxane monomer containing alkyl/aromatic group, it can produce a low-branched topological structure with a highly branched topological structure through the action of a catalyst. Viscosity-rich alkoxy-heavy-branched silicone resin and cured by heating condensation or moisture dehydrogenation condensation.
It realizes the preparation of silicone resins with low viscosity, high transparency and high activity, reduces the silicon hydroxyl content, is suitable for industrial production, forms a transparent silicone coating that is resistant to high temperature and low dielectric, is suitable for large-scale production, and can be used in special functional polymer materials. Improvement of modification.
Smart Images

Figure CN118978701A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of organic polymer materials, and more specifically, relates to a low-viscosity alkoxy-rich hyperbranched organic silicon resin and a preparation method and application thereof. Background Art
[0002] Silicone resins with high thermal stability and low dielectric loss are widely used in semiconductor packaging, flat panel displays, electronic product protection and communication equipment, with the main goals of reducing electromagnetic interference and increasing signal transmission rate. With the development of the 5G industry, the market demand for silicone resin coatings is becoming increasingly diversified, requiring not only further improvement in material performance, but also cost-effectiveness, environmental friendliness and feasibility of manufacturing processes.
[0003] Among them, alkoxy silicone resins have good processability of moisture curing under mild conditions, which helps expand their application range in high-frequency communications and microelectronics. The improvement of the synthesis technology of alkoxy silicone resins is mainly focused on improving their molecular structure and improving the performance of the matrix. By controlling the reaction conditions and using modification methods, the molecular weight distribution and molecular topological structure of the resin can be further regulated, which is conducive to optimizing the thermal stability and dielectric properties of silicone resin materials.
[0004] Chinese patent CN1283695C discloses a method for improving the heat resistance of silicone resin by using polyhedral oligomeric silsesquioxane. The silicone resin is prepared by using methyl alkoxysilane monomer as raw material, and a modified silicone resin with certain heat resistance is prepared by adding oligomeric silsesquioxane accounting for 0.5 to 10% of the mass of the silicone resin. However, the preparation route of this method is complicated, the doping degree of oligomeric silsesquioxane is required to be high, and the raw material cost is also high.
[0005] Chinese patent CN114133574A discloses a method for improving the mechanical strength of silicone resin and maintaining good heat resistance and dielectric properties of silicone resin by introducing bridged cycloalkanes into the main chain of silicone resin. However, this method still has some shortcomings. The presence of a large number of benzene rings in the resin structure leads to increased steric hindrance of phenyl silicone resin, and the reaction conditions are relatively harsh and not suitable for industrial production.
[0006] Chinese patent CN102887916A discloses an alkoxy silicone resin intermediate and its preparation method. The monomer source for synthesizing the alkoxy silicone resin intermediate is organic chlorosilane, and the resin can be used to modify organic resins containing active hydroxyl functional groups. However, the preparation method will produce a large amount of acidic by-products, and there are many post-processing steps. In addition, there are equipment corrosion problems in the production process, which does not meet the requirements of green environmental protection.
[0007] Chinese patent CN103755960A discloses a heat-stable methylphenyl silicone resin and a preparation method thereof. The resin is not easily soluble in toluene and xylene. A large amount of toluene needs to be added as a solvent during the synthesis process, and the initial thermal decomposition temperature of the resin solid is difficult to exceed 500°C.
[0008] At present, there are few types of alkoxy silicone resins in China that can meet the demand for high-temperature resistant and low-dielectric silicone resin coatings, and the preparation methods of alkoxy silicone resins disclosed in existing patent documents still have shortcomings such as complicated reaction routes, insufficient economy and environmental protection, and difficulty in batch preparation. Most alkoxy silicone resin coatings also have problems such as insufficient high-temperature stability, unclear dielectric properties, and unclear comprehensive performance, which seriously limit the use scenarios and application promotion of silicone resin coating materials. Therefore, how to provide a simple, fast, green and environmentally friendly method for preparing high-performance, low-viscosity alkoxy-rich silicone resins is critical to optimizing the performance of silicone resin coatings. Summary of the invention
[0009] In view of the above problems existing in the prior art, the technical problem to be solved by the present invention is to provide a method for preparing a low-viscosity alkoxy-rich hyperbranched silicone resin, wherein the method selects a trifunctional siloxane monomer containing an alkyl / aromatic group and a difunctional siloxane monomer containing an alkyl / aromatic group to undergo a controlled hydrolysis and polycondensation reaction under the action of a catalyst, thereby obtaining a hyperbranched silicone resin having a highly branched topological structure and rich in alkoxy functional groups. Another technical problem to be solved by the present invention is to provide a low-viscosity alkoxy-rich hyperbranched silicone resin prepared by the above method, the resin presenting the physical and chemical characteristics of low viscosity, high transparency and high activity, and can be further cured and formed by means of heating condensation or moisture dealcoholization condensation. Another technical problem to be solved by the present invention is to provide the application of the above low-viscosity alkoxy-rich hyperbranched silicone resin in a high temperature resistant and low dielectric silicone resin coating.
[0010] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:
[0011] A method for preparing a low-viscosity alkoxy-rich hyperbranched silicone resin, using a trifunctional siloxane monomer containing an alkyl group or an aromatic group as a raw material, and preparing a low-viscosity alkoxy-rich hyperbranched silicone resin through hydrolysis nucleation, condensation growth, end-capping, and purification treatment; wherein the alkoxy content is not less than 3%, and the viscosity is not higher than 1000mPa·s. The reaction formula is:
[0012]
[0013] Preferably, the trifunctional siloxane monomer containing an alkyl group or an aromatic group is selected from one or more of methyltrimethoxysilane, isobutyltrimethoxysilane, n-hexyltrimethoxysilane, cyclohexyltrimethoxysilane, n-octyltrimethoxysilane, n-dodecyltrimethoxysilane, n-hexadecyltrimethoxysilane, methyltriethoxysilane, isobutyltriethoxysilane, n-hexyltriethoxysilane, cyclohexyltriethoxysilane, n-octyltriethoxysilane, n-dodecyltriethoxysilane, n-hexadecyltriethoxysilane, phenyltrimethoxysilane, naphthyltrimethoxysilane, biphenyltrimethoxysilane, phenyltriethoxysilane, naphthyltriethoxysilane, and biphenyltriethoxysilane.
[0014] Preferably, the trifunctional siloxane monomer containing an alkyl group or an aromatic group is selected from one or more of methyltrimethoxysilane and phenyltrimethoxysilane.
[0015] The method for preparing the low-viscosity alkoxy-rich hyperbranched silicone resin comprises the following specific steps:
[0016] 1) adding a trifunctional siloxane monomer containing an alkyl group or an aromatic group and deionized water into a reactor and mixing them, and performing a hydrolysis reaction at room temperature for 3 to 5 hours;
[0017] 2) adding a difunctional siloxane monomer containing an alkyl group or an aromatic group, deionized water and a catalyst to the reaction system of step 1) and performing a condensation growth reaction at 80 to 90° C. for 11 to 13 hours;
[0018] 3) adding an alcohol capping agent and a catalyst to the reaction system of step 2) and reacting at 115-125° C. for 7-9 hours;
[0019] 4) distilling the solution after the end-capping reaction in step 3) under reduced pressure to obtain a low-viscosity alkoxy-rich hyperbranched silicone resin.
[0020] Preferably, in step 1), the molar ratio of the trifunctional siloxane monomer containing an alkyl group or an aromatic group to deionized water is 1:0.1-3.
[0021] Preferably, in step 2), the molar ratio of the difunctional siloxane monomer containing an alkyl group or an aromatic group, deionized water and the catalyst is 1:0.1-3:0.001-0.1.
[0022] Preferably, in step 2), the trifunctional siloxane monomer containing an alkyl group or an aromatic group is selected from one or more of dimethyldimethoxysilane, methylphenyldimethoxysilane, diphenyldimethoxysilane, dimethyldiethoxysilane, methylphenyldiethoxysilane and diphenyldiethoxysilane;
[0023] The catalyst is selected from one or more of hydrochloric acid, sulfuric acid, phosphoric acid, oxalic acid, glacial acetic acid, trifluoromethanesulfonic acid, p-toluenesulfonic acid, ammonium chloride, potassium hydroxide, sodium hydroxide, ammonia water, triethylamine, and tetramethylammonium hydroxide.
[0024] Preferably, in step 3), the molar ratio of the trifunctional siloxane monomer containing an alkyl group or an aromatic group, the alcohol capping agent and the catalyst is 1:0.1-10:0.01-0.1.
[0025] Preferably, in step 3), the alcohol capping agent is selected from one or more of methanol, ethanol, propanol, butanol, pentanol, hexanol, heptanol, octanol, vinyl alcohol, and propenol;
[0026] The catalyst is selected from one or more of oxalic acid, glacial acetic acid, trifluoromethanesulfonic acid and p-toluenesulfonic acid.
[0027] The method for preparing the low-viscosity alkoxy-rich hyperbranched organic silicone resin prepares the low-viscosity alkoxy-rich hyperbranched organic silicone resin.
[0028] The low-viscosity alkoxy-rich hyperbranched silicone resin is used in high-temperature resistant and low-dielectric silicone resin coatings.
[0029] Beneficial effects: Compared with the prior art, the present invention has the following advantages:
[0030] 1) The present invention selects a trifunctional siloxane monomer containing an alkyl / aromatic group and a difunctional siloxane monomer containing an alkyl / aromatic group to undergo a controlled hydrolysis and polycondensation reaction under the action of a catalyst, thereby preparing a hyperbranched silicone resin having a highly branched topological structure and rich in alkoxy functional groups. The resin has the physical and chemical characteristics of low viscosity, high transparency and high activity, and can be further cured and formed by means of heating condensation or moisture dealcoholization condensation;
[0031] 2) The present invention utilizes esterification end-capping reaction to control and reduce the content of silanol groups that is not conducive to storage, and the content of silanol groups is not higher than 1%; therefore, the prepared alkoxy-rich hyperbranched silicone resin can achieve long-term stable storage under ordinary conditions, and the alkoxy content and viscosity range of the resin can be quantitatively controlled according to different application requirements;
[0032] 3) The low-viscosity alkoxy-rich hyperbranched silicone resin prepared by the present invention can be used for modification and enhancement of special functional polymer materials and their composite materials. After curing itself, it can form a high-temperature resistant and low-dielectric silicone transparent coating. The coating preparation process is simple and controllable, and is suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is a physical picture of the low-viscosity alkoxy-rich hyperbranched silicone resin prepared in Examples 1-7;
[0034] Figure 2 This is a physical picture of the alkoxy-containing silicone resin prepared in Comparative Example 1-2;
[0035] Figure 3 The infrared spectra of the low-viscosity alkoxy-rich hyperbranched silicone resin prepared in Examples 1-7;
[0036] Figure 4 This is a real picture of the moisture-cured sample of the low-viscosity alkoxy-rich hyperbranched silicone resin prepared in Example 1 and Example 7 at room temperature;
[0037] Figure 5 This is a thermogravimetric curve of the low-viscosity alkoxy-rich hyperbranched silicone resin prepared in Example 1;
[0038] Figure 6 This is a thermogravimetric differential curve of the low-viscosity alkoxy-rich hyperbranched silicone resin prepared in Example 1;
[0039] Figure 7 This is a photo of the coating of the low-viscosity alkoxy-rich hyperbranched silicone resin prepared in Example 1 cured under heating conditions;
[0040] Figure 8 The dielectric constant and dielectric loss curve of the low-viscosity alkoxy-rich hyperbranched silicone resin cured sample prepared in Example 1;
[0041] Fig. 9 This is a loss factor curve of the cured sample of the low-viscosity alkoxy-rich hyperbranched silicone resin prepared in Example 1. DETAILED DESCRIPTION
[0042] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described below in conjunction with specific embodiments. In the following examples, unless otherwise specified, the technical means used are conventional means well known to those skilled in the art. If specific conditions are not specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0043] The performance testing method adopted by the present invention is as follows:
[0044] 1. Resin viscosity: The viscosity of liquid silicone resin was tested using a ROTAVIS rotary viscometer (IKA, Germany);
[0045] 2. Infrared spectroscopy: Infrared testing was performed using a Tensor II FT-IR spectrometer (Bruker, Germany). Liquid samples were smeared on a pressed KBr sample and the test scanning range was 400-4000 cm -1 .
[0046] 3. Thermogravimetric analysis test: Thermogravimetric analysis was performed using a STA449F3 thermogravimetric-differential scanning calorimetric simultaneous analyzer (Netzche, Germany).
[0047] 4. Alkoxy content: The alkoxy content of silicon is determined by the perchloric acid acetylation titration volumetric method.
[0048] 5.Silanol content: The silanol content is determined by the diisocyanate back titration volumetric method.
[0049] 6. Dielectric constant and dielectric loss: The dielectric test was performed using a Concept 80 broadband dielectric and impedance spectrometer (Novocontrol, Germany). The solid test samples were pre-sprayed with gold.
[0050] Example 1
[0051] A method for preparing a low-viscosity alkoxy-rich hyperbranched silicone resin comprises the following steps:
[0052] 1) Add 1362.2 g of methyltrimethoxysilane and 245 g of deionized water into a three-necked flask equipped with a stirring and condensation reflux device, and react at room temperature for 4 hours;
[0053] 2) adding 1202.2 g of dimethyldimethoxysilane, 90 g of deionized water and 20 mL of 37% HCl solution to the reaction system of step 1), and reacting at 85° C. for 12 h;
[0054] 3) Add 5.85 L of anhydrous ethanol to the reaction system of step 2), add 10 mL of trifluoromethanesulfonic acid dropwise using a constant pressure dropping funnel, heat the reaction system to 120° C. and continue the reaction for 8 h;
[0055] 4) The resin solution after the reaction is completed is subjected to reduced pressure distillation at 0.01 kPa and 85° C. to remove the solvent and small molecular monomers to obtain a low-viscosity alkoxy-rich hyperbranched silicone resin.
[0056] Example 2
[0057] A method for preparing a low-viscosity alkoxy-rich hyperbranched silicone resin comprises the following steps:
[0058] 1) Add 1226.0 g of methyltrimethoxysilane, 198.3 g of phenyltrimethoxysilane and 245 g of deionized water into a three-necked flask equipped with a stirring and condensation reflux device, and react at room temperature for 4 hours;
[0059] 2) adding 1082.0 g of dimethyldimethoxysilane, 189.3 g of methylphenyldimethoxysilane, 90 g of deionized water and 20 mL of 37% HCl solution to the reaction system of step 1), and reacting at 85° C. for 12 h;
[0060] 3) Add 5.85 L of anhydrous ethanol to the reaction system of step 2), add 10 mL of trifluoromethanesulfonic acid dropwise using a constant pressure dropping funnel, heat the reaction system to 120° C. and continue the reaction for 8 h;
[0061] 4) The resin solution after the reaction is completed is subjected to reduced pressure distillation at 0.01 kPa and 85° C. to remove the solvent and small molecular monomers to obtain a low-viscosity alkoxy-rich hyperbranched silicone resin.
[0062] Example 3
[0063] A method for preparing a low-viscosity alkoxy-rich hyperbranched silicone resin comprises the following steps:
[0064] 1) Add 953.5 g of methyltrimethoxysilane, 594.9 g of phenyltrimethoxysilane and 245 g of deionized water into a three-necked flask equipped with a stirring and condensation reflux device, and react at room temperature for 4 hours;
[0065] 2) adding 841.5 g of dimethyldimethoxysilane, 567.9 g of methylphenyldimethoxysilane, 90 g of deionized water and 20 mL of 37% HCl solution to the reaction system of step 1), and reacting at 85° C. for 12 h;
[0066] 3) Add 5.85 L of anhydrous ethanol to the reaction system of step 2), add 10 mL of trifluoromethanesulfonic acid dropwise using a constant pressure dropping funnel, heat the reaction system to 120° C. and continue the reaction for 8 h;
[0067] 4) The resin solution after the reaction is completed is subjected to reduced pressure distillation at 0.01 kPa and 85° C. to remove the solvent and small molecular monomers to obtain a low-viscosity alkoxy-rich hyperbranched silicone resin.
[0068] Example 4
[0069] A method for preparing a low-viscosity alkoxy-rich hyperbranched silicone resin comprises the following steps:
[0070] 1) Add 681.1 g of methyltrimethoxysilane, 991.5 g of phenyltrimethoxysilane and 245 g of deionized water into a three-necked flask equipped with a stirring and condensation reflux device, and react at room temperature for 4 hours;
[0071] 2) adding 601.1 g of dimethyldimethoxysilane, 946.5 g of methylphenyldimethoxysilane, 90 g of deionized water and 20 mL of 37% HCl solution to the reaction system of step 1), and reacting at 85° C. for 12 h;
[0072] 3) Add 5.85 L of anhydrous ethanol to the reaction system of step 2), add 10 mL of trifluoromethanesulfonic acid dropwise using a constant pressure dropping funnel, heat the reaction system to 120° C. and continue the reaction for 8 h;
[0073] 4) The resin solution after the reaction is completed is subjected to reduced pressure distillation at 0.01 kPa and 85° C. to remove the solvent and small molecular monomers to obtain a low-viscosity alkoxy-rich hyperbranched silicone resin.
[0074] Example 5
[0075] A method for preparing a low-viscosity alkoxy-rich hyperbranched silicone resin comprises the following steps:
[0076] 1) Add 408.7 g of methyltrimethoxysilane, 1388.0 g of phenyltrimethoxysilane and 245 g of deionized water into a three-necked flask equipped with a stirring and condensation reflux device, and react at room temperature for 4 hours;
[0077] 2) adding 360.7 g of dimethyldimethoxysilane, 1325.0 g of methylphenyldimethoxysilane, 90 g of deionized water and 20 mL of 37% HCl solution to the reaction system of step 1), and reacting at 85° C. for 12 h;
[0078] 3) Add 5.85 L of anhydrous ethanol to the reaction system of step 2), add 10 mL of trifluoromethanesulfonic acid dropwise using a constant pressure dropping funnel, heat the reaction system to 120° C. and continue the reaction for 8 h;
[0079] 4) The resin solution after the reaction is completed is subjected to reduced pressure distillation at 0.01 kPa and 85° C. to remove the solvent and small molecular monomers to obtain a low-viscosity alkoxy-rich hyperbranched silicone resin.
[0080] Example 6
[0081] A method for preparing a low-viscosity alkoxy-rich hyperbranched silicone resin comprises the following steps:
[0082] 1) Add 136.2 g of methyltrimethoxysilane, 1784.6 g of phenyltrimethoxysilane and 245 g of deionized water into a three-necked flask equipped with a stirring and condensation reflux device, and react at room temperature for 4 hours;
[0083] 2) adding 120.2 g of dimethyldimethoxysilane, 1703.6 g of methylphenyldimethoxysilane, 90 g of deionized water and 20 mL of 37% HCl solution to the reaction system of step 1), and reacting at 85° C. for 12 h;
[0084] 3) Add 5.85 L of anhydrous ethanol to the reaction system of step 2), add 10 mL of trifluoromethanesulfonic acid dropwise using a constant pressure dropping funnel, heat the reaction system to 120° C. and continue the reaction for 8 h;
[0085] 4) The resin solution after the reaction is completed is subjected to reduced pressure distillation at 0.01 kPa and 85° C. to remove the solvent and small molecular monomers to obtain a low-viscosity alkoxy-rich hyperbranched silicone resin.
[0086] Example 7
[0087] A method for preparing a low-viscosity alkoxy-rich hyperbranched silicone resin comprises the following steps:
[0088] 1) Add 1982.9 g of phenyltrimethoxysilane and 245 g of deionized water into a three-necked flask equipped with a stirring and condensation reflux device, and react at room temperature for 4 hours;
[0089] 2) adding 1892.9 g of methylphenyldimethoxysilane, 90 g of deionized water and 20 mL of 37% HCl solution to the reaction system of step 1), and reacting at 85° C. for 12 h;
[0090] 3) Add 5.85 L of anhydrous ethanol to the reaction system of step 2), add 10 mL of trifluoromethanesulfonic acid dropwise using a constant pressure dropping funnel, heat the reaction system to 120° C. and continue the reaction for 8 h;
[0091] 4) The resin solution after the reaction is completed is subjected to reduced pressure distillation at 0.01 kPa and 85° C. to remove the solvent and small molecular monomers to obtain a low-viscosity alkoxy-rich hyperbranched silicone resin.
[0092] Comparative Example 1
[0093] 1) Add 100 g of tetraethoxysilane, 31 g of hexamethyldisiloxane and 400 g of anhydrous ethanol to a three-necked flask equipped with a stirring and condensation reflux device, and stir at room temperature for 1 hour;
[0094] 2) adding 100 g of 0.2 M hydrochloric acid solution to the reaction system of step 1), and after the addition was completed, mechanical stirring was continued at room temperature for 1 h, and then the reaction system was gradually heated to 70° C. and the reaction was continued for 3 h;
[0095] 3) adding 200 g of toluene to the reaction system of step 2), mechanically stirring at room temperature for 2 h, stopping mechanical stirring, standing for 2 h, separating the liquids, and collecting the upper extract;
[0096] 4) Pour all the extracts from step 3) into another flask, add 0.5M potassium hydroxide solution dropwise, adjust the pH value of the solution to 8, connect an oil-water separator, heat the reaction system to 85°C, and keep the temperature constant for 3 hours;
[0097] 5) Cooling the reaction system in step 4) to 60°C, adding solid sodium bicarbonate to adjust the solution pH to 6.5; then filtering, collecting the filtrate, and distilling under reduced pressure at 0.01 kPa and 85°C to obtain an alkoxy-containing silicone resin. Figure 2 As shown, the resin prepared in Comparative Example 1 is a milky white viscous liquid.
[0098] Comparative Example 2
[0099] 1) Add 110 g of methyltrimethoxysilane, 394 g of dimethyldiethoxysilane, 780 g of phenyltriethoxysilane and 2.5 g of lead cyclopentaneate catalyst into a three-necked flask equipped with a stirring and condensation reflux device, stir well for 1 hour at room temperature, and continue to heat to 100° C.;
[0100] 2) Add 120 g of deionized water to the reaction system of step 1) for quantitative hydrolysis over 3 hours;
[0101] 3) After the reaction system of step 2) was reacted for 30 minutes, the system was vacuumed to 0.01 kPa and the temperature was gradually raised to 120° C. to remove small molecular impurities such as ethanol;
[0102] 4) Observation step 3) After no liquid drips out of the reaction system, the material is immediately discharged to obtain a white solid silicone resin.
[0103] The resin viscosity and the alkoxy and hydroxyl contents of the samples prepared in the above Examples 1-7 and Comparative Examples 1-2 were tested. The test results are shown in Table 1.
[0104] Table 1 Viscosity and functional group content of silicone resin samples prepared in Examples 1-7 and Comparative Examples 1-2
[0105] Resin viscosity (mPa·s) Alkoxy content (%) Silicon hydroxy content (%) Example 1 300 15.9 0.07 Example 2 420 13.6 0.07 Example 3 560 12.4 0.12 Example 4 620 10.5 0.14 Example 5 710 8.9 0.23 Example 6 810 7.3 0.29 Example 7 960 3.6 0.39 Comparative Example 1 193000 1.9 3.42 Comparative Example 2 White powder 7.0 1.52
[0106] As can be seen from Table 1, the hyperbranched silicone resin prepared by the hydrolysis nucleation, condensation growth, end-capping and purification treatment route of the present invention has a higher alkoxy content and a lower silanol content. Compared with Comparative Examples 1-2, the alkoxy-rich hyperbranched silicone resin prepared in Examples 1-7 exhibits a lower viscosity, an alkoxy content of not less than 3.5%, and a silanol content of not more than 0.5%.
[0107] Depend on Figure 1 and Figure 2 It can be seen that the alkoxy-rich hyperbranched silicone resin (Examples 1-7) prepared by the present invention is in a colorless liquid state. Compared with Comparative Examples 1-2, the alkoxy-rich hyperbranched silicone resin (Examples 1-7) prepared by the present invention has better transparency and lower resin viscosity.
[0108] Depend on Figure 3 It can be seen that the alkoxy-rich hyperbranched silicone resin (Examples 1-7) prepared by the present invention has a peak at 2972 cm -1 There are typical infrared characteristic peaks of silane alkoxy groups, proving that alkoxy groups are distributed in the silicone resin skeleton structure.
[0109] Depend on Figure 4 It can be seen that the alkoxy-rich hyperbranched silicone resin (Example 1, Example 7) prepared by the present invention can be cross-linked and cured to form a hard coating after being placed in a room temperature environment (50% RH) for 12 hours, and the coating can withstand high-temperature burning treatment with the outer flame of an alcohol blowtorch (outer flame temperature ≥800°C).
[0110] Depend on Figure 5 It can be seen that after the alkoxy-rich hyperbranched silicone resin (Example 1) prepared by the present invention is cured, the cured product has good thermal stability in nitrogen and air atmospheres, and the initial thermal decomposition temperature is higher than 500°C.
[0111] Depend on Figure 6 It can be seen that after the alkoxy-rich hyperbranched silicone resin (Example 1) prepared by the present invention is cured, the cured product has good thermal stability in nitrogen and air atmospheres, and the maximum thermal weight loss temperature is higher than 550°C.
[0112] Depend on Figure 7 It can be seen that the alkoxy-rich hyperbranched silicone resin (Example 1) prepared by the present invention has heat-curable cross-linking properties. After programmed temperature increase (100°C×2h→140°C×2h→180°C×2h→220°C×4h), a transparent and strong thermosetting silicone coating can be obtained, and can be firmly attached to the surface of the carbon fiber composite.
[0113] Depend on Figure 8 It can be seen that the alkoxy-rich hyperbranched silicone resin embodiment 1 thermal cured product prepared by the present invention exhibits the low dielectric characteristics of silicone resin. When the frequency is 1 kHz, the dielectric constant is not higher than 3.0, and the dielectric loss is about 0.01.
[0114] Depend on Fig. 9 It can be seen that the alkoxy-rich hyperbranched silicone resin embodiment 1 thermal cured product prepared by the present invention exhibits the low dielectric characteristics of silicone resin. When the frequency is 1 kHz, the loss factor is about 36.9×10 -4 .
[0115] Table 2 Test results of hyperbranched silicone resin cured samples prepared in Examples 1-7 and Comparative Examples 1-2
[0116]
[0117]
[0118] As can be seen from Table 2, the alkoxy-rich hyperbranched silicone resin (Examples 1-7) thermosetting materials prepared by the present invention have better thermal stability than the thermosetting materials of Comparative Examples 1-2, and the initial thermal decomposition temperature in air atmosphere is higher than 400°C, while the initial thermal decomposition temperature of the corresponding samples of Examples 1 and 2 can be higher than 500°C. In addition, the thermosetting materials of Examples 1-7 exhibit lower dielectric constants and dielectric losses, and have excellent dielectric properties, and are expected to be applied in the field of 5G-related materials.
[0119] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a low-viscosity alkoxy-rich hyperbranched silicone resin, characterized in that: A low-viscosity alkoxy-rich hyperbranched silicone resin is prepared from a trifunctional siloxane monomer containing an alkyl or aromatic group through hydrolysis nucleation, condensation growth, end-capping, and purification. The alkoxy content is not less than 3%, and the viscosity is not higher than 1000 mPa·s.
2. The method for preparing a low-viscosity alkoxy-rich hyperbranched silicone resin according to claim 1, wherein: The trifunctional siloxane monomer containing an alkyl group or an aromatic group is selected from one or more of methyltrimethoxysilane, isobutyltrimethoxysilane, n-hexyltrimethoxysilane, cyclohexyltrimethoxysilane, n-octyltrimethoxysilane, n-dodecyltrimethoxysilane, n-hexadecyltrimethoxysilane, methyltriethoxysilane, isobutyltriethoxysilane, n-hexyltriethoxysilane, cyclohexyltriethoxysilane, n-octyltriethoxysilane, n-dodecyltriethoxysilane, n-hexadecyltriethoxysilane, phenyltrimethoxysilane, naphthyltrimethoxysilane, biphenyltrimethoxysilane, phenyltriethoxysilane, naphthyltriethoxysilane, and biphenyltriethoxysilane.
3. The method for preparing a low-viscosity alkoxy-rich hyperbranched silicone resin according to claim 1, wherein: The specific steps include: 1) adding a trifunctional siloxane monomer containing an alkyl group or an aromatic group and deionized water into a reactor and mixing them, and performing a hydrolysis reaction at room temperature for 3 to 5 hours; 2) adding a difunctional siloxane monomer containing an alkyl or aromatic group, deionized water, and a catalyst to the reaction system of step 1), and performing a condensation growth reaction at 80-90° C. for 11-13 hours; 3) adding an alcohol capping agent and a catalyst to the reaction system of step 2) and reacting at 115-125° C. for 7-9 hours; 4) distilling the solution after the end-capping reaction in step 3) under reduced pressure to obtain a low-viscosity alkoxy-rich hyperbranched silicone resin.
4. The method for preparing a low-viscosity alkoxy-rich hyperbranched silicone resin according to claim 3, wherein: In the step 1), the molar ratio of the trifunctional siloxane monomer containing an alkyl group or an aromatic group to deionized water is 1:0.1-3.
5. The method for preparing a low-viscosity alkoxy-rich hyperbranched silicone resin according to claim 3, wherein: In the step 2), the molar ratio of the trifunctional siloxane monomer containing an alkyl or aromatic group, the difunctional siloxane monomer containing an alkyl or aromatic group, deionized water, and the catalyst is 1:0-3:0.1-5:0.001-0.
1.
6. The method for preparing a low-viscosity alkoxy-rich hyperbranched silicone resin according to claim 3, wherein: In the step 2), the difunctional siloxane monomer containing an alkyl group or an aromatic group is selected from one or more of dimethyldimethoxysilane, methylphenyldimethoxysilane, diphenyldimethoxysilane, dimethyldiethoxysilane, methylphenyldiethoxysilane, and diphenyldiethoxysilane; The catalyst is selected from one or more of hydrochloric acid, sulfuric acid, phosphoric acid, oxalic acid, glacial acetic acid, trifluoromethanesulfonic acid, p-toluenesulfonic acid, ammonium chloride, potassium hydroxide, sodium hydroxide, ammonia water, triethylamine, and tetramethylammonium hydroxide.
7. The method for preparing a low-viscosity alkoxy-rich hyperbranched silicone resin according to claim 3, wherein: In the step 3), the molar ratio of the trifunctional siloxane monomer containing an alkyl group or an aromatic group, the alcohol end-capping agent, and the catalyst is 1:0.1-10:0.01-0.
1.
8. The method for preparing a low-viscosity alkoxy-rich hyperbranched silicone resin according to claim 3, wherein: In step 3), the alcohol capping agent is selected from one or more of methanol, ethanol, propanol, butanol, pentanol, hexanol, heptanol, octanol, vinyl alcohol, and propenol; The catalyst is selected from one or more of oxalic acid, glacial acetic acid, trifluoromethanesulfonic acid and p-toluenesulfonic acid.
9. The method for preparing a low-viscosity alkoxy-rich hyperbranched organosilicon resin according to any one of claims 1 to 8, wherein the low-viscosity alkoxy-rich hyperbranched organosilicon resin is prepared.
10. Use of the low-viscosity alkoxy-rich hyperbranched silicone resin according to claim 9 in a high-temperature resistant low-dielectric silicone resin coating.
Citation Information
Patent Citations
Photosensitive hyperbranched organic silicon resin as well as preparation method and application thereof
CN117050311A
Method for preparing low-viscosity hyperbranched organic silicon resin with high silicon vinyl content
CN118185016A
Curable condensation compounds based on alkoxy-functional polysiloxanes
US20220177652A1
Cited By
Hyperbranched organic silicon modified high-strength polyether type ablation-resistant elastomer and preparation method thereof
CN119661868A
A hyperbranched silicone-modified high-strength polyether ablative-resistant elastomer and a preparation method thereof
CN119661868B
A temperature-resistant and ablation-resistant condensed silicone rubber composite material based on alkoxy hyperbranched silicone resin and a preparation method thereof
CN122978712A