A device and method for preparing nano-aluminum based on ionic liquid electrolytes
The nano-aluminum preparation device based on ionic liquid electrolyte utilizes a stirring element to generate eddy currents to peel off and collect nano-aluminum particles, solving the problems of uneven particle size, low purity, and poor safety in existing technologies, and achieving efficient and safe preparation and collection of nano-aluminum.
Patent Information
- Application Number
- CN202310494839.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-04-28
AI Technical Summary
Existing nano-aluminum preparation technologies suffer from problems such as uneven particle size, low purity, serious pollution, and poor safety. Furthermore, the preparation devices based on ionic liquid electrolytes are not yet perfect, making preparation and collection inconvenient.
A nano-aluminum preparation device based on ionic liquid electrolyte is adopted, including an electrolytic cell, a collection component, a stirring component, an electrolysis component, a liquid addition component, a liquid dispensing component, and a liquid measurement component. The stirring component generates eddy currents to peel off nano-aluminum particles, which are then collected by the collection component. Combined with a composite electrolyte system and temperature detection, the preparation and collection are made convenient.
This method enables efficient, safe, and simple preparation and collection of nano-aluminum, resulting in uniform particle size and high purity, while reducing equipment requirements and costs.
Smart Images

Figure CN116377522B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of nano-aluminum preparation technology, specifically to a nano-aluminum preparation apparatus and method based on ionic liquid electrolytes. Background Technology
[0002] Nano-aluminum is a novel material derived from aluminum, exhibiting exceptionally high surface area and chemical activity due to its nanoscale particle size. It can oxidize rapidly in air, releasing a significant amount of heat. The addition of nano-aluminum powder can substantially improve the combustion efficiency and density impulse of liquid fuels, and also has a significant effect on enhancing the efficiency of liquid rocket fuels. Therefore, nano-aluminum, as an advanced material, has a positive impact on high-tech fields such as aerospace and electronics.
[0003] The production of nano-aluminum both domestically and internationally is mainly carried out through physical or chemical methods. Physical methods primarily include electro-explosion wire method, high-energy ball milling method, and evaporation-condensation method. Among these, the electro-explosion wire method is currently the most researched and the main method for the industrial production of nano-metal materials. This method converts electrical energy into other forms of energy, such as shock wave energy, thereby altering the physical state of the aluminum material to achieve the preparation of nano-aluminum. However, the resulting nanoparticles suffer from problems such as large particle size and wide particle size distribution, thus requiring further processing before use. The high-energy ball milling method is simple and efficient, but it generates significant noise and dust pollution, and produces products with low purity and uneven particle size. The evaporation-condensation method is an earlier method for preparing nano-metal particles, producing smaller particle sizes, but this method has high manufacturing costs and requires sophisticated equipment. In addition to the above methods, chemical methods can also be used to prepare nano-aluminum. This method typically uses organic solutions as the reaction medium, offering high operability and low operating temperatures. However, the reaction system is volatile, flammable, and highly toxic, which are also significant problems. In summary, the aforementioned traditional processes, due to their inherent limitations, restrict their further development in the preparation of nano-aluminum. Therefore, my country urgently needs to develop safer, greener, and more efficient nano-aluminum preparation technologies.
[0004] Ionic liquids are a novel type of room-temperature molten electrolyte, typically composed of organic cations and organic / inorganic anions. This unique structure endows ionic liquids with advantages such as high conductivity, a wide electrochemical window, non-volatility, and non-flammability. Recent studies have shown that ionic liquids can be used as electrolytes to prepare nano-aluminum via electrodeposition. The reaction process is characterized by low temperature, low energy consumption, and high safety, offering significant technological advantages over traditional methods. Therefore, ionic liquids hold immense application potential in the preparation of nano-aluminum, attracting widespread interest and attention from both academia and industry.
[0005] Since the technology for preparing nano-aluminum based on ionic liquid electrolytes is still in its early stages, the devices for preparing and collecting nano-aluminum products using this technology are not yet perfect. Therefore, how to achieve convenient and rapid preparation and collection of nano-aluminum products is an urgent problem to be solved. Summary of the Invention
[0006] To address the shortcomings of existing technologies, this invention provides a device and method for preparing nano-aluminum based on ionic liquid electrolytes.
[0007] This invention discloses a nano-aluminum preparation device based on an ionic liquid electrolyte, comprising:
[0008] An electrolytic cell, comprising a cell body and a cover plate, the cover plate being placed over the opening of the cell body;
[0009] The collection component is located inside the tank body and at the bottom of the tank body;
[0010] A stirring assembly includes a stirring connector and a stirring element. One end of the stirring connector passes through a cover plate, and the other end extends toward the collecting assembly. The stirring element is located at the other end of the stirring connector.
[0011] An electrolysis assembly comprising an aluminum cathode and an aluminum anode, the aluminum cathode and aluminum anode being located within the tank body and arranged around a stirring element;
[0012] The liquid addition assembly, with one end located inside the tank body, is used to add ionic liquid electrolytes into the tank body.
[0013] The liquid outlet assembly, one end of which is located inside the tank body and extends close to the collection assembly; and
[0014] The liquid level measuring component is used for detecting the liquid level of the ionic liquid electrolyte inside the tank body.
[0015] According to one embodiment of the present invention, the stirring element is a propeller-type stirring fan blade or a turbine-type stirring fan blade.
[0016] According to one embodiment of the present invention, the collecting component is a conical tower or a conical trough.
[0017] According to one embodiment of the present invention, the tank body includes an upper tank body and a lower tank body, the lower tank body is detachably connected to the lower end of the upper tank body, and the collection component is located in the lower tank body; the upper tank body and the lower tank body are sealed together.
[0018] According to one embodiment of the present invention, it further includes a filter assembly; the filter assembly is disposed at the opening of the lower tank and is located between the collecting assembly and the stirring component.
[0019] According to one embodiment of the present invention, it further includes a filter assembly; the filter assembly is disposed within the tank body and located between the collecting assembly and the stirring component.
[0020] According to one embodiment of the present invention, the filter assembly has a closed mesh structure.
[0021] According to one embodiment of the present invention, it further includes a temperature detection component for detecting the temperature of the ionic liquid electrolyte inside the tank body.
[0022] A method for preparing nano-aluminum based on ionic liquid electrolytes includes the following steps:
[0023] Preparation of ionic liquid electrolytes;
[0024] The above-mentioned ionic liquid electrolyte nano-aluminum preparation device is used to prepare nano-aluminum.
[0025] According to one embodiment of the present invention, the ionic liquid electrolyte includes a composite electrolyte system or a [BmPy][Tf2N] / AlCl3 electrolyte system, wherein the composite electrolyte system includes [Emim][Al2Cl7] and [Bmim][Al2Cl7] in a volume ratio of (1-2):(8-9).
[0026] Compared with existing technologies, the preparation and collection of nano-aluminum can be conveniently and quickly achieved through the combination of an electrolytic cell, a collection component, a stirring component, an electrolysis component, a liquid addition component, a liquid dispensing component, and a liquid measurement component. In particular, the nano-aluminum particles generated by electrolysis on aluminum cathode and aluminum anode components are stripped off by eddy current through the stirring component, and then collected by the collection component at the bottom of the cell body. The entire preparation, stripping, and collection process is smooth and simple. Attached Figure Description
[0027] The accompanying drawings, which are included to provide a further understanding of this application and form part of this application, illustrate exemplary embodiments and are used to explain this application, but do not constitute an undue limitation of this application. In the drawings:
[0028] Figure 1 This is a schematic diagram of the nano-aluminum preparation device based on ionic liquid electrolyte in the embodiment;
[0029] Figure 2 This is a cross-sectional view of the nano-aluminum preparation device based on ionic liquid electrolyte in the embodiment;
[0030] Figure 3 This is a schematic diagram of the structure of the stirring connector and the stirring component in the embodiment;
[0031] Figure 4 This is a schematic diagram of the eddies generated by the rotation of the stirring component in the embodiment;
[0032] Figure 5 This is a schematic diagram of the lower tank and the collection component in the embodiment;
[0033] Figure 6 This is a comparison diagram of the open and closed states of the filter mesh pores of the filter assembly in the embodiment;
[0034] Figure 7 This is another schematic diagram of the nano-aluminum preparation device based on ionic liquid electrolyte in the embodiment;
[0035] Figure 8 This is a schematic diagram of the structure of the filter assembly, tank body, and collection assembly in the embodiment;
[0036] Figure 9 This is another structural schematic diagram of the stirring connector and the stirring component in the embodiment;
[0037] Figure 10 This is a schematic diagram of another vortex generated by the rotation of the stirring component in the embodiment;
[0038] Figure 11 SEM images of the first group of samples;
[0039] Figure 12 EDS analysis chromatograms of the first group of samples;
[0040] Figure 13 SEM images of the second group of samples;
[0041] Figure 14 This is the EDS analysis spectrum of the second group of samples. Detailed Implementation
[0042] The following drawings disclose several embodiments of the present invention. For clarity, many practical details will be described in the following description. However, it should be understood that these practical details are not intended to limit the invention. That is, in some embodiments of the invention, these practical details are not essential. Furthermore, for the sake of simplicity, some conventional structures and components will be shown in the drawings in a simple schematic manner.
[0043] Furthermore, in this invention, the use of terms such as "first" and "second" is for descriptive purposes only and does not specifically refer to any order or sequence, nor is it intended to limit the invention. They are merely used to distinguish components or operations described using the same technical terms, and should not be construed as indicating or implying relative importance or implicitly specifying the number of indicated technical features. Therefore, a feature defined with "first" or "second" may explicitly or implicitly include at least one of those features. Additionally, the technical solutions of various embodiments can be combined with each other, but only if they are feasible for those skilled in the art. If a combination of technical solutions is contradictory or impossible to implement, such a combination should be considered nonexistent and not within the scope of protection claimed by this invention.
[0044] Example 1
[0045] Reference Figure 1 and Figure 2 , Figure 1 This is a schematic diagram of the nano-aluminum preparation device based on ionic liquid electrolyte in the embodiment. Figure 2 This is a cross-sectional view of the nano-aluminum preparation device based on ionic liquid electrolyte in this embodiment. The nano-aluminum preparation device based on ionic liquid electrolyte in this embodiment includes an electrolytic cell 1, a collection assembly 2, a stirring assembly 3, an electrolysis assembly 4, a liquid addition assembly 5, a liquid outlet assembly 6, and a liquid measurement assembly 7. The electrolytic cell 1 includes a cell body 11 and a cover plate 12, with the cover plate 12 covering the opening of the cell body 11. The collection assembly 2 is located inside the cell body 11 and at the bottom of the cell body 11. The stirring assembly 3 includes a stirring connector 31 and a stirring element 32. One end of the stirring connector 31 passes through the cover plate 12, and the other end extends towards the collection assembly 2. The stirring element 32 is located at the other end of the stirring connector 31. The electrolysis assembly 4 includes an aluminum cathode 41 and an aluminum anode 42, which are located inside the cell body 11 and arranged around the stirring element 32. One end of the liquid addition assembly 5 is located inside the cell body 11, and it is used to add ionic liquid electrolyte to the inside of the cell body 11. One end of the liquid outlet assembly 6 is located inside the tank body 11 and extends close to the collection assembly 2. It is used to extract the ionic liquid electrolyte inside the tank body 11. The liquid level measuring assembly 7 is used to detect the liquid level of the ionic liquid electrolyte inside the tank body 11.
[0046] The ionic liquid electrolyte is added to the tank body 11 through the liquid addition component 5, and then electrolysis is carried out through the aluminum cathode 41 and aluminum anode 42. At the same time, the eddy current generated by the stirring component 32 carries the nano-aluminum particles generated by electrolysis away from the electrode surface. The nano-aluminum particles are then deposited and collected by the collection component 2 at the bottom of the tank body 11. Then, the liquid discharge component 6 extracts the residual solution inside the tank body 11, and the liquid level is detected by the liquid level measuring component 7. After the preset liquid level is reached, the collection component 2 is removed, and the nano-aluminum particles are transferred, collected, and stored, thus enabling convenient and quick preparation and collection of nano-aluminum. In particular, this invention uses the stirring component 32 to peel off the nano-aluminum particles generated by electrolysis on the aluminum cathode 41 and aluminum anode 42 through the eddy current, and then the particles are naturally deposited to the bottom of the tank body 11 by the eddy current, and collected by the collection component 2. The entire process of nano-aluminum particle preparation, peeling, and collection is smooth, simple, and convenient.
[0047] Specifically, the tank body 11 is an open tank with internal space, and the collecting component 2 is located at the bottom of the tank body 11. A cover plate 12 covers the opening of the tank body 11, and its surface has multiple through holes that communicate with the internal space of the tank body 11, allowing the stirring connector 31, aluminum cathode 41, aluminum anode 42, liquid adding component 5, liquid discharging component 6, and liquid measuring component 7 to pass through the through holes and be supported by the cover plate 12. Preferably, each through hole of the cover plate 12 is provided with a hole sealing plug 121, which can be a rubber ring, to seal and isolate the internal space of the tank body 11 from the external atmosphere.
[0048] The aluminum cathode component 41 includes a first connecting rod 411 and a cathode electrode plate 412. The cathode electrode plate 412 is located inside the tank body 11. One end of the first connecting rod 411 is connected to the cathode electrode plate 412, and the other end passes through a through hole in the cover plate 12 for electrical connection to an external power source. Similarly, the aluminum anode component 42 includes a second connecting rod 421 and an anode electrode plate 422. The anode electrode plate 422 is located inside the tank body 11. One end of the second connecting rod 421 is connected to the anode electrode plate 422, and the other end passes through a through hole in the cover plate 12 for electrical connection to an external power source. The cathode electrode plate 412 and the anode electrode plate 422 are arranged around the stirring member 32. In this embodiment, the cathode electrode plate 412 and the anode electrode plate 422 are located on opposite sides of the stirring member 32. The first connecting rod 411, the stirring connector 31, and the second connecting rod 421 are arranged sequentially at intervals. The first connecting rod 411 and the second connecting rod 421 are equidistantly located on opposite sides of the stirring connector 31, and all three are perpendicular to the cover plate 12. In this embodiment, both the cathode electrode plate 412 and the anode electrode plate 422 are made of high-purity aluminum plates with a purity greater than 99.9%. In specific applications, electrolysis is achieved by energizing the first connecting rod 411 and the second connecting rod 421. In this embodiment, the ionic liquid electrolyte is a composite electrolyte system, which includes [Emim][Al2Cl7] and [Bmim][Al2Cl7] in a volume ratio of (1-2):(8-9). Toluene is added as an additive solvent. After electrolysis in the composite electrolyte system, the cathode electrode plate 412 and the anode electrode plate 422 will produce nano-aluminum particles.
[0049] Please refer to the following: Figure 3 and Figure 4 , Figure 3 This is a schematic diagram of the structure of the stirring connector and the stirring component in the embodiment. Figure 4This is a schematic diagram of the eddy currents generated by the rotation of the stirring element in the embodiment. The stirring assembly 3 includes a stirring driver (not shown in the figure), a stirring connector 31, and a stirring element 32. The driving end of the stirring driver is connected to one end of the stirring connector 31, and the other end of the stirring connector 31 passes vertically through the through hole of the cover plate 12 and connects to the stirring element 32 inside the tank body 11. The stirring connector 31 is a connecting rod, and the stirring driver can be a motor. The first connecting rod 411 and the second connecting rod 421 are located on opposite sides of the stirring connector 31, and the distance between the first connecting rod 411 and the stirring connector 31 is equal to the distance between the second connecting rod 421 and the stirring connector 31. This arrangement further ensures that the cathode electrode plate 412 and the anode electrode plate 422 are located on opposite sides of the stirring element 32, making it easier for the eddy currents generated on both sides of the stirring element 32 to carry away the nano-aluminum particles on the cathode electrode plate 412 and the anode electrode plate 422.
[0050] Preferably, the stirring element 32 is a propeller-type stirring fan blade. In specific applications, the stirring assembly 3 can be a propeller-type stirrer. For example... Figure 3 and Figure 4 As shown, when the propeller-type stirring blades rotate, they carry the nano-aluminum particles generated by the cathode electrode plate 412 and the anode electrode plate 422 away from the electrode surface through radial flow. Preferably, the collection component 2 is a conical tower. It can be understood that the eddies generated by the stirring element 32 of the propeller-type stirring blades are mainly concentrated on both sides, which can better carry away the nano-aluminum particles generated by the cathode electrode plate 412 and the anode electrode plate 422 on opposite sides of the stirring element 32. Moreover, the generated nano-aluminum particles are also carried to both sides. By setting the collection component 2 as a conical tower, collection grooves are formed on both sides of the bottom of the tank body 11, which makes it easier to collect the nano-aluminum particles on both sides. That is to say, in this embodiment, the nano-aluminum particle collection groove is specifically formed by the space between the inner wall of the bottom of the tank body 11 and the outer wall of the conical tower.
[0051] The liquid addition assembly 5 is a liquid addition pipe connected to an external storage device for the ionic liquid electrolyte. It can quantitatively add ionic liquid electrolyte to the tank body 11, facilitating the addition or replenishment of the ionic liquid electrolyte within the tank body 11. The liquid discharge assembly 6 is a liquid discharge pipe connected to an external pump, used to extract residual ionic liquid electrolyte from the tank body 11. The extracted ionic liquid electrolyte can be recycled and regenerated before being returned to the storage device. Both the storage device and the pump can be existing devices, and will not be described in detail here. The liquid level measurement assembly 7 is a liquid level detection device. In practical applications, an existing liquid level detector can be used to detect the capacity of the ionic liquid electrolyte inside the tank body 11, facilitating the control of replenishment and extraction of the ionic liquid electrolyte. It also allows for real-time monitoring of the remaining ionic liquid electrolyte in the tank body 11, facilitating the control of the electrolysis reaction.
[0052] Rereference Figure 1 and Figure 2 The nano-aluminum preparation apparatus based on ionic liquid electrolyte in this embodiment also includes a temperature detection component 9, which is used to detect the temperature of the ionic liquid electrolyte inside the tank body 11. Specifically, the temperature detection component 9 passes through a through hole in the cover plate 12, and a silicone ring is installed inside the through hole for sealing. The detection end of the temperature detection component 9 is located inside the tank body 11 to monitor the temperature of the ionic liquid electrolyte inside the tank body 11, thereby facilitating the control of the ionic liquid electrolysis temperature in the tank body 11 and ensuring that the ionic liquid electrolyte system can be prepared at the required temperature. The temperature detection component 9 can be a thermometer, and the temperature control of the liquid inside the tank body 11 can use an existing temperature control system, which will not be elaborated here.
[0053] Please refer to the following: Figure 1 , Figure 2 and Figure 5 , Figure 5 This is a schematic diagram of the lower tank and the collection component in the embodiment. Furthermore, the tank body 11 includes an upper tank 111 and a lower tank 112. The lower tank 112 is detachably connected to the lower end of the upper tank 111, and the collection component 2 is located inside the lower tank 112. A sealing treatment is applied between the upper tank 111 and the lower tank 112. Dividing the tank body 11 into the upper tank 111 and the lower tank 112 allows for a detachable connection of the lower tank 112, which carries the collection component 2, facilitating the collection of nano-aluminum particles.
[0054] Specifically, the tank body 11 also includes a snap-fit structure 113, which can be disposed on the outer wall of the upper tank body 111 and the lower tank body 112. The upper tank body 111 and the lower tank body 112 have matching grooves and protrusions at their opposite ends, and the grooves have corrosion-resistant sealing rings to prevent the leakage of ionic liquid electrolytes. After the upper tank body 111 and the lower tank body 112 are joined, they are secured by the snap-fit structure 113 on the outer wall. Alternatively, a snap-fit connection structure with a corrosion-resistant sealing ring can be directly disposed at the joint ends of the upper tank body 111 and the lower tank body 112.
[0055] At this point, the conical tower-shaped collecting component 2 is positioned at the bottom of the lower tank 112, forming a collecting trough between the outer wall of the conical tower and the lower tank 112. After the electrolysis reaction is complete, the pump extracts the liquid, i.e., the ionic liquid electrolyte, from the main tank 11 through the liquid outlet component 6 until the liquid level in the main tank 11 is detected by the liquid measuring component 7 to have dropped to a preset position in the lower tank 112, for example, the position of the tip of the conical tower of the collecting component 2. At this point, the pumping stops. The lower tank 112 is then disassembled from the upper tank 111, and the entire lower tank 112 can be transferred to collect the nano-aluminum particles.
[0056] Please refer to the following: Figure 6 , Figure 6 This is a comparison diagram of the open and closed states of the filter mesh assembly in this embodiment. The nano-aluminum preparation device based on ionic liquid electrolyte in this embodiment also includes a filter mesh assembly 8; the filter mesh assembly 8 is located at the opening of the lower tank 112, between the collection assembly 2 and the stirring element 32. The filter mesh assembly 8 has a closed mesh structure. It is understood that during the electrolytic preparation process, the anode electrode plate is continuously consumed. This consumption is not uniform; the electrode is consumed faster at the electrolyte interface. This poses a risk of the anode electrode plate breaking and falling during electrolytic preparation. To prevent the fallen anode electrode plate from falling directly into the bottom "conical tower" type collection tank and becoming difficult to remove, a filter mesh assembly 8 is set at the opening of the lower tank 112. The dense pores ensure that the prepared nano-aluminum particles can fall into the collection tank, while the fallen anode will only remain above the filter mesh assembly 8 and will not fall into the collection tank, thus avoiding the risk of device damage.
[0057] In practical applications, the filter screen pores of the filter assembly 8 are open during electrolysis. After electrolysis, when it is necessary to collect the nano-aluminum particles in the lower tank 112, the filter screen pores of the filter assembly 8 need to be closed to seal the opening of the lower tank 112, preventing the ionic liquid electrolyte inside the lower tank 112 from splashing out, and also isolating the internal and external environments of the lower tank 112. In practical applications, existing filter structures with closable pores can be used. For example, the filter assembly 8 can be equipped with upper and lower filter screens. The lower filter screen can be moved by a knob 81. The lower filter screen has a plate-like structure that blocks the filter pores of the upper filter screen. By rotating the knob 81, the lower filter screen is misaligned with the upper filter screen, blocking the filter pores of the upper filter screen, thereby achieving spatial isolation between the upper and lower sides of the filter assembly 8. This structure can refer to existing technology and will not be elaborated here.
[0058] The nano-aluminum particles deposited in the collection tank of the disassembled lower tank 112 are transferred to a container containing an ethanol solution. After the nano-aluminum particles are transferred to the ethanol solution, they are washed with the ethanol solution 3 to 4 times. The agglomerated nano-aluminum particles are then broken up under ultrasonic conditions. After that, they are centrifuged and separated by a high-speed centrifuge and collected and stored to obtain the desired nano-aluminum particles.
[0059] Example 2
[0060] Continue to refer to Figure 7-10 , Figure 7 This is another schematic diagram of the nano-aluminum preparation device based on ionic liquid electrolyte in the embodiment. Figure 8 This is a schematic diagram of the structure of the filter assembly, tank body, and collection assembly in the embodiment. Figure 9 This is another structural schematic diagram of the stirring connector and the stirring component in the embodiment. Figure 10This is a schematic diagram of another eddy current generated by the rotation of the stirring element in this embodiment. The nano-aluminum preparation device based on ionic liquid electrolyte in this embodiment differs from the nano-aluminum preparation device based on ionic liquid electrolyte in Embodiment 1 in that: the tank body 11 is a single piece. The collecting component 2 is a conical tank, which is located at the bottom of the tank body 11, with the opening of the conical tank facing the stirring element 32. The conical collecting component 2 directly collects the electrolytically deposited nano-aluminum particles. The stirring element 32 is a turbine-type stirring fan. In specific applications, the stirring component 3 can be a turbine-type stirrer. Figure 9 and Figure 10 As shown, the turbine-type stirring blades of the stirring component 32 can generate a strong radial flow to carry the nano-aluminum particles away from the electrode surface and prevent them from sticking to the wall. At the same time, the radial flow at the bottom, combined with the conical groove-shaped collection component in the form of an "inverted conical tower," facilitates the deposition of nano-aluminum particles to the bottom of the collection component 2, thus making collection easier. Moreover, the turbine-type stirrer can still perform good stirring in electrolytes with medium to high viscosity, resulting in good application performance. Therefore, the ionic liquid electrolyte in this embodiment can be a higher viscosity [BmPy][Tf2N] / AlCl3 electrolyte system.
[0061] The liquid measuring component 7 in this embodiment can adopt the method in Embodiment 1, or it can adopt a physical detection method, such as intuitively understanding the remaining amount of ionic liquid electrolyte in the tank body 11 through the liquid level tube.
[0062] Preferably, in this embodiment, the filter assembly 8 is disposed within the tank body 11 and located between the collecting assembly 2 and the stirring member 32. The filter assembly 8 has a closed mesh structure. In this embodiment, the filter assembly 8 is provided with a handle 82. The handle 82 can function as the knob 81 in Embodiment 1. After the preparation reaction is completed, rotating the handle 82 closes the holes of the porous filter device of the filter assembly 8. It can also be used as a handle to lift the entire collecting assembly 2 upwards. The specific filter assembly 8 can adopt an existing structure, which will not be described in detail here. Subsequently, the nano-aluminum particles deposited in the collecting assembly 2 are transferred to an ethanol solution. After washing with the ethanol solution 3-4 times, the agglomerated nano-aluminum particles are dispersed under ultrasonic conditions. Then, they are centrifuged using a high-speed centrifuge and collected for storage.
[0063] The above Examples 1 and 2 are merely illustrative examples. In specific applications, different stirring blades can be selected based on the viscosity of the ionic liquid electrolyte. Furthermore, the function of each stirring blade determines whether to use the collection component 2 structure from Example 1 or Example 2. In this invention, because the [BmPy][Tf2N] / AlCl3 ionic liquid electrolyte has a high viscosity, the stirring blade structure from Example 2, suitable for high-viscosity liquids, is selected. Then, based on the different material mixing methods caused by the stirring blades, the "inverted conical tower" type conical trough-shaped collection component 2 is selected.
[0064] Example 3
[0065] The method for preparing nano-aluminum based on ionic liquid electrolyte in this embodiment includes the following steps:
[0066] S1, to prepare ionic liquid electrolytes.
[0067] S2, Nano-aluminum is prepared using the nano-aluminum preparation apparatus of ionic liquid electrolyte in Example 1 or Example 2.
[0068] S3, the nano-aluminum particles prepared by the nano-aluminum preparation device for ionic liquid electrolyte are washed and collected.
[0069] In step S1, the ionic liquid electrolyte includes either a composite electrolyte system or a [BmPy][Tf2N] / AlCl3 electrolyte system. The composite electrolyte system comprises [Emim][Al2Cl7] and [Bmim][Al2Cl7] in a volume ratio of (1–2):(8–9). In practical applications, toluene is added as a solvent to the composite electrolyte system. The [BmPy][Tf2N] / AlCl3 electrolyte system does not add toluene as an additive because the two are incompatible and the reaction temperature is too high.
[0070] The preparation process of the composite electrolyte system in this embodiment is as follows:
[0071] First, [Emim][Al2Cl7] ionic liquid and [Bmim][Al2Cl7] ionic liquid, namely 1-ethyl-3-methylimidazolium chloroaluminate and 1-butyl-3-methylimidazolium chloroaluminate, were prepared respectively.
[0072] The synthesis steps of the [Emim][Al2Cl7] ionic liquid are as follows:
[0073] The first step is the synthesis of [Emim]Cl, and its chemical formula is as follows.
[0074] C4H6N2 + C2H5Cl → [Emim]Cl
[0075] The second step is the synthesis of [Emim][Al2Cl7], the chemical formula of which is as follows.
[0076] [Emim]Cl+AlCl3→[Emim][AlCl4]
[0077] [Emim][[AlCl4]+AlCl3→[Emim][Al2Cl7]
[0078] The synthesis steps of the [Bmim][Al2Cl7] ionic liquid are as follows:
[0079] The first step is the synthesis of [Bmim]Cl, and its chemical formula is as follows.
[0080] C4H6N2 + C4H9Cl → [Bmim]Cl
[0081] The second step is the synthesis of [Bmim][Al2Cl7], the chemical formula of which is as follows.
[0082] [Bmim]Cl+AlCl3→[Bmim][AlCl4]
[0083] [Bmim][AlCl4]+AlCl3→[Bmim][Al2Cl7]
[0084] Then, [Emim][Al2Cl7] and [Bmim][Al2Cl7] in a volume ratio of (1-2):(8-9) were uniformly mixed, and toluene was added as a solvent to obtain a composite electrolyte system.
[0085] The molar ratio of aluminum chloride (AlCl3) to two imidazole chloride ionic liquids ([Emim]Cl and [Bmim]Cl) is 2:1, where [Emim]Cl / AlCl3 and [Bmim]Cl / AlCl3 are single liquid phases. When mixing, the two ionic liquid electrolytes to be mixed are mixed at a volume ratio of 10:90 or 20:80 under the condition of 20-60℃, stirred for 1-2 hours, and then allowed to stand for 1 hour.
[0086] This invention proposes a composite electrolyte system, specifically a composite ionic liquid electrolyte system. It utilizes two ionic liquids, [Emim][Al₂Cl₇] and [Bmim][Al₂Cl₇], which are easier to prepare, cheaper, and have suitable viscosity and conductivity. In practical applications, toluene is added as an additive to utilize its solvation effect and promote the electrolytic generation of aluminum nanoparticles within the composite ionic liquid electrolyte. This type of composite ionic liquid electrolyte combines the advantages of simple and low-cost manufacturing processes of [Emim][Al₂Cl₇] and [Bmim][Al₂Cl₇], with the excellent co-solvent effect of toluene, resulting in a composite ionic liquid electrolyte system with promising applications in the future nano-aluminum preparation industry.
[0087] The synthesis process of the [BmPy][Tf2N] / AlCl3 ionic liquid electrolyte, namely 1-butyl-1-methylpyrrolidine bis(trifluoromethanesulfonylimide) / aluminum trichloride, is as follows:
[0088] The first step is the synthesis of [BmPy]Br, and its chemical formula is as follows.
[0089] C5H 11 N+C4H9Br→[BmPy]Br
[0090] The second step is the synthesis of [BmPy][Tf2N], whose chemical formula is as follows.
[0091] [BmPy]Br+Li[N(CF3SO2)2]→[BmPy][Tf2N]+LiBr
[0092] The third step is the synthesis of [BmPy][Tf2N] / AlCl3, and its chemical formula is as follows.
[0093] [BmPy][Tf2N]+AlCl3→[BmPy][Tf2N] / AlCl3
[0094] The molar ratio of aluminum chloride (AlCl3) to [BmPy][Tf2N] ionic liquid is 1:0.5 to 1.0, the reaction temperature is 20-100℃, and the resulting electrolyte system [BmPy][Tf2N] / AlCl3 ionic liquid electrolyte has two phases, with the upper phase being the electrolyte used in electrolysis.
[0095] It is understandable that the [BmPy][Tf2N] / AlCl3 ionic liquid electrolyte contains [BmPy] +The more concentrated charge distribution in cations weakens the interaction between anions and cations, thus facilitating the formation of nanoscale aluminum electrodeposition. However, due to its inherent properties, the [BmPy][Tf2N] / AlCl3 ionic liquid electrolyte has a higher viscosity and lower conductivity compared to the [Emim][Al2Cl7] and [Bmim][Al2Cl7] ionic liquid electrolytes, and it exhibits a two-phase system after preparation, making its application more difficult. To address this issue, the nano-aluminum preparation apparatus based on ionic liquid electrolyte in Embodiment 2 can monitor the temperature inside the tank body 11 using the temperature detection component 9. By controlling the reaction temperature and adding a stirring device, the purpose of preparing nano-aluminum by electrolysis in a high-viscosity [BmPy][Tf2N] / AlCl3 ionic liquid electrolyte can be achieved. Simultaneously, with the help of the turbine-type stirring paddle of the stirring component 32 and the conical collection component 2 ("inverted conical tower"), the generated nano-aluminum particles are carried away from the electrode surface by the radial flow generated by the turbine-type stirring paddle blades and naturally precipitated in the conical collection component 2. After the reaction is completed, the collection component is removed, and the nano-aluminum particles are processed, collected, and stored.
[0096] To further illustrate step S2, the nano-aluminum preparation devices based on ionic liquid electrolytes in Examples 1 and 2 were used to prepare nano-aluminum particles using a composite electrolyte system and a [BmPy][Tf2N] / AlCl3 electrolyte system, respectively. The specific processes are as follows.
[0097] This step will use the ionic liquid electrolytes listed in Table 1 as experimental examples. Referring to Table 1, which shows the composition of the composite ionic liquid electrolyte and [BmPy]... + Reference table for basic ionic liquid electrolyte systems.
[0098] <![CDATA[[Emim][Al2Cl7]]]> <![CDATA[[Bmim][Al2Cl7]]]> <![CDATA[[BmPy][Tf2N] / AlCl3]]> Toluene 1# 10ml 90ml 0 20ml 2# 20ml 80ml 0 20ml 3# 0 0 100ml 0
[0099] Table 1
[0100] S21, the composite ionic liquid electrolytes of Experimental Examples 1 and 2 in Table 1 are added to the tank body 11 of the nano-aluminum preparation device based on ionic liquid electrolyte in Example 1, and the [BmPy][Tf2N] / AlCl3 of Experimental Example 3 in Table 1 is added to the tank body 11 of the nano-aluminum preparation device based on ionic liquid electrolyte in Example 2.
[0101] S22, a constant current is applied to the first connecting rod 411 and the second connecting rod 421 respectively. The constant current is a DC current of 30-80mA, and in this embodiment, the constant current is a DC current of 40mA. The cathode electrode plate 412 and the anode electrode plate 422, with an aluminum purity >99.9%, are used as the cathode and anode of the electrolysis reaction.
[0102] The electrolytic preparation reaction is as follows:
[0103] Anode reaction:
[0104] Cathode reaction: 4Al2Cl 7- +3e - →Al+7AlCl 4-
[0105] The reaction temperature during the preparation process is 20–100℃, the electrode spacing is 2–4 cm, and the electrolysis time is 48–96 h. In Example 1, the reaction temperature of the nano-aluminum preparation device based on ionic liquid electrolyte is 40℃, the electrode spacing is 3 cm, and the electrolysis time is 72 h. In Example 2, the reaction temperature of the nano-aluminum preparation device based on ionic liquid electrolyte is 60℃, the electrode spacing is 3 cm, and the electrolysis time is 72 h.
[0106] At the same time, the eddy current generated by the rotation of the stirring element 32 carries the nano-aluminum particles away from the electrode surface and deposits them towards the bottom of the tank body 11.
[0107] S23. After the reaction is complete, the nano-aluminum particles are mainly deposited at the bottom of the tank body 11. At this time, it is necessary to let it stand for 4-8 hours before removing the anode and cathode from the tank body 11. Use a scraper to scrape off the nano-aluminum particles attached to the cathode, and then extract the ionic liquid from the tank body 11 for use in the next electrolytic preparation.
[0108] Step S3: Transfer the nano-aluminum particles deposited at the bottom of the tank body 11 to an ethanol solution, wash with ethanol solution 3 to 4 times, break up the agglomerated nano-aluminum particles under ultrasonic conditions, and then collect and store them after centrifugation with a high-speed centrifuge.
[0109] The entire process described above must be carried out in an inert gas atmosphere filled with nitrogen or argon gas of higher purity than 99.99%.
[0110] Refer to Table 2, which shows the composition of the composite ionic liquid electrolyte and [BmPy]. + The size and purity of the nano-aluminum particles obtained after the above electrolysis process in the basic ionic liquid electrolyte system.
[0111] Ionic liquid electrolyte number Aluminum particle size Aluminum particle purity 1# 300nm~500nm 98.99% 2# 500nm~1000nm 98.60% 3# <100nm 96.77%
[0112] Table 2
[0113] Using the same preparation conditions as described above, a control experiment was conducted. Refer to Table 3, which shows the composition of the ionic liquid electrolytes in each group of the control experiments:
[0114]
[0115]
[0116] Table 3
[0117] Referring to Table 4, which shows the aluminum particle size and purity obtained in each group of ionic liquid electrolyte systems in the control experiment:
[0118] Ionic liquid electrolyte number Aluminum particle size Aluminum particle purity 1# 2~3μm 99.04% 2# 3μm 99.23% 3# ~25μm 99.47% 4# 4~5μm 99.47% 5# <1μm 98.96% 6# <1μm 98.61% 7# N / A N / A
[0119] Table 4
[0120] In Table 4, Group 7 cannot be prepared by electrolysis because [BmPy][Tf2N] / AlCl3 is not well compatible with the toluene additive and cannot form a usable liquid electrolyte system.
[0121] Please refer to the following: Figures 11 to 14 , Figure 11 This is the SEM image of the first group of samples. Figure 12 This is the EDS analysis chromatogram of the first group of samples. Figure 13 This is a SEM image of the second group of samples. Figure 14 This is the EDS analysis spectrum of the second group of samples. Nano-aluminum particles were placed on the SEM sample stage, compacted, and then the SEM image was taken.
[0122] By combining the composite ionic liquid electrolyte and [BmPy] in Table 2... + The following conclusions can be drawn from the comparison of the aluminum particle size and purity obtained in the basic ionic liquid electrolyte system with the data in Table 4 of the control group:
[0123] First, comparing the two sets of data (1#), it can be seen that the aluminum particles obtained by electrolysis in the ionic liquid electrolyte without added toluene are in the micrometer range, while the aluminum particles obtained in the ionic liquid electrolyte with added toluene are in the nanometer range. Figure 11 As shown, although its purity is slightly lower, analysis revealed that this is mainly due to the easy oxidation of nano-sized aluminum particles in air, leading to a decrease in purity. Subsequent purity analysis also confirmed this. EDS purity analysis showed that the impurities were primarily oxygen, caused by the oxidation of the nano-aluminum particles. Figure 12 As shown.
[0124] Secondly, comparing the two sets of data #2 shows that as the [Emim]Cl / AlCl3 ratio increases, the size of the aluminum particles increases, but they still remain at the nanoscale, although their particle size distribution becomes wider. Figure 13As shown, its purity is also slightly lower, mainly due to oxidation. In the control group, the aluminum particles are tightly attached to the electrode plates, so their oxidation is weaker. In the preparation of nano-aluminum, the aluminum particles need to be detached from the electrode plates and then collected. Therefore, the aluminum particles obtained have a larger surface area and are more easily oxidized compared to the attached aluminum.
[0125] Third, based on the data in Tables 1 and 2 (number 3), it can be concluded that [BmPy] is a cation... + The ionic liquid-based electrolyte system can directly produce nanoscale aluminum products with particle sizes smaller than 100 nm without the addition of additives. However, the nanoscale aluminum products obtained from this electrolyte have strong adhesion, requiring a scraper to remove the nanoscale aluminum deposits from the electrode surface before use. This process easily leads to severe oxidation of the nanoscale aluminum products, resulting in low product quality and purity. Simultaneously, the electrolyte has the disadvantage of high viscosity, requiring a dedicated electrolysis device for preparation. However, this electrolyte system has the advantage of being stable in water and air, making it suitable for use in conventional environments without the need for strict dehydration and deoxygenation procedures. With the use of a dedicated electrolysis device, it has considerable market application potential in the future.
[0126] Furthermore, due to [BmPy] + The ionic liquid electrolyte system based on toluene is incompatible with toluene, therefore toluene cannot be used as an additive to help improve its conductivity and viscosity, as has been confirmed by experiment #7 in the control experiment.
[0127] Fourth, comparing the data from experiments 3# to 6# in control examples with the experimental data from experiments 1# and 2# in experimental examples, it can be seen that, without mixing, simply adding toluene to [Emim]Cl / AlCl3 and [Bmim]Cl / AlCl3 can disrupt the regular arrangement of anions and cations at the electrode-ionic liquid electrolyte interface through solvation, thus producing some nanoscale aluminum particles. However, the particle size distribution is relatively large, and some micron-sized aluminum deposits also exist. Furthermore, the nanoscale aluminum particles prepared without ionic liquid doping have strong adhesion and will firmly adhere to the electrode surface, which is not conducive to the final collection of nanoscale aluminum products. By combining the two ionic liquid electrolytes, the electronic layer composition of the original cathode electrode surface can be changed, making the aluminum deposit layer formed during the electrode deposition process at the electrode interface more porous, with poorer adhesion and more dendrite formation. Combined with the radial flow created by mechanical stirring, the nanoscale aluminum deposit particles are automatically detached from the electrode surface and fall to the bottom of the electrolytic cell, facilitating collection.
[0128] In summary, toluene additives can significantly reduce the particle size of the final aluminum deposit, thereby helping to obtain nanoscale aluminum deposited particles. The combination of the two ionic liquids weakens the adhesion of aluminum particles to the electrode, improves dendrite formation, and makes the structure of the aluminum deposit layer more porous, thus making it easier to detach from the electrode.
[0129] In summary, the nano-aluminum preparation device and method based on ionic liquid electrolytes in this embodiment can conveniently and quickly realize the preparation and collection of nano-aluminum.
[0130] The above description is merely an embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principle of the present invention should be included within the scope of the claims of the present invention.
Claims
1. A method for preparing nano-aluminum based on ionic liquid electrolytes, characterized in that, Includes the following steps: Preparation of ionic liquid electrolytes; the ionic liquid electrolytes include a composite electrolyte system, the composite electrolyte system comprising a [Emim][Al] mixture with a volume ratio of (1~2):(8~9). Cl ] and [Bmim][Al Cl [, and by adding toluene as an additive solvent; by combining the two ionic liquid electrolytes, the electronic layer composition on the original cathode electrode surface can be changed, making the aluminum deposition layer formed by the electrode deposition process at the electrode interface more porous, with poorer adhesion and more dendrite phenomena. Nano-aluminum is prepared using an ionic liquid electrolyte nano-aluminum preparation device; wherein, the nano-aluminum preparation device includes an electrolytic cell (1), a collection component (2), a stirring component (3), an electrolysis component (4), a liquid addition component (5), a liquid dispensing component (6), and a liquid measuring component (7); the electrolytic cell (1) includes a cell body (11) and a cover plate (12), the cover plate (12) covering the opening of the cell body (11); the collection component (2) is located inside the cell body (11) and at the bottom of the cell body (11); the stirring component (3) includes a stirring connector (31) and a stirring element (32), one end of the stirring connector (31) passing through the cover plate (12), and the other end facing the collection component (32). The collecting component (2) extends, and the stirring element (32) is located at the other end of the stirring connector (31); the electrolysis component (4) includes an aluminum cathode (41) and an aluminum anode (42), the aluminum cathode (41) and the aluminum anode (42) are located inside the tank body (11) and are arranged around the stirring element (32); one end of the liquid adding component (5) is located inside the tank body (11), and it is used to add ionic liquid electrolyte to the tank body (11); one end of the liquid discharging component (6) is located inside the tank body (11) and extends close to the collecting component (2); the liquid measuring component (7) is used to detect the liquid level of the ionic liquid electrolyte inside the tank body (11).
2. The method for preparing nano-aluminum based on ionic liquid electrolyte according to claim 1, characterized in that, The stirring component (32) is a propeller-type stirring fan blade or a turbine-type stirring fan blade.
3. The method for preparing nano-aluminum based on ionic liquid electrolyte according to claim 1, characterized in that, The collection component (2) is a conical tower or a conical trough.
4. The method for preparing nano-aluminum based on ionic liquid electrolyte according to claim 1, characterized in that, The main body of the tank (11) includes an upper tank (111) and a lower tank (112). The lower tank (112) is detachably connected to the lower end of the upper tank (111). The collection component (2) is located inside the lower tank (112). The upper tank (111) and the lower tank (112) are sealed together.
5. The method for preparing nano-aluminum based on ionic liquid electrolyte according to claim 4, characterized in that, It also includes a filter assembly (8); the filter assembly (8) is located at the opening of the lower tank (112) and between the collection assembly (2) and the stirring component (32).
6. The method for preparing nano-aluminum based on ionic liquid electrolyte according to claim 1, characterized in that, It also includes a filter assembly (8); the filter assembly (8) is disposed inside the tank body (11) and located between the collection assembly (2) and the stirring component (32).
7. The method for preparing nano-aluminum based on ionic liquid electrolyte according to claim 5 or 6, characterized in that, The filter assembly (8) has a closed mesh structure.
8. The method for preparing nano-aluminum based on ionic liquid electrolyte according to claim 1, characterized in that, It also includes a temperature detection component (9) for detecting the temperature of the ionic liquid electrolyte inside the tank body (11).
Citation Information
Patent Citations
Method for preparing nanometer aluminum or nanometer aluminum coating in low-temperature electro-deposition form by using ion liquid / additive system
CN102888630A
Electrolyte circulating tank capable of filtering and collecting silver powder
CN213232531U
Nano-aluminum preparation device based on ionic liquid electrolyte
CN220335322U