A method for manufacturing a down conductor cable for a pre-embedded lightning arrester in a wind turbine blade.
By manufacturing small-diameter down conductor cables using a specific process, the economic and performance issues of down conductor cables in wind turbine lightning protection systems have been resolved. This has enabled the manufacture of high-performance, long-life cables suitable for lightning protection systems of wind turbine generators and other electrical equipment.
Patent Information
- Application Number
- CN202310425209.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-20
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-04-20
AI Technical Summary
In the existing technology, the design of the down conductor cable used in the wind turbine lightning protection system, which combines the inside and outside of the wind turbine blade, has economic problems, and it is difficult to meet the requirements for small wire diameter and long service life.
Small-diameter downlead cables are manufactured using specific processes, including the production of tinned copper monofilaments, stranded conductors, double-layer co-extruded shielding and insulation layers, and extrusion processes for the outer sheath. Salt spray resistant and low-temperature resistant cable materials are used to ensure the cable's mechanical properties, flexibility, and low-temperature resistance.
It achieves high-performance manufacturing of small-diameter down conductor cables, possessing excellent mechanical properties, flexibility, salt spray resistance, and low-temperature resistance, extending the cable's service life, meeting wind turbine lightning protection requirements, and suitable for complex working conditions.
Smart Images

Figure CN116403782B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of cable manufacturing technology, specifically a method for manufacturing a down conductor cable for a pre-embedded lightning arrester in a wind turbine blade. Background Technology
[0002] In the current technology, wind turbines are mostly located at high altitudes or in open areas, and the electrical equipment inside the turbines is concentrated. These factors make the wind turbines more susceptible to lightning strikes and their impact.
[0003] In existing technologies, wind turbine lightning protection systems involve installing lightning arresters at the tips of the wind turbine blades, embedding down conductors within the blades, connecting the lightning arresters to the blade roots via the down conductors, and then further connecting to the grounding terminal via down conductors outside the blades. For example, Chinese patent ZL201080010748X describes a "wind turbine blade with a lightning protection system," in which a specifically designed down conductor is embedded. Since the down conductors inside the blades are short and used in small quantities, designing and manufacturing down conductors solely for use inside the blades is uneconomical. Therefore, the down conductors inside and outside the blades can be combined into one cable with a specific structural design. This type of cable is characterized by its small diameter, suitability for coastal and mountainous environments, and long lifespan, while also meeting the functional / performance requirements of the down conductor itself. Therefore, its structure puts forward new requirements for production, especially the down conductor, which needs to have small wire diameter and long service life. It also puts forward new requirements for the cable material used in the new structure cable and the process of wrapping the cable material on the cable. Summary of the Invention
[0004] This invention proposes a new manufacturing process for downleader cables with a novel structure. This process allows for the production of small-diameter downleader cables while meeting all cable performance requirements, thus solving the aforementioned technical problems.
[0005] A method for manufacturing a down conductor cable for a pre-embedded lightning arrester on a wind turbine blade includes the following steps:
[0006] 1) Fabricate conductors according to the specified cross-sectional area, and set aside for later use;
[0007] 2) Take the conductor obtained in step 1) and extrude the shielding layer and insulation layer to obtain the wire core;
[0008] 3) In step 2), an outer sheath layer is formed around the wire core;
[0009] In step 1),
[0010] 1.1) Fabrication of Metal Monofilaments: A copper rod is drawn into a copper monofilament corresponding to the required conductor diameter. The tolerance of the copper monofilament is controlled within ±1%d, where d is the diameter. During drawing, the lubricant temperature and cooling water temperature are controlled between 20 and 49°C, the annealing coefficient is 8.0 ± 0.2, the elongation of the copper monofilament is ≥25%, and the resistivity of the copper monofilament does not exceed 0.017700 Ω·mm. 2 / m;
[0011] 1.2) Tin plating treatment on copper monofilament: the concentration of acid in the electroplating solution is controlled within the range of (170~220) mL / L, the temperature is controlled within the range of (40~50)℃, the pH value of the washing solution is controlled within the range of 8.5~10.0, and the plating thickness of the round copper wire after tin plating is (6.00±0.50)μm.
[0012] 1.3) Use a wire bundling machine to bundle and twist metal monofilaments into conductors: the direction of strand bundling is right-hand Z, and the pitch ratio is 15 to 17 times; when re-twisting, each layer is set to left-hand S, the pitch ratio of the inner layer is 13 to 16 times, and the pitch ratio of the outer layer is 12 to 14 times.
[0013] 1.4) Non-woven fabric tape is wrapped tightly around the conductor in overlapping layers;
[0014] In step 2),
[0015] The shielding layer and the insulation layer are manufactured using a double-layer co-extrusion process to obtain the wire core;
[0016] The semi-conductive inner shielding cable material used in the inner shielding layer is a cable material whose performance meets the requirements of thermoplastic semi-conductive shielding material for PSD conductors in JB / T 10738-2007;
[0017] The outer insulation layer uses a salt spray resistant and low-temperature resistant flexible elastomer insulation material;
[0018] The process parameters for double-layer co-extrusion are set as follows:
[0019] The shielding layer is extruded using a Φ70 extruder. Along the feed to discharge direction, the temperatures of the first to sixth temperature zones of the extruder are 145±5℃, 155±5℃, 165±5℃, 170±5℃, 170±5℃ and 175±5℃ respectively. The screw speed of the extruder is 15.0 rpm.
[0020] The insulation layer is extruded using a Φ90 extruder. Along the feed to discharge direction, the temperatures of the first to sixth temperature zones of the extruder are 145±5℃, 150±5℃, 165±5℃, 175±5℃, 175±5℃ and 175±5℃ respectively. The screw speed of the extruder is 20.0 rpm.
[0021] The die dimensions for the double-layer co-extrusion are: core Φ12.4mm, die sleeve Φ18.6mm;
[0022] The average linear speed of the production line is 15 ± 0.3 m / min;
[0023] In step 3),
[0024] The outer sheath layer is manufactured using an extrusion process to obtain the cable product;
[0025] The outer sheath layer uses salt spray and low temperature resistant PVC sheath material;
[0026] The extrusion process parameters are set as follows: using a Φ120 extruder, the temperatures of the first to tenth temperature zones of the extruder along the feed to discharge direction are 126±5℃, 140±5℃, 148±5℃, 150±5℃, 150±5℃, 152±5℃, 153±5℃, 153±5℃, 154±5℃ and 155±5℃ respectively, and the screw speed of the extruder is 12.0 rpm;
[0027] The dimensions of the extrusion mold for the sheath are: core Φ28.0mm, sleeve Φ35.0mm;
[0028] The average line speed of the production line is 10 ± 0.5 m / min.
[0029] Steps 1.1) to 1.3) yield a conductor with a DC resistance of <0.277Ω / km at 20℃; the outer diameter of the conductor is 11.6±0.2mm.
[0030] In step 1.4), the thickness of the nonwoven tape is 0.10 mm, the width is 25 mm, and the overlap rate of the wrapping is 15% to 17%; the outer diameter of the cable after wrapping is 11.9 ± 0.2 mm.
[0031] To meet the requirements of cable application scenarios and reduce the insulation layer thickness while satisfying various cable performance requirements, the formulation system of the salt spray and low temperature resistant flexible elastomer insulation material specifically used in this method is shown in Table 1:
[0032] Table 1 shows the composition of the insulation material by weight of the following raw materials.
[0033] Serial Number Material Name Number of parts by weight / part 1 SEBS 10-30 2 Propylene elastomer 20-40 3 polypropylene 10-20 4 White oil 8-20 5 Masterbatch 3-5 6 Silicone Masterbatch 3-5 7 Nitrogen-phosphorus flame retardants 35-45 8 antioxidants 0.5-1.5 9 lubricant 0.8-1.5
[0034] In this insulation material, 10-20 parts of block copolymer polypropylene are added to improve the overall salt spray resistance. To enhance the material's flame retardancy and extrusion processability, propylene elastomer is introduced to replace part of the polypropylene, while the amount of oil-extended SEBS is reduced. This ensures both material flexibility and improved low-temperature resistance. Polypropylene and SEBS resins possess excellent electrical properties, while SEBS and propylene elastomer exhibit good low-temperature resistance. The selected block copolymer polypropylene, containing ethylene-propylene copolymer monomers, boasts the best low-temperature resistance among the three types of polypropylene. SEBS, propylene elastomer, and polypropylene are all non-polar materials, do not readily absorb water, and possess good salt spray resistance. The above materials exhibit good compatibility, and after blending, extrusion, and granulation, the material displays excellent overall performance.
[0035] The outer sheath primarily serves a mechanical protection function. To ensure the overall flexibility of the cable, the Shore hardness value of its material should be 80±5A.
[0036] The formulation system of the salt spray and low-temperature resistant PVC cable sheath material used in this method is shown in Table 2:
[0037] Table 2 shows the composition of the sheath material by the following parts by weight.
[0038] Serial Number Material Name Number of parts by weight / part 1 PVC resin 1 (degree of polymerization 1300) 40-50 2 PVC resin 2 (degree of polymerization 1800) 40-50 3 stabilizer 4-8 4 Polyethylene wax 0.2-0.5 5 Calcium stearate 0.2-0.5 6 Cold-resistant plasticizer DOS 5-10 7 Cold-resistant plasticizer SH-912 20-30 8 Plasticizer DOTP 20-30 9 EMA (Extracorporeal Membrane) 6-10 10 Nano calcium carbonate 40-50
[0039] To ensure the material's low-temperature resistance, the sheath material formulation uses a blend of high-polymerization and low-polymerization PVC, increasing the degree of molecular chain entanglement and thus enhancing the material's low-temperature performance. Cold-resistant plasticizers and toughening agents are used to ensure stable operation at -40°C. Salt spray stabilizers are employed to prevent sodium ions from damaging the material's surface and internal structure.
[0040] In this technical solution, in order to improve the performance of the cable and avoid the performance deficiencies or redundancies that may occur when directly using existing similar functional cable materials, a new cable material was designed, and a processing technology was formulated in combination with the characteristics of the cable structure.
[0041] The cable manufactured using this method meets all the performance requirements of lightning arrester down conductors, and also satisfies the special requirements for mechanical properties, flexibility, salt spray resistance, and low-temperature resistance under operating conditions. This method achieves high-quality manufacturing of small-diameter lightning arrester down conductor cables.
[0042] Advantages of this invention:
[0043] The specific thickness and material of the outer sheath, when used in cables, endow them with excellent mechanical properties, flexibility, salt spray resistance, and low-temperature resistance. Furthermore, the inherent properties of the sheath material itself provide flame-retardant characteristics, ensuring the cable's long-term, reliable, and safe operation.
[0044] The cable core is made of tin-plated copper conductor, semi-conductive shielding material, and thermoplastic elastomer insulation, which homogenizes the conductor's electric field. The conductor of this cable employs a flexible structure to enhance cable flexibility; the insulation thickness is uniform, ensuring an eccentricity of no more than 5%.
[0045] The beneficial effects of this invention are: the cable manufacturing method improves the cable's flexibility, giving it resistance to salt spray and low temperatures, enabling it to cope with various complex working conditions and extending its service life; it also improves the cable's electrical insulation performance, ensuring that the lightning current will not generate dangerous sparks on surrounding electrical conductive components when lightning strikes; and it can pass a 200kA (10 / 350μs) impulse current test, meeting the lightning protection requirements for wind turbines in IEC61400-24.
[0046] Based on the above characteristics, this cable can be used in the lightning protection system of wind turbine generator sets, and is also suitable for use as the down conductor of the lightning arrester in the lightning protection system of other electrical equipment. Attached Figure Description
[0047] Figure 1 This is a schematic diagram of the cable being embedded in the wind turbine blades in this embodiment;
[0048] Figure 2 This is a schematic diagram of the radial cross-section of the cable in this embodiment;
[0049] In the diagram: 1. Lightning arrester, 2. Down conductor cable, 3. Conductor, 4. Shielding layer, 5. Insulation layer, 6. Outer sheath layer. Detailed Implementation
[0050] The technical solution will be further explained below with reference to specific embodiments:
[0051] A method for manufacturing a down conductor cable for a pre-embedded lightning arrester on a wind turbine blade includes the following steps:
[0052] 1) Fabricate conductor 3 according to the conductor cross-sectional area specifications, and set it aside;
[0053] 2) Take the conductor obtained in step 1) and extrude the shielding layer 4 and the insulation layer 5 to obtain the wire core;
[0054] 3) In step 2), the outer sheath layer 6 is obtained to wrap the wire core.
[0055] The radial cross-section of the manufactured downlead cable is as follows: Figure 2 .
[0056] In step 1):
[0057] 1.1) Making metal monofilaments:
[0058] A copper rod with a diameter of 8mm is drawn into a copper single wire with a diameter of 0.400mm. The tolerance of the copper single wire is ±1%d (d is the diameter). During wire drawing, the lubricant temperature is controlled between 20 and 49℃, the cooling water temperature is controlled between 20 and 49℃, the annealing coefficient is 8.0 ± 0.2, the elongation of the copper single wire is ≥25%, and the resistivity of the copper single wire does not exceed 0.017700Ω·mm. 2 / m;
[0059] 1.2) Tin plating is performed on the surface of copper single wire with a diameter of Φ0.400mm. The concentration of acid in the electroplating solution (sulfuric acid can be used) is controlled within the range of (170~220)mL / L, the temperature is (40~50)℃, the pH value of the washing water is controlled within the range of 8.5~10.0, and the plating thickness of the round copper wire after tin plating is (6.00±0.50)μm.
[0060] 1.3) Use a wire bundling machine to bundle the conductor monofilaments: the direction of bundling the strands is right-hand Z, and the direction of each layer of re-twisting is left-hand S. The conductor pitch ratio is 15 to 17 times for the strands, 13 to 16 times for the inner layer, and 12 to 14 times for the outer layer.
[0061] The conductor must meet the following requirements: DC resistance at 20℃ < 0.277 Ω / km; and a weighing cross-sectional area of 68 mm². 2 The outer diameter of the conductor is 11.6 ± 0.2 mm.
[0062] 1.4) Wrap a non-woven fabric with a thickness of 0.10 mm and a width of 25 mm around the conductor from step 1.3);
[0063] The overlap rate of the wrapping is 15% to 17%; the outer diameter of the cable after wrapping is 11.9 ± 0.2 mm.
[0064] In step 2), a double-layer co-extrusion process is used to extrude the conductor shielding layer and the insulation layer to obtain the insulated wire core; the insulated wire core is processed and produced using a 70+90 extrusion production line.
[0065] Conductor shielding layer: The conductor shielding layer is formed by extrusion of semi-conductive inner shielding cable material. The thickness of the shielding layer is 0.8mm, and the thickness at the thinnest point is not less than 90% of the nominal value. The performance of the semi-conductive inner shielding cable material meets the requirements of thermoplastic semi-conductive shielding material for PSD conductors in JB / T 10738-2007.
[0066] Insulation layer: The insulation layer is made of salt spray resistant and low temperature resistant flexible elastomer insulation material extruded. The thickness of the insulation layer is 3.0mm, and the thickness of the thinnest point is not less than 90% of the nominal value.
[0067] The design of this down conductor cable conforms to the structural design requirements of GB / T 14049-2008 "10kV Rated Voltage Overhead Insulated Cables". During the manufacturing process, a double-layer co-extrusion process for conductor shielding and insulation is employed. This process ensures the cleanliness of the insulation interface during extrusion, guaranteeing insulation performance. The conductor shielding layer structure further homogenizes the electric field. The material for the conductor shielding layer conforms to the thermoplastic semi-conductive shielding material for PSD conductors in JB / T 10738-2007.
[0068] Insulation layer design: To ensure the flexibility requirements of the cable, the preferred insulation material is an elastomer. Based on the waveform and characteristics of lightning pulse waves, the electric field distribution of the cable, and the design principles of insulation thickness, a feasibility study was conducted in the early stages of the design.
[0069] The waveform of lightning overvoltage is a pulse wave, and its shape is related to the distance of the lightning strike and backflashover, as well as system parameters. According to IEC 60060-1 "High Voltage Testing Techniques - Part 1: General Definitions and Test Requirements", the wavefront time of a lightning impulse voltage wave is 1–5 μs, and the half-peak time is 40–60 μs. Its characteristics are rapid waveform change and short duration.
[0070] When struck by lightning, a lightning impulse wave is generated on the conductor and propagates to both ends of the conductor at the speed of electromagnetic waves. If the amplitude of the lightning impulse wave exceeds the withstand voltage of the electrical equipment insulation, damage will occur. The cable manufactured using this method is intended for pre-embedded installation, cast with epoxy resin inside the wind turbine blades. Therefore, the insulation withstand voltage level must be considered to prevent insulation breakdown from causing dangerous sparks from lightning current and other conductive components. Referring to the lightning impulse withstand voltage specifications for 3–1000kV transmission and transformation lines in GB 311.1-1997, the rated lightning impulse pulse voltage (BIL) for a 10kV design is taken as 75kV.
[0071] Design using the average electric field strength formula, under pulsed voltage:
[0072] Δi=BIL / GL k1k2k3=75 / 35*1.1*1.1*1.1=2.85mm.
[0073] In the formula, GL represents the breakdown strength of the insulation material under pulse voltage, which is 35 MV / m; K1 represents the temperature coefficient of the breakdown strength under pulse voltage, which is 1.1; K2 represents the aging coefficient, which is 1.1; and K3 represents the safety factor introduced by uncertain factors, which is 1.1. Calculations show that a nominal insulation thickness of Δi = 3.0 mm meets the safety margin. Designing the insulation with this thickness and material is entirely feasible.
[0074] To meet the requirements of cable application scenarios and reduce the insulation layer thickness while satisfying various cable performance requirements, the formulation system of the salt spray-resistant and low-temperature-resistant flexible elastomer insulation material used in this step is shown in Table 1:
[0075] Table 1 shows the composition of the insulation material by weight of the following raw materials.
[0076] Serial Number Material Name Number of parts by weight / part The optimal number of portions in this example Optional manufacturers / models, brands 1 SEBS 10-30 25 TSRC 6151 2 Propylene elastomer 20-40 30 Exxon 3000 3 polypropylene 10-20 15 Formosa Plastics 5090T 4 White oil 8-20 10 Kairun No. 36 5 Masterbatch 3-5 4 Cabot 6269 6 Silicone Masterbatch 3-5 4 Wujiang AL-15 7 Nitrogen-phosphorus flame retardants 35-45 40 Edenda 8813 8 antioxidants 0.5-1.5 0.8 BASF B225 9 lubricant 0.8-1.5 1 Sino Additives E
[0077] In this insulation material, 10-20 parts of block copolymer polypropylene are added to improve the overall salt spray resistance of the material; to give the material good flame retardant properties and extrusion processing properties, propylene elastomer is introduced to replace part of the polypropylene, while reducing the amount of oil-extended SEBS added, which can both ensure the material's softness and improve its low-temperature resistance.
[0078] Polypropylene and SEBS resins possess excellent electrical properties, while SEBS and propylene elastomers exhibit good low-temperature resistance. The selected block copolymer polypropylene, containing ethylene-propylene comonomers, demonstrates the best low-temperature resistance among the three types of polypropylene. SEBS, propylene elastomers, and polypropylene are all non-polar materials, do not readily absorb water, and possess good salt spray resistance. These materials exhibit good compatibility, and after blending, extrusion, and granulation, the resulting material displays excellent overall performance.
[0079] The shielding layer is extruded using a Φ70 extruder, and the die head filter screen is made of 2 layers of 40 mesh. The temperatures of the first to sixth temperature zones of the extruder are 145℃, 155℃, 165℃, 170℃, 170℃ and 175℃ respectively, and the screw speed of the extruder is 15.0 rpm.
[0080] The insulation layer is extruded using a Φ90 extruder, and the die head filter screen is made of two layers of 40 mesh. The temperatures of the first to sixth temperature zones of the extruder are 145℃, 150℃, 165℃, 175℃, 175℃ and 175℃ respectively, and the screw speed of the extruder is 20.0 rpm.
[0081] The die dimensions for the double-layer co-extrusion are Φ12.4mm and Φ18.6mm respectively;
[0082] The average speed of the production line is 15 ± 0.3 m / min;
[0083] The EVA resin used in the shielding material has good compatibility with SEBS, propylene elastomer, and polypropylene. After extrusion, it has strong adhesion to the insulating material, preventing partial discharge caused by gaps. At the same time, there is a certain peel force between the two, and the double-layer co-extrusion process of the shielding material and the insulating material does not affect the mechanical and electrical properties of either.
[0084] This method's double-layer co-extrusion scheme significantly improves production efficiency. The equipment is equipped with an automatic online deviation measuring instrument, which can accurately distinguish the thickness and eccentricity of the cable's shielding and insulation layers, as well as the cable's overall outer diameter and ellipticity, and perform online closed-loop control. This ensures consistent cable quality and improves the uniformity of extrusion across layers by eliminating the need for a die-calibrated extruder head. The self-developed insulation material of this invention exhibits excellent processing performance, particularly high tensile properties, with a tensile strength exceeding 13.5 MPa and an elongation at break exceeding 400% (see relevant test data). This allows for better control of thickness during production, and the equipped extrusion die further enhances the control of insulation layer thickness. These tensile properties enable the processing of thinner layers.
[0085] In step 3), the outer sheath is made of soft sheath-grade low-temperature resistant, salt spray resistant, and flame-retardant polyvinyl chloride sheath material extruded. The nominal thickness of the outer sheath is 1.4mm to 1.8mm, and the thickness at the thinnest point is not less than 90% of the nominal value.
[0086] The outer sheath primarily serves a mechanical protection function. To ensure the overall flexibility of the cable, the Shore hardness value of its material should be 80±5A.
[0087] In this method, the formulation system for a dedicated salt spray and low-temperature resistant PVC cable sheath material is shown in Table 2:
[0088] Table 2 shows the composition of the sheath material by the following parts by weight.
[0089] Serial Number Material Name Number of copies The optimal number of portions in this example Optional manufacturers / models, brands 1 PVC resin 1 (degree of polymerization 1300) 40-50 50 United US-70 2 PVC resin 2 (degree of polymerization 1800) 40-50 50 Formosa Plastics S-80 3 stabilizer 4-8 8 Bear Brand 9700 4 Polyethylene wax 0.2-0.5 0.5 SCG LP0100P 5 Calcium stearate 0.2-0.5 0.5 Shanghai Saponification 200 Type 6 Cold-resistant plasticizer DOS 5-10 10 Sanmu Chemical 7 Cold-resistant plasticizer SH-912 20-30 30 Senhe Chemical 8 Plasticizer DOTP 20-30 30 Sanmu Chemical 9 EMA (Extracorporeal Membrane) 6-10 10 DuPont HP4501 10 Nano calcium carbonate 40-50 50 Jiangxi Guangyuan Chemical GY-1012
[0090] To ensure the material's low-temperature resistance, the sheath material formulation uses a blend of high-polymerization and low-polymerization PVC, increasing the degree of molecular chain entanglement and thus enhancing the material's low-temperature performance. Cold-resistant plasticizers and toughening agents are used to ensure stable operation at -40°C. Salt spray stabilizers are employed to prevent sodium ions from damaging the material's surface and internal structure.
[0091] Since the downlead cable of this invention is mainly used inside the wind turbine blades, there is no high risk of external damage; only the impact of environmental factors on the cable needs to be considered. According to the GB / T 12706-2020 standard, a sheath thickness of 1.4mm to 1.8mm can meet the basic protection requirements of the cable. In the sheath material formulation, a PVC cold-resistant modifier (cold-resistant toughening agent EMA) HP4051 is added. HP4051 is a copolymer of ethylene and vinyl acetate, similar to a rubber-elastic thermoplastic resin. The solubility parameters of HP4051 are similar to those of PVC resin, and it acts as a binder between the various levels of PVC resin particles. During the PVC processing and mixing, it forms a homogeneous phase and is distributed in particle form within the continuous phase, exhibiting a "sea-island" structure. This structure endows the PVC material with excellent cold and low-temperature resistance.
[0092] The extruded sheath material is produced using a Φ120 extruder. The temperatures of the first to tenth temperature zones of the extruder are 126℃, 140℃, 148℃, 150℃, 150℃, 152℃, 153℃, 153℃, 154℃ and 155℃, respectively. The screw speed of the extruder is 12.0 rpm.
[0093] The dimensions of the extrusion molds for the sheath are: Φ28.0mm (mold core) and Φ35.0mm (mold sleeve);
[0094] The average speed of the production line is 10 ± 0.5 m / min;
[0095] The outer sheath extrusion process employs a tube extrusion method, which is mature, stable, and highly adaptable to various equipment. Furthermore, the self-made low-temperature and salt spray resistant PVC cable sheath material of this invention exhibits excellent processing performance. The added special additives stabilize its processing properties, resulting in superior mechanical properties. During extrusion, the material's tensile properties are enhanced, and by controlling the stretch ratio, sheath thickness can be effectively controlled, achieving a smaller finished cable outer diameter. The uniformity of the outer sheath thickness is controlled through the selection and configuration of the extrusion die.
[0096] The outer diameter of the downlead cable manufactured by this invention is controlled within 25mm.
[0097] Because down conductors need to withstand complex environments such as coastal and mountainous locations, ordinary down conductors often have a short service life. Long-term corrosion and aging will affect the normal operation of the entire lightning protection system. The tin-plated conductor produced by this method meets the requirements for use under harsh conditions and can satisfy salt spray requirements. At the same time, the conductor has high strength, with a tensile strength exceeding 25kN. The conductor's 90° bending resistance exceeds 30 cycles, making it less prone to core breakage during long-term use.
[0098] Advantages of the small-diameter conductor of this invention:
[0099] 1. Within a reasonable outer diameter range, it can withstand simulated lightning current impact and meet the 200kA 10 / 350μs (10MJ) conduction current test requirements specified in IEC61400-24.
[0100] 2. Small outer diameter conductors, while meeting usage requirements, compress the outer diameter of the conductor to reduce the space occupied by the down conductor inside the fan blade.
[0101] 3. The conductor section diameter ratio of the present invention is small, which makes the conductor more flexible and convenient for installation and laying.
[0102] The wrapping structure mentioned in step 1.4) not only serves to tighten the conductor and prevent it from loosening, but more importantly, it weakens the electric field, allowing the lightning current to be discharged along a controllable path. This prevents surface flashover on the conductor surface and avoids dangerous sparks from other conductive components, thus meeting the requirements for down conductors in the Lightning Protection System (LPS) of IEC 62305-3.
[0103] Cables manufactured using this method are characterized by flexibility, corrosion resistance, low-temperature resistance, and aging resistance. They can pass a 200kA (10 / 350μs) impulse current test and meet the lightning protection requirements for wind turbines in IEC61400-24.
[0104] The conductor is made of tin-plated copper conductor bundled and stranded, with non-metallic strips wrapped around the outside of the conductor to prevent the stranded conductor from loosening; the shielding layer uses a semi-conductive material (YJP-10 from Jiangyin Haijiang Polymer Materials Co., Ltd. in this example) to shield the electric field; the insulation layer is flexible and insulated from the surrounding environment to ensure that the current does not leak.
[0105] During wind turbine blade manufacturing, the embedded portion of the lead cable can be pre-embedded inside the wind turbine blade; the flexible cable structure facilitates construction. (Reference) Figure 1 There are one or more lightning rods on each side of the wind turbine blade. The down conductors are connected to the lightning rods on both sides and then connected in parallel and crimped together to form a tree-like structure. The down conductors are then led from inside the blade to the tower and finally to the ground.
[0106] The cable possesses insulating properties, ensuring safe conduction of lightning current to the ground without generating dangerous sparks on surrounding electrical conductive components. It meets requirements for low-temperature resistance and corrosion resistance, and can also be used as an external lead wire for wind blades, extending its service life in harsh environments. This cable can be used in wind turbine generator lightning protection systems, and is also suitable for use as a down conductor in lightning arresters of other electrical equipment lightning protection systems.
[0107] The results of the test showed that the main parameters of the cable in this example include:
[0108]
[0109]
Claims
1. A method for manufacturing a down conductor cable for a pre-embedded lightning arrester on a wind turbine blade, characterized by comprising the following steps: 1) Fabricate conductors according to the specified cross-sectional area, and set aside for later use; 2) Take the conductor obtained in step 1) and extrude the shielding layer and insulation layer to obtain the wire core; 3) In step 2), an outer sheath layer is formed around the wire core; In step 1), 1.1) Fabrication of copper monofilament: A copper rod is drawn into a copper monofilament corresponding to the required conductor diameter. The tolerance of the copper monofilament is controlled within ±1%d, where d is the diameter. During drawing, the lubricant temperature and cooling water temperature are controlled between 20 and 49°C, the annealing coefficient is 8.0 ± 0.2, the elongation of the copper monofilament is ≥25%, and the resistivity of the copper monofilament does not exceed 0.017700 Ω·mm. 2 / m; 1.2) Tin plating treatment on copper monofilament: the concentration of acid in the electroplating solution is controlled within the range of 170-220 mL / L, the temperature is 40-50℃, the pH value of the washing solution is controlled within the range of 8.5-10.0, and the thickness of the coating of the round copper wire after tin plating is 6.00±0.50μm. 1.3) Copper monofilaments are bundled into conductors using a wire bundling machine: the strand bundling direction is right-hand Z, and the pitch ratio is 15 to 17 times; during re-twisting, each layer is set to left-hand S, with the inner layer pitch ratio being 13 to 16 times and the outer layer pitch ratio being 12 to 14 times. 1.4) Non-woven fabric tape is wrapped tightly around the conductor in overlapping layers; In step 2), The shielding layer and the insulation layer are manufactured using a double-layer co-extrusion process to obtain the wire core; The semi-conductive inner shielding cable material used in the inner shielding layer is a cable material whose performance meets the requirements of thermoplastic semi-conductive shielding material for PSD conductors in JB / T 10738-2007; The outer insulation layer uses a salt spray-resistant and low-temperature-resistant flexible elastomer insulation material, and its formula, by weight, consists of the following raw material components: , The process parameters for double-layer co-extrusion are set as follows: The shielding layer is extruded using a Φ70 extruder. Along the feed to discharge direction, the temperatures of the first to sixth temperature zones of the extruder are 145±5℃, 155±5℃, 165±5℃, 170±5℃, 170±5℃ and 175±5℃ respectively. The screw speed of the extruder is 15.0 rpm. The insulation layer is extruded using a Φ90 extruder. Along the feed to discharge direction, the temperatures of the first to sixth temperature zones of the extruder are 145±5℃, 150±5℃, 165±5℃, 175±5℃, 175±5℃ and 175±5℃ respectively. The screw speed of the extruder is 20.0 rpm. The die dimensions for the double-layer co-extrusion are: core Φ12.4mm, die sleeve Φ18.6mm; The average linear speed of the production line is 15 ± 0.3 m / min; In step 3), The outer sheath layer is manufactured using an extrusion process to obtain the cable product; The outer sheath layer uses a salt spray and low-temperature resistant PVC sheath material, and its formula, by weight, consists of the following raw material components: , The extrusion process parameters are set as follows: using a Φ120 extruder, the temperatures of the first to tenth temperature zones of the extruder along the feed to discharge direction are 126±5℃, 140±5℃, 148±5℃, 150±5℃, 150±5℃, 152±5℃, 153±5℃, 153±5℃, 154±5℃ and 155±5℃ respectively, and the screw speed of the extruder is 12.0 rpm; The dimensions of the extrusion mold for the sheath are: core Φ28.0mm, sleeve Φ35.0mm; The average line speed of the production line is 10 ± 0.5 m / min.
2. The method for manufacturing the down conductor cable of the wind turbine blade pre-embedded lightning arrester according to claim 1, characterized in that, Steps 1.1) to 1.3) yield a conductor with a DC resistance of <0.277Ω / km at 20℃; the outer diameter of the conductor is 11.6±0.2mm.
3. The method for manufacturing the down conductor cable of the wind turbine blade pre-embedded lightning arrester according to claim 1, characterized in that, in In step 1.4), the thickness of the nonwoven tape is 0.10 mm, the width is 25 mm, and the overlap rate of the wrapping is 15% to 17%; the outer diameter of the conductor after wrapping is 11.9 ± 0.2 mm.
Citation Information
Patent Citations
Manufacturing method of 80-year-life K3 type control cable for nuclear power station and cable
CN115881368A
Method for manufacturing 105°c torsion-resistant wind energy cable and cable
WO2023024308A1