3D printed hydrogel bone repair scaffold, preparation method of ion-crosslinked chitosan-based hydrogel
By using short-chain chitosan and alternating cycle immersion methods in 3D printing technology, the problems of poor mechanical properties and insufficient biocompatibility of traditional materials are solved, and the problem of poor quality and insufficient biocompatibility is achieved. It is a bone repair material with excellent mechanical properties and good biocompatible properties, suitable for fracture repair, meeting the needs of high-precision customization.
Patent Information
- Application Number
- CN202310335681.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional natural polymers have poor mechanical properties and insufficient biocompatibility. Artificial synthetic polymers have limited their application in vivo due to their poor biocompatibility. The existing hydrogels have challenges in the combination of soft structures and hard bones. , it is difficult to prepare bone repair materials with excellent mechanical properties and good biocompatibility.
By introducing short-chain chitosan and using alternating cycle soaking dipotassium hydrogen phosphate and calcium chloride in situ depositing hydroxyapatite, combined with 3D printing technology, ion crosslinked chitosan-based hydrogel bone repair was prepared by preparing ionic crosslinked chitosan-based hydrogel bone repair using alternating cycles of soaking dipotassium hydrogen phosphate and calcium chloride. The scaffold improves its mechanical properties and biocompatibility and avoids toxic residues modified by chitosan.
Achieves hydrogel bone repair material with excellent mechanical properties and good biocompatible properties, which can be well integrated with bones, and while optimizing the bone formation function, it is easy to operate, widens the application range, and meets high-precision personalization. Customized requirements.
Smart Images

Figure CN116407680B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of hydrogels, and in particular to a method for preparing a 3D printed hydrogel bone repair scaffold and an ion-crosslinked chitosan-based hydrogel. Background Art
[0002] With the development of medical technology, the use of tissue engineering technology to treat bone injuries caused by diseases, accidents, etc., such as fractures, osteoarthritis, etc., has become a major research hotspot in this field, and more and more research teams are focusing on using biomaterials to repair bone defects. Traditional natural polymers have poor mechanical properties and cannot meet the mechanical strength that bones bear in daily life. Artificially synthesized polymers have poor biocompatibility, which limits their application in the body. Therefore, as biomedical materials applied to the human body, the joint use of natural polymers and synthetic polymers has become a general trend.
[0003] Chitosan is the second most abundant polysaccharide in nature. It can be extracted from waste shells such as shrimp and crabs. It is cheap and easy to obtain. However, due to its poor solubility in aqueous solutions and organic solvents, chitosan has not been put into practical use. Chitosan is made by thermochemical deacetylation of chitosan under alkaline conditions. Chitosan can promote cell growth and mineral deposition in the matrix. Its good biocompatibility minimizes local inflammation caused by implant materials. Although chitosan itself is non-toxic, due to some of its properties, such as poor solubility and low mechanical strength, chitosan is often modified for use. Some modifications may make it more or less toxic, and any residual reactants should be carefully removed.
[0004] In addition, although many tough hydrogels have been developed for repairing bone defects, even if the material itself has the advantage of promoting cell osteogenic differentiation, the combination of its soft structure and hard bone is still a major challenge. Therefore, it is of great significance to prepare a chitosan-based hydrogel scaffold material with excellent mechanical properties, good biocompatibility and good integration with bone. Summary of the invention
[0005] In order to overcome the above-mentioned shortcomings and deficiencies of the prior art, the object of the present invention is to provide a method for preparing a 3D printed hydrogel bone repair scaffold, by introducing short-chain chitosan and utilizing a method of in-situ deposition of hydroxyapatite by alternating cycles of soaking in dipotassium hydrogen phosphate and calcium chloride, to prepare a hydrogel bone repair material having excellent mechanical properties and good biocompatibility, which can optimize the osteogenic function of the material while enabling it to be well integrated with the bone, and chitosan does not need to be modified during the preparation process, and there is no toxic residue.
[0006] Another object of the present invention is to provide an ion-crosslinked chitosan-based hydrogel, which utilizes the ionic crosslinking of short-chain chitosan and the covalent crosslinking of polyethylene glycol diacrylate PEGDA, as well as the hydrogen bonding between the two crosslinking networks, so that the hydrogel exhibits excellent mechanical properties; then, the mechanical strength of the hydrogel is significantly improved by alternately immersing the generated hydroxyapatite inorganic phase in a dipotassium hydrogen phosphate solution and a calcium chloride solution.
[0007] The purpose of the present invention is achieved through the following technical solutions:
[0008] The preparation method of 3D printed hydrogel bone repair scaffold comprises the following steps:
[0009] Sequentially add 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone, sodium citrate, polyethylene glycol diacrylate PEGDA, and short-chain chitosan into deionized water, stir and mix evenly to obtain a slurry;
[0010] Wherein, the mass ratio of initiator, sodium citrate, short-chain chitosan, and polyethylene glycol diacrylate PEGDA is (0.003-0.005): (0.067-0.133): (1-2): 1;
[0011] The slurry is transferred to a 3D printing cylinder and centrifuged to remove bubbles to obtain a 3D printing slurry;
[0012] The scaffold is printed by an extrusion 3D printer, and after being cured under ultraviolet light, it is immersed in a mixed ion solution of sodium citrate and sodium tripolyphosphate to obtain an ion-crosslinked chitosan-based hydrogel;
[0013] The ion-crosslinked chitosan-based hydrogel was soaked in a tris-hydroxymethylaminomethane buffer solution Tris-HCl; then, it was alternately soaked in a potassium hydrogen phosphate solution and a calcium chloride solution for multiple times to deposit amorphous calcium phosphate in situ on the ion-crosslinked chitosan-based hydrogel, and then soaked in a calcium chloride solution to incubate the amorphous calcium phosphate into hydroxyapatite, thereby obtaining a 3D printed hydrogel bone repair scaffold.
[0014] Preferably, in the mixed ion solution of sodium citrate and sodium tripolyphosphate, the mass concentration of sodium citrate is 3-5%, and the mass concentration of sodium tripolyphosphate is 3-5%.
[0015] Preferably, the concentration of the dipotassium hydrogen phosphate solution is 250-300 mM.
[0016] Preferably, the concentration of the calcium chloride solution is 450-500 mM.
[0017] Preferably, the step of alternately immersing the mixture in the potassium hydrogen phosphate solution and the calcium chloride solution for multiple times is as follows:
[0018] Soak in dipotassium hydrogen phosphate solution and calcium chloride solution alternately for 1 to 5 times, with each soaking time being 30 to 120 seconds.
[0019] Preferably, the immersion in a mixed ion solution of sodium citrate and sodium tripolyphosphate is specifically:
[0020] Soak in a mixed ion solution of sodium citrate and sodium tripolyphosphate for 10 to 80 minutes.
[0021] Preferably, the curing under ultraviolet light is specifically:
[0022] Cure under UV light for 3 to 30 minutes.
[0023] Preferably, the ion-crosslinked chitosan-based hydrogel is immersed in a tris-HCl buffer solution, specifically:
[0024] The ion-crosslinked chitosan-based hydrogel is immersed in a pH 9.0 to pH 9.2 tris-HCl buffer solution for 10 to 12 hours.
[0025] Preferably, the soaking in calcium chloride solution to incubate amorphous calcium phosphate into hydroxyapatite is specifically:
[0026] The amorphous calcium phosphate is incubated into hydroxyapatite by soaking in a calcium chloride solution of pH 11.0 to pH 11.2 at 36 to 37° C. for 20 to 24 hours.
[0027] The method for preparing ion-crosslinked chitosan-based hydrogel comprises the following steps:
[0028] 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone, polyethylene glycol diacrylate PEGDA, and short-chain chitosan were sequentially added into deionized water, and stirred and mixed to obtain a sol;
[0029] Wherein, the mass ratio of initiator, short-chain chitosan, and polyethylene glycol diacrylate PEGDA is (0.003-0.005): (1-2): 1;
[0030] The sol is solidified under ultraviolet light and then immersed in a mixed ion solution of sodium citrate and sodium tripolyphosphate to obtain an ion-crosslinked chitosan-based hydrogel.
[0031] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0032] (1) The preparation method of the 3D printed hydrogel bone repair scaffold of the present invention introduces short-chain chitosan and utilizes the method of in situ deposition of hydroxyapatite to prepare a hydrogel bone repair material with excellent mechanical properties and good biocompatibility. While optimizing the osteogenic function of the material, it can also enable it to be well integrated with the bone. In addition, the chitosan does not need to be modified during the preparation process, and there is no toxic residue.
[0033] (2) The preparation method of the 3D printed hydrogel bone repair scaffold of the present invention can meet the precision requirements of 3D printing by pre-adding a trace amount of sodium citrate to the slurry, and meet the needs of high-precision and personalized customization of biomaterials in the repair process, which greatly expands the application range of ion-crosslinked chitosan-based hydrogels.
[0034] (3) The preparation method of the 3D printed hydrogel bone repair scaffold of the present invention is based on the semi-permeability of the hydrogel. By cyclically immersing the hydrogel in a solution containing calcium and phosphorus elements, hydroxyapatite is deposited in situ on the hydrogel, thereby improving the compressive strength of the bone repair scaffold; while optimizing the osteogenic function of the material, it can also enable it to be well integrated with the bone, and the preparation process is simple and easy to operate.
[0035] (4) The ion-crosslinked chitosan-based hydrogel of the present invention utilizes the ionic crosslinking of short-chain chitosan and the covalent crosslinking of polyethylene glycol diacrylate PEGDA, as well as the hydrogen bonding between the two crosslinking networks, so that the hydrogel exhibits excellent mechanical properties. At the same time, the hydroxyapatite inorganic phase is generated by cyclically immersing in a dipotassium hydrogen phosphate solution and a calcium chloride solution, thereby significantly improving the mechanical strength of the hydrogel. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 It is a tensile stress-strain curve diagram of the ion-crosslinked chitosan-based hydrogels of Example 1 and Comparative Examples 1 to 3 of the present invention.
[0037] Figure 2 This is a comparison chart of X-ray diffraction of the 3D printed hydrogel bone repair scaffolds of Example 2 and Comparative Example 4 of the present invention.
[0038] Figure 3 This is a comparison chart of the compressive stress-strain curves of the 3D printed hydrogel bone repair scaffolds of Example 2 and Comparative Examples 4 to 5 of the present invention.
[0039] Figure 4 This is a tungsten filament scanning electron microscope image of hydroxyapatite inside the hydrogel of Example 2 of the present invention.
[0040] Figure 5 This is a comparison chart of alkaline phosphatase ALP activity of the 3D printed hydrogel bone repair scaffolds of Example 2 and Comparative Examples 4 to 5 of the present invention.
[0041] Figure 6 This is a live and dead staining image of cells on the 3D printed hydrogel bone repair scaffold of Comparative Example 4 of the present invention. DETAILED DESCRIPTION
[0042] The present invention will be further described in detail below in conjunction with examples, but the embodiments of the present invention are not limited thereto.
[0043] Example 1
[0044] The method for preparing the ion-crosslinked chitosan-based hydrogel of this embodiment comprises the following steps:
[0045] 1) Add 8 mg of photoinitiator i2959, 2 g of polyethylene glycol diacrylate PEGDA, and 3 g of short-chain chitosan to 30 ml of deionized water, stir and mix well to obtain a sol;
[0046] 2) placing the sol of step 1) in a UV light box for UV curing for 30 minutes to obtain a single network hydrogel after photocrosslinking;
[0047] 3) Soaking the single network hydrogel in step 2) in a mixed ion solution of sodium citrate and sodium tripolyphosphate for 80 minutes; wherein the mixed ion solution of sodium citrate and sodium tripolyphosphate is prepared by adding 5g of sodium citrate powder and 5g of sodium tripolyphosphate powder into 100ml of deionized water.
[0048] The tensile stress-strain curve of the ion-crosslinked chitosan-based hydrogel material prepared in this example is shown in FIG. Figure 1 As shown in DN-TC.
[0049] Comparative Example 1
[0050] The preparation method of the hydrogel material of this comparative example comprises the following steps:
[0051] 1) Add 8 mg of photoinitiator i2959, 2 g of polyethylene glycol diacrylate PEGDA, and 3 g of short-chain chitosan to 30 ml of deionized water, stir and mix well to obtain a sol;
[0052] 2) placing the sol of step 1) in a UV light box for UV curing for 30 minutes to obtain a single network hydrogel after photocrosslinking.
[0053] The tensile stress-strain curve of the ion-crosslinked chitosan-based hydrogel material prepared in this comparative example is as follows: Figure 1 As shown in CS / PEGDA.
[0054] Comparative Example 2
[0055] The preparation method of the hydrogel material of this comparative example comprises the following steps:
[0056] 1) Add 8 mg of photoinitiator i2959, 2 g of polyethylene glycol diacrylate PEGDA, and 3 g of short-chain chitosan to 30 ml of deionized water, stir and mix well to obtain a sol;
[0057] 2) placing the sol of step 1) in a UV light box for UV curing for 30 minutes to obtain a single network hydrogel after photocrosslinking;
[0058] 3) Soaking the single network hydrogel in step 2) in a sodium citrate ion solution with a mass concentration of 10% for 80 minutes.
[0059] The tensile stress-strain curve of the ion-crosslinked chitosan-based hydrogel material prepared in this comparative example is as follows: Figure 1 As shown in DN-Cit.
[0060] Comparative Example 3
[0061] The preparation method of the hydrogel material of this comparative example comprises the following steps:
[0062] 1) Add 8 mg of photoinitiator i2959, 2 g of polyethylene glycol diacrylate PEGDA, and 3 g of short-chain chitosan to 30 ml of deionized water, stir and mix well to obtain a sol;
[0063] 2) placing the sol of step 1) in a UV light box for UV curing for 30 minutes to obtain a single network hydrogel after photocrosslinking;
[0064] 3) Soaking the single network hydrogel in a sodium tripolyphosphate ion solution with a mass concentration of 10% for 80 minutes.
[0065] The tensile stress-strain curve of the ion-crosslinked chitosan-based hydrogel material prepared in this comparative example is as follows: Figure 1 As shown in DN-Tpp.
[0066] Combined with Example 1, Comparative Examples 1 to 3 and Figure 1 It can be seen that the tensile strength of the chitosan-based hydrogels of Example 1, Comparative Example 2, and Comparative Example 3 after immersion in the ionic solution is significantly higher than that of Comparative Example 1, wherein the tensile strength of the ion-crosslinked chitosan-based hydrogel DN-TC obtained by immersion and crosslinking in the mixed ionic solution in Example 1 is close to 1.7 MPa, which is better than DN-Tpp and DN-Cit obtained by immersion in a single solution.
[0067] Example 2
[0068] The preparation method of the 3D printed hydrogel bone repair scaffold of this embodiment comprises the following steps:
[0069] 1) 8 mg of photoinitiator, 0.2 g of sodium citrate, 2 g of polyethylene glycol diacrylate PEGDA, and 3 g of short-chain chitosan were added to 30 mL of deionized water in sequence, and stirred to mix well to obtain a slurry;
[0070] 2) Transfer the slurry to a printing cylinder and centrifuge at 5000 rpm for 2 minutes to remove bubbles generated during the preparation process to obtain a 3D printable slurry;
[0071] 3) Set the printing parameters of the extrusion 3D printer: create a new printing model, set the bracket printing pressure to 0.12Mpa, the printing speed to 10mm / s, the printing needle diameter to 0.41mm, determine the printing path, and start printing the bracket;
[0072] 4) Place the scaffold obtained in step 3) in a UV light box for photocuring for 30 minutes, and then immerse it in a mixed ion solution of sodium citrate and sodium tripolyphosphate for 80 minutes to obtain an ion-crosslinked chitosan-based hydrogel. The mixed ion solution of sodium citrate and sodium tripolyphosphate is prepared by adding 5g of sodium citrate powder and 5g of sodium tripolyphosphate powder to 100ml of deionized water;
[0073] 5) Soaking the 3D printable ion-crosslinked chitosan-based hydrogel obtained in step 4) in a pH 9.0 tris-HCl buffer solution overnight;
[0074] 6) The next day, the hydrogel obtained in step 5) was alternately immersed in 300 mM potassium hydrogen phosphate solution and 500 mM calcium chloride solution to deposit amorphous calcium phosphate in situ, the immersion time was 120 s, and the number of alternate immersion cycles was 5 times;
[0075] 7) After the above hydrogel has been circulated and soaked, it is soaked in a 500 mM calcium chloride solution with a pH of 11.0 at 37° C. and reacted for 24 hours to incubate the amorphous calcium phosphate into hydroxyapatite, thereby obtaining a 3D printed hydrogel bone repair scaffold.
[0076] The XRD test results of the 3D printed hydrogel bone repair scaffold prepared in this example are as follows: Figure 2 As shown in CaP-c-TC.
[0077] The compressive stress-strain curve of the 3D printed hydrogel bone repair scaffold prepared in this example is as follows: Figure 3 As shown in CaP-c-TC.
[0078] The tungsten filament scanning electron microscope image of the hydroxyapatite inside the 3D printed hydrogel bone repair scaffold prepared in this example is as follows: Figure 4 As shown, it can be seen from the figure that a large number of white particles are attached to the internal network of the hydrogel.
[0079] The alkaline phosphatase (ALP) activity of cells cultured on the hydrogel scaffold of this embodiment was quantitatively tested using a BCA protein concentration detection kit and an alkaline phosphatase detection kit. The results are shown in FIG. Figure 5 As shown in CaP-c-TC.
[0080] Comparative Example 4
[0081] The preparation method of the 3D printed hydrogel bone repair scaffold of this embodiment comprises the following steps:
[0082] 1) 8 mg of photoinitiator, 0.2 g of sodium citrate, 2 g of polyethylene glycol diacrylate PEGDA, and 3 g of short-chain chitosan were added to 30 mL of deionized water in sequence, and stirred to mix well to obtain a slurry;
[0083] 2) Transfer the slurry to a printing cylinder and centrifuge at 5000 rpm for 2 minutes to remove bubbles generated during the preparation process to obtain a 3D printable slurry;
[0084] 3) Set the printing parameters of the extrusion 3D printer: create a new printing model, set the bracket printing pressure to 0.12Mpa, the printing speed to 10mm / s, the printing needle diameter to 0.41mm, determine the printing path, and start printing the bracket;
[0085] 4) The scaffold obtained in step 3) was placed in a UV light box for photocuring for 30 minutes, and then immersed in a 10% mass concentration of sodium citrate and sodium tripolyphosphate mixed ion solution for 80 minutes to obtain a 3D printed hydrogel bone repair scaffold.
[0086] The XRD test results of the 3D printed hydrogel bone repair scaffold prepared in this comparative example are as follows Figure 2 As shown in DN-c-TC.
[0087] The compressive stress-strain curve of the 3D printed hydrogel bone repair scaffold prepared in this comparative example is as follows Figure 3 As shown in DN-c-TC.
[0088] The alkaline phosphatase (ALP) activity of cells cultured on the hydrogel scaffold of this comparative example was quantitatively tested using a BCA protein concentration test kit and an alkaline phosphatase test kit. The results are shown in FIG. Figure 5 As shown in DN-c-TC.
[0089] The cells seeded on the 3D printed hydrogel bone repair scaffold prepared in this comparative example were stained for live and dead cells using a cell live and dead fluorescent staining kit. The results are as follows: Figure 6 As shown, living cells appear green under fluorescence. It can be seen from the figure that a large number of living cells adhere to the scaffold, indicating that the scaffold material has good biocompatibility.
[0090] Comparative Example 5
[0091] 1) 8 mg of photoinitiator, 0.2 g of sodium citrate, 2 g of polyethylene glycol diacrylate PEGDA, and 3 g of short-chain chitosan were added to 30 mL of deionized water in sequence, and stirred to mix well to obtain a slurry;
[0092] 2) Transfer the slurry to a printing cylinder and centrifuge at 5000 rpm for 2 minutes to remove bubbles generated during the preparation process to obtain a 3D printable slurry;
[0093] 3) Set the printing parameters of the extrusion 3D printer: create a new printing model, set the bracket printing pressure to 0.12Mpa, the printing speed to 10mm / s, the printing needle diameter to 0.41mm, determine the printing path, and start printing the bracket;
[0094] 4) The scaffold obtained in step 3) was placed in a UV light box for photocuring for 30 minutes, and then immersed in a sodium citrate ion solution with a mass concentration of 10% for 80 minutes to obtain a 3D printed hydrogel bone repair scaffold.
[0095] The compressive stress-strain curve of the 3D printed hydrogel bone repair scaffold prepared in this comparative example is as follows Figure 3 As shown in DN-c-Cit.
[0096] The alkaline phosphatase (ALP) activity of cells cultured on the hydrogel scaffold of this comparative example was quantitatively tested using a BCA protein concentration test kit and an alkaline phosphatase test kit. The results are shown in FIG. Figure 5 As shown in DN-c-Cit.
[0097] Combined with Example 2, Comparative Example 4 and Figure 2 It can be seen that the XRD spectrum of Example 2 clearly shows the characteristic peak of hydroxyapatite, indicating that the inorganic calcium phosphate phase generated after the hydrogel is cyclically immersed in a solution containing calcium and phosphorus elements is hydroxyapatite.
[0098] Combined with Example 2, Comparative Examples 4-5 and Figure 3 It can be seen that the compressive strength of the 3D printed hydrogel bone repair scaffold CaP-c-TC introduced with the inorganic phase in Example 2 is better than that of the hydrogels DN-c-Cit and DN-c-TC without the inorganic phase.
[0099] Combined with Example 2, Comparative Examples 4-5 and Figure 5It can be seen that the alkaline phosphatase activity of Example 2 is significantly higher than that of Comparative Example 4 and Comparative Example 5, and the ALP activity of Comparative Example 4 is higher than that of Comparative Example 5. Analysis shows that in the presence of osteogenic induction solution, although the 3D printable chitosan-based hydrogel soaked in sodium citrate in Comparative Example 5 can also promote cell osteogenic differentiation, the ALP activity of Example 2 and Comparative Example 4 on the 7th and 14th days is significantly higher than that of Comparative Example 5. This experimental result shows that the hydroxyapatite layer generated after cyclic immersion and the chitosan-based hydrogel containing tripolyphosphate both have the effect of promoting cell osteogenic differentiation, but the osteogenic effect of in situ deposited hydroxyapatite is better.
[0100] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A method for preparing an ion-crosslinked chitosan-based hydrogel, characterized in that: The following steps are involved: 8 mg of photoinitiator i2959, 2 g of polyethylene glycol diacrylate PEGDA, and 3 g of short-chain chitosan were added to 30 ml of deionized water in sequence, and stirred to mix well to obtain a sol; The sol was cured under ultraviolet light for 30 minutes and then immersed in a mixed ion solution of sodium citrate and sodium tripolyphosphate for 80 minutes to obtain an ion-crosslinked chitosan-based hydrogel; the mixed ion solution of sodium citrate and sodium tripolyphosphate was prepared by adding 5g of sodium citrate powder and 5g of sodium tripolyphosphate powder to 100ml of deionized water.
2. A method for preparing a 3D printed hydrogel bone repair scaffold, characterized in that: The following steps are involved: Sequentially add 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone, sodium citrate, polyethylene glycol diacrylate PEGDA, and short-chain chitosan into deionized water, stir and mix evenly to obtain a slurry; Among them, the mass ratio of initiator, sodium citrate, short-chain chitosan, and polyethylene glycol diacrylate PEGDA is 0.004:0.1:1.5:1; The slurry is transferred to a 3D printing cylinder and centrifuged to remove bubbles to obtain a 3D printing slurry; The scaffold is printed by an extrusion 3D printer, and after being cured under ultraviolet light, it is immersed in a mixed ion solution of sodium citrate and sodium tripolyphosphate to obtain an ion-crosslinked chitosan-based hydrogel; in the mixed ion solution of sodium citrate and sodium tripolyphosphate, the mass concentration of sodium citrate is 5%, and the mass concentration of sodium tripolyphosphate is 5%; The ion-crosslinked chitosan-based hydrogel was soaked in a tris-hydroxymethylaminomethane buffer solution Tris-HCl; then, it was alternately soaked in a potassium hydrogen phosphate solution and a calcium chloride solution for multiple times to deposit amorphous calcium phosphate in situ on the ion-crosslinked chitosan-based hydrogel, and then soaked in a calcium chloride solution to incubate the amorphous calcium phosphate into hydroxyapatite, thereby obtaining a 3D printed hydrogel bone repair scaffold.
3. The method for preparing the 3D printed hydrogel bone repair scaffold according to claim 2, characterized in that: The concentration of the dipotassium hydrogen phosphate solution is 250-300 mM.
4. The method for preparing the 3D printed hydrogel bone repair scaffold according to claim 2, characterized in that: The concentration of the calcium chloride solution is 450-500 mM.
5. The method for preparing the 3D printed hydrogel bone repair scaffold according to claim 2, characterized in that: The method comprises the following steps: Soak in dipotassium hydrogen phosphate solution and calcium chloride solution alternately for 1 to 5 times, with each soaking time being 30 to 120 seconds.
6. The method for preparing the 3D printed hydrogel bone repair scaffold according to claim 2, characterized in that: The soaking in the mixed ion solution of sodium citrate and sodium tripolyphosphate is specifically as follows: Soak in a mixed ion solution of sodium citrate and sodium tripolyphosphate for 10 to 80 minutes.
7. The method for preparing the 3D printed hydrogel bone repair scaffold according to claim 2, characterized in that: The curing under ultraviolet light is specifically: Cure under UV light for 3 to 30 minutes.
8. The method for preparing the 3D printed hydrogel bone repair scaffold according to claim 2, characterized in that: The ion-crosslinked chitosan-based hydrogel is immersed in a tris-HCl buffer solution, specifically: The ion-crosslinked chitosan-based hydrogel was immersed in Tris-HCl buffer (pH 9.0-pH 9.2) for 10-12 hours.
9. The method for preparing the 3D printed hydrogel bone repair scaffold according to claim 2, characterized in that: The soaking in calcium chloride solution allows amorphous calcium phosphate to be incubated into hydroxyapatite, specifically: Soak in a calcium chloride solution with a pH of 11.0 to 11.2 at 36 to 37°C and react for 20 to 24 hours to incubate amorphous calcium phosphate into hydroxyapatite.